A dam-free COB LED substrate and its preparation method and application
By adding a pressed metal or inorganic non-metallic material substrate to the COB LED substrate to form a double-layer or multi-layer metal-based or combined-based pressed structure, the problem of poor transverse heat conduction and heat dissipation capabilities of COB LED light sources is solved, and the light source is extended Lifespan and ensure light-emitting type.
Patent Information
- Application Number
- CN202110219664.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-02-26
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2041-02-26
AI Technical Summary
The existing COB LED light sources have poor transverse heat conduction and heat dissipation capabilities, resulting in shorter life.
Using the COB LED substrate design without dams, the two-layer or multi-layer metal base or combined base pressing structure is formed by adding compressed metal or inorganic non-metallic material substrates to the traditional COB substrates, replacing the traditional dam process and enhancing the The transverse heat conduction and heat dissipation capability are used, and the secondary light distribution is performed through the substrate appearance design.
Improve the lateral heat conduction and heat dissipation ability of COB light sources, extend the life of the light source, and ensure the setting of light output type, which is manifested as lateral heat conduction ability of 60-65℃, heat dissipation ability of 70-75℃, light source life of 10000-10200H, light output Light type 100-110°.
Smart Images

Figure CN112820814B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of LED display, and in particular relates to a dam-free COB LED substrate and a preparation method and application thereof. Background Art
[0002] At present, most of the COB structure products on the market are the following two solutions: 1) Use silicone jelly-like dam glue, use a specific dam machine to perform dam operations according to specific shape, height and other required parameters, and then use an oven for long-term curing. Disadvantages: long process flow and cycle, large equipment requirements; 2) When making the substrate, use plastic to plasticize the dam, and no dam operation is required. Disadvantages: the plastic model is fixed, the mold cost is expensive, and the plastic dam mold cycle is long.
[0003] CN111463198A discloses a COB packaging structure of UVC-LED and a manufacturing method thereof, which comprises a ceramic circuit board, a ceramic dam, a transparent cover plate, a UVC-LED chip, a ceramic insulating plate and a reflective layer plate, wherein the light emitted by the UVC-LED chip is reflected out of the transparent cover plate through the reflective coating of the expanded hole, thereby effectively improving the directivity of the light and greatly improving the light output efficiency of the COB light source; and the ceramic insulating plate has stable performance compared with the insulating glue, thus avoiding the risk of short circuit due to aging and having high safety; a metal protective layer is plated at the adhesive portion of the transparent cover plate, however, the COB packaging structure requires the provision of a ceramic dam, resulting in poor lateral heat conduction and heat dissipation capabilities of the COB light source and poor lifespan of the COB light source.
[0004] CN206490058U discloses a dam-free COB light source packaging structure, including a substrate, a mirror reflection area is provided on the substrate, LED light-emitting chips are evenly distributed on the mirror reflection area, and fluorescent glue is filled between the LED light-emitting chips; a BT resin ring is provided on the periphery of the mirror reflection area, and the thickness of the BT resin ring is the same as that of the fluorescent glue. The surface of the BT resin ring adopts an irregular gong shape, the LED light-emitting chip is packaged with a lens, and the LED light-emitting chip packaged with a lens can be integrated with a reflective cup. Although it removes the process flow of the traditional COB light source using chemical materials such as silica gel and resin to enclose the dam, the COB light source still has the problems of poor lateral heat conduction, heat dissipation capacity and COB light source life.
[0005] Therefore, it is necessary to provide a COB LED light source module with a new structure to overcome the above defects. Summary of the invention
[0006] In view of the shortcomings of the prior art, the present invention aims to provide a damless COB LED substrate and a preparation method and application thereof. The damless COB LED substrate increases the lateral heat conduction and heat dissipation capabilities of the COB light source, thereby increasing the life of the COB light source.
[0007] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0008] In a first aspect, the present invention provides a dam-free COB LED substrate, comprising a first base layer, an insulating adhesive layer, a copper foil layer, an ink layer, a pure adhesive layer and a second base layer stacked in sequence.
[0009] Among them, COB stands for Chip On Board, which means that the bare chip is adhered to the interconnection substrate with conductive or non-conductive glue, and then wire bonding is performed to achieve its electrical connection. COB LED is also called COB LED source, COB LED module. There are many packaging forms such as long strip / square / circular / ring / triangular / fan-shaped.
