A semiconductor epitaxial structure and its manufacturing method, and LED chip
By using alternate stacked barrier layers and potential well layers in the GaN-based semiconductor epitaxial structure and controlling the temperature transition during their growth, the stress problems caused by lattice mismatch are solved, and luminescence efficiency and production convenience are improved.
Patent Information
- Application Number
- CN202110176774.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-02-07
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2041-02-07
AI Technical Summary
In the GaN-based semiconductor light emitting epitaxial structure, the lattice mismatch between the well layer and the barrier layer leads to an increase in stress, affecting the recombination efficiency of electrons and holes.
Design a semiconductor epitaxial structure, by stacking the first type semiconductor layer, the active region and the second type semiconductor layer in sequence on the substrate surface, including alternately stacked barrier layers and potential well layers, and installing them on both sides of the potential well layer. There are cooling and heating layers, deep well layers and shallow well layers for electron restriction, growth temperature transitions to release stress.
It effectively improves the internal quantum efficiency of the quantum well luminescent layer, reduces stress, increases the number of holes, and simplifies the production process.
Smart Images

Figure CN112768578B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of light emitting diodes, and in particular to a semiconductor epitaxial structure and a manufacturing method thereof, and an LED chip. Background Art
[0002] Light Emitting Diode (LED) is a semiconductor electronic component that can emit light. LED has the advantages of high efficiency, long life, small size, low power consumption, etc. It can be used in indoor and outdoor white light lighting, screen display, backlight and other fields. In the development of LED industry, gallium nitride (GaN)-based materials are typical representatives of V-III group compound semiconductors. Improving the optoelectronic performance of GaN-based LEDs has become the key to the semiconductor lighting industry.
[0003] Epitaxial wafers are the primary finished products in the LED manufacturing process. Existing GaN-based LED epitaxial wafers include substrates, N-type semiconductor layers, active regions, and P-type semiconductor layers. The substrate is used to provide a growth surface for the epitaxial material, the N-type semiconductor layer is used to provide electrons for compound luminescence, the P-type semiconductor layer is used to provide holes for compound luminescence, and the active region is used for radiative compound luminescence of electrons and holes.
[0004] In the prior art, in the process of growing the quantum well light-emitting layer of the GaN-based semiconductor light-emitting epitaxial structure, an InGaN well layer is usually stacked on a GaN barrier layer. However, due to the lattice mismatch between InGaN and GaN, when the InGaN well layer is grown on the GaN barrier layer, dislocation defects will be generated in the InGaN well layer, thereby reducing the luminescence efficiency of the entire quantum well light-emitting layer.
[0005] In view of this, the inventor specially designed a semiconductor epitaxial structure and a manufacturing method thereof, and an LED chip, and this case was thus generated. Summary of the invention
[0006] The purpose of the present invention is to provide a semiconductor epitaxial structure and a method for manufacturing the same, as well as an LED chip, so as to solve the problem that the stress generated by the accumulation of lattice mismatches will seriously affect the recombination efficiency of electrons and holes in space due to the large lattice mismatch between the well layer and the barrier layer, and the large lattice mismatch between the well layer and the first type semiconductor layer.
[0007] In order to achieve the above object, the technical solution adopted by the present invention is as follows:
[0008] A semiconductor epitaxial structure, comprising:
[0009] substrate;
[0010] A first-type semiconductor layer, an active region, and a second-type semiconductor layer are sequentially stacked on the surface of the substrate;
[0011] The active region includes alternately stacked barrier layers and potential well layers, and a cooling layer and a deep well layer are sequentially arranged on the surface of at least one potential well layer close to the first type semiconductor layer, and a shallow well layer and a heating layer are sequentially arranged on the surface of at least one potential well layer close to the second type semiconductor layer; wherein the cooling layer and the heating layer are used for growth temperature transition between the barrier layer and the potential well layer; and the deep well layer and the shallow well layer are used for strengthening electron confinement of the well layer.