[0010] The present invention eliminates the process flow of using chemical materials such as silicone and resin to form a dam in traditional COB light sources through a substrate lamination process, and adds a laminated metal or inorganic non-metallic material substrate on the traditional COB substrate to achieve a double-layer or multi-layer metal base or combined base lamination effect. The shape design of the upper substrate replaces the traditional COB light source dam operation, while increasing the lateral thermal conductivity and heat dissipation capacity of the COB light source, thereby extending the life of the COB light source. The shape design of the upper substrate directly performs secondary light distribution on the COB light source to ensure the light output type.
[0011] Preferably, the thickness of the first base layer is 800-2000 μm, for example, 800 μm, 820 μm, 840 μm, 860 μm, 880 μm, 900 μm, 920 μm, 940 μm, 960 μm, 980 μm, 1000 μm, 1200 μm, 1400 μm, 1600 μm, 2000 μm, etc.
[0012] Preferably, the number of layers of the first base layer is 1 or more, for example, it can be 1 layer, 2 layers, 3 layers, 4 layers, 5 layers, 6 layers, etc.
[0013] Preferably, the first base layer is selected from any one of a copper substrate, a ceramic substrate, a mirror aluminum substrate or plastic.
[0014] Preferably, the thickness of the insulating adhesive layer is 50-150 μm, for example, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, 110 μm, 120 μm, 130 μm, 140 μm, 150 μm, etc.
[0015] Preferably, the insulating adhesive layer is formed by high-temperature curing of insulating adhesive, and the insulating adhesive is selected from polyester insulating adhesive and / or epoxy insulating adhesive.
[0016] The above-mentioned insulating adhesives can all be purchased from the market, for example, the present invention uses: polyester insulating adhesive (manufacturer: New Power, brand 450A80); epoxy insulating adhesive (manufacturer: Hongchang), etc.
[0017] Preferably, the high temperature curing temperature is 100-150°C, for example, it may be 100°C, 105°C, 110°C, 115°C, 120°C, 125°C, 130°C, 135°C, 140°C, 145°C, 150°C, etc.
[0018] Preferably, the copper foil layer has a thickness of 20-50 μm, for example, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, etc.
[0019] Preferably, the ink layer has a thickness of 10-30 μm, for example, 10 μm, 12 μm, 14 μm, 16 μm, 18 μm, 20 μm, 22 μm, 24 μm, 26 μm, 28 μm, 30 μm, etc.
[0020] Preferably, the ink layer is selected from any one of WT05, LEW7S or LB-1900W, or a combination of at least two of them.
[0021] Preferably, the thickness of the pure glue layer is 10-30 μm, for example, 10 μm, 12 μm, 14 μm, 16 μm, 18 μm, 20 μm, 22 μm, 24 μm, 26 μm, 28 μm, 30 μm, etc.
[0022] Preferably, the pure adhesive layer is selected from any one of epoxy, silicone or polyurethane, or a combination of at least two of them.
[0023] The above pure glue can be purchased from the market, for example: epoxy (such as manufacturer: Langbowan, brand: NO.1-6120; manufacturer: Shilin, brand: SL3029, etc.); silicone (such as manufacturer: Flory Optoelectronic Materials, brand A05-01H, A05-01M, A05-01L, etc.); polyurethane (manufacturer: New Power, brand 450A80, etc.).
[0024] Preferably, the second base layer has a thickness of 700-2000 μm, for example, 700 μm, 720 μm, 740 μm, 760 μm, 780 μm, 800 μm, 820 μm, 840 μm, 860 μm, 880 μm, 900 μm, 1000 μm, 1200 μm, 1400 μm, 1600 μm, 1800 μm, 2000 μm, etc.
[0025] Preferably, the number of layers of the second base layer is 1 or more, for example, it can be 1 layer, 2 layers, 3 layers, 4 layers, 5 layers, 6 layers, etc.
[0026] Preferably, the second base layer is selected from any one of a copper substrate, a ceramic substrate, and a mirror aluminum substrate.