[0012] Preferably, during the growth of the deep well layer, its growth temperature is reduced from the growth temperature of the cooling layer to a temperature lower than the growth temperature of the potential well layer; during the growth of the shallow well layer, its growth temperature is increased from the growth temperature of the potential well layer to the growth temperature of the heating layer.
[0013] Preferably, the growth temperature of the temperature rising layer is lower than the growth temperature of the barrier layer.
[0014] Preferably, the deep well layer and the shallow well layer respectively include Al with a gradient In composition. x Ga y In z N material layer, wherein 0≤x≤1, 0≤y≤1, 0≤z≤1; further, it may be an AlGaInN material layer or a GaInN material layer.
[0015] Preferably, the deep well layer and the shallow well layer comprise material layers with gradually changing bandgap widths, and the bandgap width of the shallow well layer is always greater than the bandgap width of the potential well layer, and the local bandgap width of the deep well layer is less than the bandgap width of the potential well layer.
[0016] Preferably, the temperature-raising layer and the temperature-lowering layer respectively include non-doped material layers, and the deep well layer and the shallow well layer respectively include P-type doped material layers, and the doping concentration is not higher than 5*10 17 cm -3 .
[0017] Preferably, the temperature increasing layer and the temperature decreasing layer respectively include Al a Ga b N material layer, wherein 0≤a≤1, 0≤b≤1; further, it may be an AlGaN material layer or a GaN material layer.
[0018] Preferably, the thickness of the potential well layer is 3 times or more than the thickness of the deep well layer or the shallow well layer.
[0019] Preferably, the thickness of the deep well layer and the shallow well layer are both 0-10 nm.
[0020] Preferably, the thickness of the barrier layer is 4 times or more than the thickness of the temperature rising layer or the temperature falling layer.
[0021] Preferably, the thickness of the temperature rising layer and the temperature falling layer are both 0-20 nm.
[0022] Preferably, the barrier layer is doped with n-type impurities.
[0023] The present invention also provides a method for manufacturing a semiconductor epitaxial structure, the method comprising the following steps:
[0024] Step S01, providing a substrate;
[0025] Step S02, sequentially growing a first-type semiconductor layer, an active region, and a second-type semiconductor layer on the surface of the substrate;
[0026] The active region comprises barrier layers and potential well layers stacked alternately, and a cooling layer and a deep well layer are sequentially arranged on the surface of at least one potential well layer close to the first type semiconductor layer, and a shallow well layer and a heating layer are sequentially arranged on the surface of at least one potential well layer close to the second type semiconductor layer; wherein the cooling layer and the heating layer are used for the growth temperature transition between the barrier layer and the potential well layer; and the deep well layer and the shallow well layer are used for electron confinement of the barrier layer;
[0027] Furthermore, the deep well layer and the shallow well layer respectively include Al with a gradient In composition. x Ga y In z N material layer, wherein 0≤x≤1, 0≤y≤1, 0≤z≤1; the temperature-raising layer and the temperature-lowering layer respectively include Al a Ga b N material layer, wherein 0≤a≤1, 0≤b≤1.
[0028] Preferably, during the growth of the deep well layer, its growth temperature is reduced from the growth temperature of the cooling layer to a temperature lower than the growth temperature of the potential well layer; during the growth of the shallow well layer, its growth temperature is increased from the growth temperature of the potential well layer to the growth temperature of the heating layer.
[0029] Preferably, the growth temperature of the temperature rising layer is lower than the growth temperature of the barrier layer.
[0030] The present invention further provides an LED chip, comprising an epitaxial layer, an N-type electrode and a P-type electrode, wherein the epitaxial layer comprises any of the semiconductor epitaxial structures described above.