[0027] In a second aspect, the present invention provides a method for preparing a dam-free COB LED substrate as described in the first aspect, wherein the method for preparing a dam-free COB LED substrate comprises the following steps:
[0028] (1) After applying the insulating adhesive to the first base layer, the insulating adhesive layer is formed by high-temperature pressing;
[0029] (2) After the copper foil is fixed to the insulating adhesive layer, it is pressed at high temperature to form a copper foil layer;
[0030] (3) printing or spraying the ink on the copper foil layer and then curing it to form an ink layer;
[0031] (4) After applying pure glue to the ink layer, high temperature pressing is performed to form a pure glue layer;
[0032] (5) After the second base layer is fixed to the pure adhesive layer, it is pressed at high temperature to form the second base layer.
[0033] Preferably, in step (1), step (2), step (3) and step (4), the temperature of the high-temperature pressing is independently 100-150°C, for example, it can be 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, etc., and the time of the high-temperature pressing is independently 1.5-2h, for example, it can be 1.5h, 1.6h, 1.7h, 1.8h, 1.9h, 2h, etc.
[0034] Preferably, the curing in step (3) is natural curing and / or baking curing.
[0035] Preferably, the natural curing temperature is 20-30°C, such as 20°C, 22°C, 24°C, 26°C, 28°C, 30°C, etc., and the natural curing time is 2-3h, such as 2h, 2.2h, 2.4h, 2.6h, 2.8h, 3h, etc.
[0036] Preferably, the curing temperature is 100-110°C, for example, 100°C, 102°C, 104°C, 106°C, 108°C, 110°C, etc., and the curing time is 0.1-1h, for example, 0.1h, 0.2h, 0.4h, 0.6h, 0.8h, 1h, etc.
[0037] In a third aspect, the present invention provides a use of the dam-free COB LED substrate as described in the first aspect in preparing an LED light source.
[0038] The present invention reserves the coating and packaging area at the back end of the COB process by using the outer shape design of the pressed substrate, so as to achieve a production solution that replaces the traditional dam process. The different materials of the pressed substrate can be used to assist the lateral heat dissipation of the phosphor and silica gel mixture in the COB light-emitting area. The shape and thickness of the pressed substrate can also achieve the effect of secondary light distribution of the COB light-emitting area, meeting the setting of the final COB LED light output light type.
[0039] Compared with the prior art, the present invention has the following beneficial effects:
[0040] (1) The present invention achieves this through the design of the COB substrate, eliminating the process of the traditional COB light source requiring a dam, enhancing the heat conduction path of the COB light source to increase the life of the light source, and utilizing the substrate to achieve a secondary light distribution effect;
[0041] (2) The lateral thermal conductivity of the damless COB LED substrate described in the present invention is 60-65°C as shown by thermal imaging test; the heat dissipation capacity is 70-75°C as shown by thermal imaging test; the light source life is 10000-10200 hours; and the light output type is 100-110° as shown by remote equipment test. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 This is a schematic diagram of the structure of the dam-free COB LED substrate of the present invention;
[0043] 1 is the first base layer, 2 is the insulating adhesive layer, 3 is the copper foil layer, 4 is the ink layer, 5 is the pure adhesive layer, and 6 is the second base layer. DETAILED DESCRIPTION
[0044] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0045] Figure 1 FIG. 1 is a schematic diagram of the structure of the dam-free COB LED substrate of the present invention. Figure 1As shown, the dam-free COB LED substrate includes a first base layer 1, an insulating adhesive layer 2, a copper foil layer 3, an ink layer 4, a pure adhesive layer 5 and a second base layer 6 which are stacked in sequence.
[0046] The sources of the components in the following examples are as follows: polyester insulating glue (manufacturer: New Power, brand 450A80), epoxy insulating glue (manufacturer: Hongchang), epoxy pure glue (manufacturer: Shilin, brand: SL3029), silicone pure glue (Flory Optoelectronic Materials, brand A05-01H), polyurethane pure glue (manufacturer: New Baoli, brand 450A80, etc.).