[0031] Through the above technical solutions, it can be known that the semiconductor epitaxial structure provided by the present invention is provided with a cooling layer and a deep well layer in sequence on at least one side of the potential well layer close to the first type semiconductor layer, and a shallow well layer and a heating layer in sequence on at least one side of the potential well layer close to the second type semiconductor layer; wherein the cooling layer and the heating layer are used for the growth temperature transition between the barrier layer and the potential well layer; the deep well layer and the shallow well layer are used to strengthen the electron confinement of the well layer; further, during the growth process of the deep well layer, its growth temperature is reduced from the growth temperature of the cooling layer to a temperature lower than the growth temperature of the potential well layer; during the growth process of the shallow well layer, its growth temperature is increased from the growth temperature of the potential well layer to the growth temperature of the heating layer. By controlling the growth temperature, the stress between the barrier layer and the potential well layer can be effectively released; at the same time, a well-like structure is further formed at the front and rear ends of the potential well layer, which is conducive to strengthening the electron confinement of the well layer, thereby improving its internal quantum efficiency.
[0032] Secondly, the heating layer and the cooling layer respectively include non-doped material layers, the deep well layer and the shallow well layer respectively include P-type doped material layers, and the doping concentration is not higher than 5*10 17 cm -3 The deep well layer and the shallow well layer respectively include a P-type doped material layer, and the doping concentration is not higher than 5*10 17 cm -3 On the one hand, the V-pits structure formed by the growth of the active area is combined with the micro-doped P-type impurities in the deep well layer and the shallow well layer, which can effectively handle different crystal interface energies and effectively release the stress between the deep well layer and the shallow well layer and the potential well layer and the barrier layer during their growth; on the other hand, it can effectively increase the number of holes in the active area and avoid the formation of a new built-in electric field in the active area, thereby effectively improving the internal quantum efficiency of the active area.
[0033] Furthermore, the thickness of the potential well layer is 3 times or more than the thickness of the deep well layer or the shallow well layer, and the thickness of the barrier layer is 4 times or more than the thickness of the temperature rising layer or the temperature falling layer; while avoiding the poor crystal quality of the entire active area due to the small thickness of the barrier layer; effectively releasing the stress between the potential well layer and the barrier layer during the growth of the deep well layer and the shallow well layer, and increasing the number of holes in the active area.
[0034] It can be seen from the above technical solutions that the method for manufacturing a semiconductor epitaxial structure provided by the present invention, while achieving the beneficial effects of the above semiconductor epitaxial structure, has a simple and convenient manufacturing process and is easy to produce.
[0035] It can be seen from the above technical solutions that the LED chip provided by the present invention is obtained on the basis of the above semiconductor epitaxial structure. Therefore, while it has the beneficial effects of the above semiconductor epitaxial structure, its manufacturing process is simple and convenient, and it is easy to produce. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0037] Figure 1 A schematic diagram of the structure of a semiconductor epitaxial structure provided by an embodiment of the present invention;
[0038] Figure 2 A schematic structural diagram of an active region of a semiconductor epitaxial structure provided by an embodiment of the present invention;
[0039] Figure 3 A schematic diagram of the growth temperature relationship of each component layer in the active region provided by an embodiment of the present invention;
[0040] Figure 4 A schematic diagram of the relationship between the barrier heights of various component layers in the active region provided by an embodiment of the present invention;
[0041] Explanation of symbols in the figure: 1. substrate, 2. first type semiconductor layer, 3. active region, 31. cooling layer, 32. deep well layer, 33. potential well layer, 34. shallow well layer, 35. heating layer, 36. barrier layer, 4. second type semiconductor layer, 5. buffer layer, Q1. barrier height of potential well layer, Q2. barrier height of barrier layer, T1. growth temperature of potential well layer, T2. growth temperature of barrier layer. DETAILED DESCRIPTION
[0042] To make the content of the present invention clearer, the content of the present invention is further described below in conjunction with the accompanying drawings. The present invention is not limited to this specific embodiment. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0043] like Figure 1 , Figure 2 As shown, a semiconductor epitaxial structure comprises:
[0044] Substrate 1;
[0045] A first-type semiconductor layer 2, an active region 3, and a second-type semiconductor layer 4 are sequentially stacked on the surface of a substrate 1;
[0046] The active region 3 includes alternately stacked barrier layers 36 and potential well layers 33, and a cooling layer 31 and a deep well layer 32 are sequentially provided on the surface of at least one side of the potential well layer 33 close to the first-type semiconductor layer 2, and a shallow well layer 34 and a heating layer 35 are sequentially provided on the surface of at least one side of the potential well layer 33 close to the second-type semiconductor layer 4; wherein the cooling layer 31 and the heating layer 35 are used for growth temperature transition between the barrier layer 36 and the potential well layer 33; and the deep well layer 32 and the shallow well layer 34 are used for strengthening the electron confinement of the well layer.
[0047] It is worth mentioning that the type of the substrate 11 is not limited in the semiconductor epitaxial structure of this embodiment. For example, the substrate 11 can be but not limited to a sapphire substrate 1, a silicon substrate 1, etc. In addition, the specific material types of the first-type semiconductor layer 22, the active region 33, and the second-type semiconductor layer 45 are also not limited in the semiconductor epitaxial structure of this embodiment. For example, the first-type semiconductor layer 2 can be but not limited to a gallium nitride layer, and correspondingly, the second-type semiconductor layer 4 can be but not limited to a gallium nitride layer.
[0048] In this embodiment, a buffer layer 5 may be further provided between the substrate 1 and the first-type semiconductor layer 2 .
[0049] like Figure 3 As shown, in this embodiment, during the growth process of the deep well layer 32, its growth temperature is reduced from the growth temperature of the cooling layer 31 to a growth temperature T1 lower than the potential well layer 33; during the growth process of the shallow well layer 34, its growth temperature is increased from the growth temperature T1 of the potential well layer 33 to the growth temperature of the heating layer 35.
[0050] It should be noted that Figure 3 The figure shows the relationship between the growth temperatures of the components in the active region 3 provided in the present embodiment. It only illustrates the linear change of the growth temperature of the components in the active region 3. The present embodiment does not limit the specific temperature and its change trend during the growth of the cooling layer 31, the deep well layer 32, the potential well layer 33, the shallow well layer 34, the heating layer 35, and the barrier layer 36, which can be linear or nonlinear. At the same time, the temperature difference between the growth temperature of the deep well layer 32 and the potential well layer 33 is not limited in the present embodiment, as long as the temperature difference transition is achieved and the stress between the barrier layer 36 and the potential well layer 33 is effectively released.
[0051] like Figure 3 As shown, in this embodiment, the growth temperature of the temperature-elevating layer 35 is lower than the growth temperature T2 of the barrier layer 36. It should be noted that the temperature difference between the growth temperatures of the temperature-elevating layer 35 and the barrier layer 36 is not limited in this embodiment, as long as the growth temperature transition between the two can be achieved while ensuring the growth quality.
[0052] In this embodiment, the deep well layer 32 and the shallow well layer 34 respectively include Al xGa y In z N material layer, wherein 0≤x≤1, 0≤y≤1, 0≤z≤1; further, it may be an AlGaInN material layer or a GaInN material layer.
[0053] like Figure 4 As shown, in this embodiment, the deep well layer 32 and the shallow well layer 34 include material layers with gradually changing bandgap widths, and the bandgap width of the shallow well layer 34 is always greater than the bandgap width of the potential well layer 33 , and the local bandgap width of the deep well layer 32 is less than the bandgap width of the potential well layer 33 .
[0054] It should be noted that Figure 4 The figure shows a schematic diagram of the barrier height relationship of each component layer in the active area 3 provided in an embodiment of the present invention. It only illustrates the linear change of the energy band relationship of each component layer in the active area 3. This embodiment does not limit the specific energy band values and their change trends during the growth process of the cooling layer 31, the deep well layer 32, the potential well layer 33, the shallow well layer 34, the heating layer 35, and the barrier layer 36, which can be linear or nonlinear.