[0047] Example 1
[0048] This embodiment provides a dam-free COB LED substrate, wherein the dam-free COB LED substrate comprises a first base layer, an insulating adhesive layer, a copper foil layer, an ink layer, a pure adhesive layer, and a second base layer stacked in sequence;
[0049] The first base layer is a 900μm thick mirror aluminum substrate; the insulating glue layer is a 120μm thick insulating glue layer (the insulating glue is polyester insulating glue); the copper foil layer is 35μm thick; the ink layer is a 20μm thick ink layer (the ink is WT05); the pure glue layer is a 20μm thick pure glue layer (the pure glue is epoxy pure glue); the second base layer is a 800μm thick mirror aluminum substrate.
[0050] The method for preparing the dam-free COB LED substrate described in this embodiment comprises the following steps:
[0051] (1) After applying the insulating adhesive to the first base layer, the insulating adhesive is pressed at a high temperature of 120° C. for 2 hours to form an insulating adhesive layer;
[0052] (2) After the copper foil is fixed to the insulating adhesive layer, it is pressed at a high temperature of 120°C for 2 hours to form a copper foil layer;
[0053] (3) After printing the ink on the copper foil layer, it is cured at 25° C. for 2.5 hours to form an ink layer;
[0054] (4) After applying the pure glue to the ink layer, high temperature pressing is performed at 120° C. for 1.5 h to form a pure glue layer;
[0055] (5) After the second base layer is fixed to the pure adhesive layer, it is pressed at a high temperature of 120° C. for 1.5 hours to form the second base layer.
[0056] Example 2
[0057] This embodiment provides a dam-free COB LED substrate, wherein the dam-free COB LED substrate comprises a first base layer, an insulating adhesive layer, a copper foil layer, an ink layer, a pure adhesive layer, and a second base layer stacked in sequence;
[0058] The first base layer is a 900μm thick ceramic substrate; the insulating glue layer is a 120μm thick insulating glue layer (the insulating glue is epoxy insulating glue); the copper foil layer is 35μm thick; the ink layer is a 20μm thick ink layer (the ink is LEW7S); the pure glue layer is a 20μm thick pure glue layer (the pure glue is silicone pure glue); the second base layer is a 800μm thick ceramic substrate.
[0059] The method for preparing the dam-free COB LED substrate described in this embodiment comprises the following steps:
[0060] (1) After applying the insulating adhesive to the first base layer, the insulating adhesive layer is formed by high temperature pressing at 150° C. for 1.5 hours;
[0061] (2) After fixing the copper foil to the insulating adhesive layer, press at 100°C for 2 hours to form a copper foil layer;
[0062] (3) After printing the ink on the copper foil layer, it is cured at 25° C. for 2.5 hours to form an ink layer;
[0063] (4) After applying the pure glue to the ink layer, high temperature pressing is performed at 150° C. for 1.5 h to form a pure glue layer;
[0064] (5) After the second base layer is fixed to the pure adhesive layer, it is pressed at a high temperature of 100° C. for 2 hours to form the second base layer.
[0065] Example 3
[0066] This embodiment provides a dam-free COB LED substrate, wherein the dam-free COB LED substrate comprises a first base layer, an insulating adhesive layer, a copper foil layer, an ink layer, a pure adhesive layer, and a second base layer stacked in sequence;
[0067] The first base layer is a 900μm thick copper substrate; the insulating glue layer is a 120μm thick insulating glue layer (the insulating glue is silicone insulating glue); the copper foil layer is 35μm thick; the ink layer is a 20μm thick ink layer (the ink is LB-1900W); the pure glue layer is a 20μm thick pure glue layer (the pure glue is polyurethane pure glue); the second base layer is a 800μm thick copper substrate.
[0068] The method for preparing the dam-free COB LED substrate described in this embodiment comprises the following steps:
[0069] (1) After applying the insulating adhesive to the first base layer, the insulating adhesive is pressed at 100° C. for 2 h to form an insulating adhesive layer;
[0070] (2) After the copper foil is fixed to the insulating adhesive layer, it is pressed at a high temperature of 150°C for 1.5 hours to form a copper foil layer;
[0071] (3) After printing the ink on the copper foil layer, it is cured at 25° C. for 2.5 hours to form an ink layer;
[0072] (4) After applying the pure glue to the ink layer, high temperature pressing is performed at 150° C. for 1.5 h to form a pure glue layer;
[0073] (5) After the second base layer is fixed to the pure adhesive layer, it is pressed at a high temperature of 100° C. for 2 hours to form the second base layer.