[0055] In this embodiment, the temperature raising layer 35 and the temperature lowering layer 31 respectively include non-doped material layers, and the deep well layer 32 and the shallow well layer 34 respectively include P-type doped material layers, and the doping concentration is not higher than 5*10 17 cm -3 .
[0056] In this embodiment, the temperature raising layer 35 and the temperature lowering layer 31 respectively include Al a Ga b N material layer, wherein 0≤a≤1, 0≤b≤1; further, it may be an AlGaN material layer or a GaN material layer.
[0057] In this embodiment, the thickness of the potential well layer 33 is three times or more than the thickness of the deep well layer 32 or the shallow well layer 34 .
[0058] In this embodiment, the thickness of the deep well layer 32 and the shallow well layer 34 are both 0-10 nm.
[0059] In this embodiment, the thickness of the barrier layer 36 is 4 times or more than the thickness of the temperature rising layer 35 or the temperature falling layer 31 .
[0060] In this embodiment, the thickness of the temperature rising layer 35 and the temperature falling layer 31 are both 0-20 nm.
[0061] In this embodiment, the barrier layer 36 is doped with n-type impurities.
[0062] This embodiment also provides a method for manufacturing a semiconductor epitaxial structure, the manufacturing method comprising the following steps:
[0063] Step S01, providing a substrate 1;
[0064] Step S02, sequentially growing a buffer layer 5, a first-type semiconductor layer 2, an active region 3, and a second-type semiconductor layer 4 on the surface of the substrate 1;
[0065] The active region 3 includes alternately stacked barrier layers 36 and potential well layers 33, and a cooling layer 31 and a deep well layer 32 are sequentially provided on the surface of at least one side of the potential well layer 33 close to the first type semiconductor layer 2, and a shallow well layer 34 and a heating layer 35 are sequentially provided on the surface of at least one side of the potential well layer 33 close to the second type semiconductor layer 4; wherein the cooling layer 31 and the heating layer 35 are used for the growth temperature transition between the barrier layer 36 and the potential well layer 33; the deep well layer 32 and the shallow well layer 34 are used for strengthening the electron confinement of the well layer;
[0066] Furthermore, the deep well layer 32 and the shallow well layer 34 respectively include Al x Ga y In z N material layer, wherein 0≤x≤1, 0≤y≤1, 0≤z≤1; preferably, it may be an AlGaInN material layer or a GaInN material layer;
[0067] The temperature raising layer 35 and the temperature lowering layer 31 respectively include Al a Ga b N material layer, wherein 0≤a≤1, 0≤b≤1; preferably, it may be an AlGaN material layer or a GaN material layer;
[0068] In this embodiment, during the growth process of the deep well layer 32, its growth temperature is reduced from the growth temperature of the cooling layer 31 to a temperature lower than the growth temperature of the potential well layer 33; during the growth process of the shallow well layer 34, its growth temperature is increased from the growth temperature of the potential well layer 33 to the growth temperature of the heating layer 35.
[0069] In this embodiment, the growth temperature of the temperature rising layer 35 is lower than the growth temperature of the barrier layer 36 .
[0070] This embodiment further provides an LED chip, including an epitaxial layer, an N-type electrode and a P-type electrode, wherein the epitaxial layer includes any of the semiconductor epitaxial structures described above.
[0071] It can be known from the above technical scheme that the semiconductor epitaxial structure provided in this embodiment is provided with a cooling layer 31 and a deep well layer 32 in sequence on the surface of at least one side of a potential well layer 33 close to the first type semiconductor layer 2, and a shallow well layer 34 and a heating layer 35 in sequence on the surface of at least one side of a potential well layer 33 close to the second type semiconductor layer 4; wherein the cooling layer 31 and the heating layer 35 are used for the growth temperature transition between the barrier layer 36 and the potential well layer 33; the deep well layer 32 and the shallow well layer 34 are used for strengthening the electron confinement of the well layer; further, during the growth process of the deep well layer 32, its growth temperature is reduced from the growth temperature of the cooling layer 31 to a temperature lower than the growth temperature of the potential well layer 33; during the growth process of the shallow well layer 34, its growth temperature is increased from the growth temperature of the potential well layer 33 to the growth temperature of the heating layer 35. By controlling the growth temperature, the stress between the barrier layer 36 and the potential well layer 33 can be effectively released; at the same time, a well-like structure is further formed at the front and rear ends of the potential well layer 33, which is beneficial to strengthen the electron confinement of the well layer, thereby improving its internal quantum efficiency.
[0072] Secondly, the temperature raising layer 35 and the temperature lowering layer 31 respectively include non-doped material layers, the deep well layer 32 and the shallow well layer 34 respectively include P-type doped material layers, and the doping concentration is not higher than 5*10 17 cm -3 The deep well layer 32 and the shallow well layer 34 respectively include a P-type doped material layer, and the doping concentration is not higher than 5*10 17 cm -3 On the one hand, the V-pits structure formed by the growth of the active area 3 is combined with the micro-doping of P-type impurities in the deep well layer 32 and the shallow well layer 34, which can effectively handle different crystal interface energies and effectively release the stress between the deep well layer 32 and the shallow well layer 34 and the potential well layer 33 and the barrier layer 36 during the growth process; on the other hand, it can effectively increase the number of holes in the active area 3 and avoid the formation of a new built-in electric field in the active area 3, thereby effectively improving the internal quantum efficiency of the active area 3.
[0073] Furthermore, the thickness of the potential well layer 33 is 3 times or more than the thickness of the deep well layer 32 or the shallow well layer 34, and the thickness of the barrier layer 36 is 4 times or more than the thickness of the temperature rising layer 35 or the temperature falling layer 31; while avoiding the poor crystal quality of the active area 3 as a whole due to the small thickness of the barrier layer 36; effectively releasing the stress between the deep well layer 32 and the shallow well layer 34 and the potential well layer 33 and the barrier layer 36 during the growth process, and increasing the number of holes in the active area 3.
[0074] It can be seen from the above technical solutions that the method for manufacturing a semiconductor epitaxial structure provided in this embodiment, while achieving the beneficial effects of the above semiconductor epitaxial structure, has a simple and convenient manufacturing process and is easy to produce.
[0075] It can be seen from the above technical solutions that the LED chip provided in this embodiment is obtained on the basis of the above semiconductor epitaxial structure. Therefore, while it has the beneficial effects of the above semiconductor epitaxial structure, its manufacturing process is simple and convenient, and it is easy to produce.
[0076] The various embodiments in this specification are described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the various embodiments can be referenced to each other.
[0077] It should also be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "comprises", "comprising" or any other variants thereof are intended to cover non-exclusive inclusion, so that an article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such article or device. In the absence of further restrictions, the elements defined by the sentence "comprising a ..." do not exclude the existence of other identical elements in the article or device including the above elements.
[0078] The above description of the disclosed embodiments enables those skilled in the art to implement or use the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A semiconductor epitaxial structure, It is characterized in that include: substrate; A first-type semiconductor layer, an active region, and a second-type semiconductor layer are sequentially stacked on the surface of the substrate; The active region comprises barrier layers and potential well layers stacked alternately, and a cooling layer and a deep well layer are sequentially arranged on the surface of at least one potential well layer close to the first type semiconductor layer, and a shallow well layer and a heating layer are sequentially arranged on the surface of at least one potential well layer close to the second type semiconductor layer; wherein the cooling layer and the heating layer are used for the growth temperature transition between the barrier layer and the potential well layer; and the deep well layer and the shallow well layer are used to strengthen the electron confinement of the well layer by adjusting the bandgap width; The temperature-raising layer and the temperature-lowering layer respectively include non-doped material layers, and the deep well layer and the shallow well layer respectively include P-type doped material layers, and the doping concentration is not higher than 5*10 17 cm -3 .