[0074] Example 4
[0075] This embodiment provides a dam-free COB LED substrate, wherein the dam-free COB LED substrate comprises a first base layer, an insulating adhesive layer, a copper foil layer, an ink layer, a pure adhesive layer, and a second base layer stacked in sequence;
[0076] The first base layer is a 1000μm thick mirror aluminum substrate; the insulating glue layer is a 100μm thick insulating glue layer (the insulating glue is polyester insulating glue); the copper foil layer is 30μm thick; the ink layer is a 15μm thick ink layer (the ink is WT05); the pure glue layer is a 30μm thick pure glue layer (the pure glue is epoxy pure glue); the second base layer is a 700μm thick mirror aluminum substrate.
[0077] The preparation method of the dam-free COB LED substrate described in this embodiment is the same as that in Embodiment 1.
[0078] Example 5
[0079] This embodiment provides a dam-free COB LED substrate, wherein the dam-free COB LED substrate comprises a first base layer, an insulating adhesive layer, a copper foil layer, an ink layer, a pure adhesive layer, and a second base layer stacked in sequence;
[0080] The first base layer is a 800μm thick mirror aluminum substrate; the insulating glue layer is a 150μm thick insulating glue layer (the insulating glue is polyester insulating glue); the copper foil layer is 20μm thick; the ink layer is a 25μm thick ink layer (the ink is WT05); the pure glue layer is a 10μm thick pure glue layer (the pure glue is epoxy pure glue); the second base layer is a 900μm thick mirror aluminum substrate.
[0081] The preparation method of the dam-free COB LED substrate described in this embodiment is the same as that in Embodiment 1.
[0082] Comparative Example 1
[0083] This comparative example provides a COB LED substrate, which is different from Example 1 in that it does not contain a first base layer, but contains a dam, specifically: an aluminum base layer+insulating layer+copper foil layer+ink layer+silicone dam layer.
[0084] Comparative Example 2
[0085] This comparative example provides a COB LED substrate, which is different from Example 1 in that it does not contain a second base layer, but contains a dam, specifically an aluminum base layer+insulating layer+copper foil layer+ink layer+injection molded dam layer.
[0086] Performance Testing
[0087] Various performance tests were performed on the dam-free COB LED substrates provided in the above-mentioned embodiments 1-5 and the COB LED substrates provided in the comparative examples 1-2, respectively. The specific test methods are as follows:
[0088] (1) Horizontal thermal conductivity: measured by thermal imaging, refer to UTi220A;
[0089] (2) Heat dissipation capability: Based on thermal imaging test performance, refer to UTi220A;
[0090] (3) Light source life: Based on thermal imaging test performance, refer to UTi220A;
[0091] (4) Light output type: Tested with remote equipment, refer to HAAS-1200.
[0092] The specific test results are shown in Table 1:
[0093] Table 1
[0094]
[0095]
[0096] It can be seen from the test data in Table 1 that the lateral thermal conductivity of the dam-free COB LED substrate described in the present invention is 60-65°C as shown in the thermal imaging test; the heat dissipation capacity is 70-75°C as shown in the thermal imaging test; the light source life is 10000-10200H; the light emission type is 100-110° as shown in the remote device test. This fully illustrates that the present invention removes the dam process of chemical materials such as silica gel and resin used in traditional COB light sources through the substrate lamination process, and adds a pressed metal or inorganic non-metallic material substrate to the traditional COB substrate to achieve the effect of double-layer or multi-layer metal base or combined base lamination. While replacing the traditional COB light source dam operation through the shape design of the upper substrate, the lateral thermal conductivity and heat dissipation capacity of the COB light source are increased, thereby increasing the life of the COB light source, and directly performing secondary light distribution on the COB light source through the shape design of the upper substrate to ensure the light emission type.