2. The semiconductor epitaxial structure according to claim 1, It is characterized in that During the growth of the deep well layer, its growth temperature is reduced from the growth temperature of the cooling layer to a temperature lower than the growth temperature of the potential well layer; during the growth of the shallow well layer, its growth temperature is increased from the growth temperature of the potential well layer to the growth temperature of the heating layer.
3. The semiconductor epitaxial structure according to claim 1, It is characterized in that The growth temperature of the temperature rising layer is lower than the growth temperature of the barrier layer.
4. The semiconductor epitaxial structure according to claim 1, It is characterized in that The deep well layer and the shallow well layer respectively include Al x Ga y In z N material layer, wherein 0≤x≤1, 0≤y≤1, 0≤z≤1.
5. The semiconductor epitaxial structure according to claim 1, It is characterized in that The deep well layer and the shallow well layer include material layers with gradually changing bandgap widths, and the bandgap width of the shallow well layer is always greater than the bandgap width of the potential well layer, while the local bandgap width of the deep well layer is less than the bandgap width of the potential well layer.
6. The semiconductor epitaxial structure according to claim 1, It is characterized in that The temperature increasing layer and the temperature decreasing layer respectively include Al a Ga b N material layer, wherein 0≤a≤1, 0≤b≤1.
7. The semiconductor epitaxial structure according to claim 1, It is characterized in that The thickness of the potential well layer is 3 times or more than the thickness of the deep well layer or the shallow well layer.
8. The semiconductor epitaxial structure according to claim 1, It is characterized in that The thickness of the deep well layer and the shallow well layer are both 0-10 nm.
9. The semiconductor epitaxial structure according to claim 1, It is characterized in that The thickness of the barrier layer is 4 times or more than the thickness of the temperature rising layer or the temperature falling layer.
10. The semiconductor epitaxial structure according to claim 1, It is characterized in that The thickness of the temperature increasing layer and the temperature decreasing layer are both 0-20 nm.
11. A method for manufacturing a semiconductor epitaxial structure, It is characterized in that The production method comprises the following steps: Step S01, providing a substrate; Step S02, sequentially growing a first-type semiconductor layer, an active region, and a second-type semiconductor layer on the surface of the substrate; The active region comprises barrier layers and potential well layers stacked alternately, and a cooling layer and a deep well layer are sequentially arranged on the surface of at least one potential well layer close to the first type semiconductor layer, and a shallow well layer and a heating layer are sequentially arranged on the surface of at least one potential well layer close to the second type semiconductor layer; wherein the cooling layer and the heating layer are used for the growth temperature transition between the barrier layer and the potential well layer; and the deep well layer and the shallow well layer are used to strengthen the electron confinement of the well layer by adjusting the bandgap width; Furthermore, the deep well layer and the shallow well layer respectively include Al with a gradient In composition. x Ga y In z N material layer, wherein 0≤x≤1, 0≤y≤1, 0≤z≤1; the temperature-raising layer and the temperature-lowering layer respectively include Al a Ga b N material layer, wherein 0≤a≤1, 0≤b≤1; The temperature-raising layer and the temperature-lowering layer respectively include non-doped material layers, and the deep well layer and the shallow well layer respectively include P-type doped material layers, and the doping concentration is not higher than 5*10 17 cm -3 .
12. The method for manufacturing a semiconductor epitaxial structure according to claim 11, It is characterized in that During the growth of the deep well layer, its growth temperature is reduced from the growth temperature of the cooling layer to a temperature lower than the growth temperature of the potential well layer; during the growth of the shallow well layer, its growth temperature is increased from the growth temperature of the potential well layer to the growth temperature of the heating layer.
13. The method for manufacturing a semiconductor epitaxial structure according to claim 12, It is characterized in that The growth temperature of the temperature rising layer is lower than the growth temperature of the barrier layer.
14. An LED chip comprising an epitaxial layer, an N-type electrode and a P-type electrode, It is characterized in that The epitaxial layer comprises the semiconductor epitaxial structure according to any one of claims 1 to 10.