[0097] The applicant declares that the present invention uses the above-mentioned embodiments to illustrate the damless COB LED substrate and its preparation method and application, but the present invention is not limited to the above-mentioned embodiments, that is, it does not mean that the present invention must rely on the above-mentioned embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A dam-free COB LED substrate, It is characterized in that The dam-free COB LED substrate comprises a first base layer, an insulating adhesive layer, a copper foil layer, an ink layer, a pure adhesive layer and a second base layer which are stacked in sequence; The dam-free COB LED substrate is prepared by the following method, which comprises: (1) After applying the insulating adhesive to the first base layer, the insulating adhesive layer is formed by high-temperature pressing; (2) After the copper foil is fixed to the insulating adhesive layer, it is pressed at high temperature to form a copper foil layer; (3) printing or spraying the ink on the copper foil layer and then curing it to form an ink layer; (4) After applying pure glue to the ink layer, high temperature pressing is performed to form a pure glue layer; (5) After the second base layer is fixed to the pure adhesive layer, it is pressed at high temperature to form the second base layer.
2. The dam-free COB LED substrate according to claim 1, It is characterized in that The thickness of the first base layer is 800-2000 μm.
3. The dam-free COB LED substrate according to claim 1, It is characterized in that The number of layers of the first base layer is one or more.
4. The dam-free COB LED substrate according to claim 1, It is characterized in that The first base layer is selected from any one of a copper substrate, a ceramic substrate, a mirror aluminum substrate or plastic.
5. The dam-free COB LED substrate according to claim 1, It is characterized in that The thickness of the insulating adhesive layer is 50-150 μm.
6. The dam-free COB LED substrate according to claim 1, It is characterized in that The insulating adhesive layer is formed by high-temperature curing of insulating adhesive, and the insulating adhesive is selected from polyester insulating adhesive and / or epoxy insulating adhesive.
7. The dam-free COB LED substrate according to claim 6, It is characterized in that The high temperature curing temperature is 100-150°C.
8. The dam-free COB LED substrate according to claim 1, It is characterized in that The thickness of the copper foil layer is 20-50 μm.
9. The dam-free COB LED substrate according to claim 1, It is characterized in that The thickness of the ink layer is 10-30 μm.
10. The dam-free COB LED substrate according to claim 1, It is characterized in that The ink layer is selected from any one of WT05, LEW7S or LB-1900W or a combination of at least two thereof.
11. The dam-free COB LED substrate according to claim 1, It is characterized in that The thickness of the pure glue layer is 10-30 μm.
12. The dam-free COB LED substrate according to claim 1, It is characterized in that The pure adhesive layer is selected from any one of epoxy, silicone or polyurethane, or a combination of at least two of them.
13. The dam-free COB LED substrate according to claim 1, It is characterized in that The thickness of the second base layer is 700-2000 μm.
14. The dam-free COB LED substrate according to claim 1, It is characterized in that The number of layers of the second base layer is one or more.
15. The dam-free COB LED substrate according to claim 1, It is characterized in that The second base layer is selected from any one of a copper substrate, a ceramic substrate, a mirror aluminum substrate, and plastic.
16. The method for preparing a dam-free COB LED substrate according to any one of claims 1 to 15, It is characterized in that The method for preparing the dam-free COB LED substrate comprises the following steps: (1) After applying the insulating adhesive to the first base layer, the insulating adhesive layer is formed by high-temperature pressing; (2) After the copper foil is fixed to the insulating adhesive layer, it is pressed at high temperature to form a copper foil layer; (3) printing or spraying the ink on the copper foil layer and then curing it to form an ink layer; (4) After applying pure glue to the ink layer, high temperature pressing is performed to form a pure glue layer; (5) After the second base layer is fixed to the pure adhesive layer, it is pressed at high temperature to form the second base layer.
17. The method for preparing a dam-free COB LED substrate according to claim 16, It is characterized in that In step (1), step (2), step (3) and step (4), the temperature of the high temperature pressing is independently 100-150° C., and the time of the high temperature pressing is independently 1.5-2 h.
18. The method for preparing the dam-free COB LED substrate according to claim 16, It is characterized in that The curing in step (3) is natural curing and / or baking curing.
19. The method for preparing a dam-free COB LED substrate according to claim 18, It is characterized in that The temperature of the natural curing is 20-30° C., and the time of the natural curing is 2-3 hours.
20. The method for preparing a dam-free COB LED substrate according to claim 18, It is characterized in that The baking and curing temperature is 100-110° C., and the baking and curing time is 0.1-1 h.
21. Use of the dam-free COB LED substrate according to any one of claims 1 to 15 in preparing an LED light source.