A special-shaped graphite crucible and a method for preparing silicon carbide polycrystalline powder using the graphite crucible

By designing a special-shaped graphite crucible, using step-shaped columns to support the screen plate and silicon-carbon mixed protective material, the existing graphite crucible is easily worn and the powder purity is low, and the efficient preparation of high-purity silicon carbide polycrystalline powder is achieved and The increase in the number of times of use of crucibles reduces production costs.

CN112877778BActive Publication Date: 2024-11-19SHAOXING JINGCAI TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110268810.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-03-12
Publication Date
2024-11-19
Estimated Expiration
2041-03-12

AI Technical Summary

Technical Problem

Existing graphite crucibles are prone to wear and difficult to improve the purity of silicon carbide polycrystalline powder, resulting in high production costs and poor powder quality.

Method used

A special-shaped graphite crucible was designed, including an upper cover, crucible body and external threaded graphite tube. The screen plate crucible is supported by step-shaped columns, combined with silicon-carbon mixed protective material, and fully contacted with carbon powder using silicon steam to prepare high-purity silicon carbide. Polycrystalline powder.

Benefits of technology

The purity of silicon carbide polycrystalline powder and the number of crucibles are improved, the wear rate and production cost are reduced, and the efficient preparation of high-purity powder is achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112877778B_ABST
    Figure CN112877778B_ABST
Patent Text Reader

Abstract

A special-shaped graphite crucible and a method for preparing silicon carbide polycrystalline powder using the graphite crucible, which relates to a special-shaped graphite crucible and a method for using the same, and aims to solve the technical problems of easy wear of the existing graphite crucible and low purity of the polycrystalline powder. The crucible includes an upper cover, a crucible body, a sub-crucible and an externally threaded graphite tube; a column lowered in a step-like manner is arranged in the crucible body, the sub-crucible is placed on the step of the column, the tube wall of the crucible body is evenly distributed with air holes, and the upper cover is connected to the crucible body with an externally threaded graphite tube. Usage: Place silicon at the bottom of the shell; place carbon powder in the sub-crucible, and then place the sub-crucible on the step of the column; tighten the upper cover and the shell with an externally threaded graphite tube and place them in a high-temperature furnace; introduce gas into the bottom of the shell through the externally threaded graphite tube, heat up the reaction, and obtain high-purity silicon carbide polycrystalline powder. The graphite crucible has a low wear rate, and the silicon carbide polycrystalline prepared by using 7N-9N silicon particles or silicon blocks has a purity of 6N, and is used in the field of silicon carbide preparation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a special-shaped graphite crucible and to the field of SiC polycrystalline powder preparation. Background Art

[0002] With the rapid development of the semiconductor field, SiC materials are considered to be ideal materials for the third generation of semiconductors because of their advantages such as large bandgap, high thermal conductivity, large electron saturation drift rate, high critical breakdown electric field, low dielectric constant and good chemical stability. With the development of single crystal technology, the market demand for high-purity silicon carbide polycrystalline powder is growing. At present, high-purity silicon carbide polycrystalline powder is mainly prepared by carbon thermal reduction, chemical vapor infiltration and chemical vapor deposition. The prepared polycrystalline powder is greatly affected by the purity of the raw materials. It is difficult to highly purify the powdered raw materials by conventional methods, which makes it difficult to improve the purity of the polycrystalline powder. In addition, a high-purity graphite crucible is usually used as a reaction container. The structure of a general graphite crucible is a hollow cylindrical shape. The crucible wall is at right angles to the bottom of the crucible. The stress it bears during use is small. When Si changes from a solid to a molten state, the stress increases. In severe cases, the crucible will break. At the same time, the general crucible is generally eroded by Si at high temperatures, so that the graphite crucible will be scrapped after a few uses. The number of uses seriously affects the production cost. Summary of the invention

[0003] The present invention aims to solve the technical problems of easy wear of existing graphite crucibles and low purity of polycrystalline powder, and provides a special-shaped graphite crucible and a method for preparing silicon carbide polycrystalline powder using the graphite crucible. The new protective special-shaped graphite crucible is suitable for preparing high-purity silicon carbide polycrystalline powder by silicon evaporation method.

[0004] The special-shaped graphite crucible of the present invention comprises an upper cover, a crucible body, a sub-crucible and an externally threaded graphite tube;

[0005] The upper cover is composed of a cylindrical cover body and a partition located in the middle of the cover body. An internal threaded hole is arranged on the partition. The upper part of the partition and the cover body form an upper cavity, and the lower part of the partition and the cover body form a lower cavity. The upper cavity is used to contain the silicon-carbon mixed protective material.

[0006] The crucible body consists of a shell, at least three stepped columns and a protective groove.

[0007] The outer wall of the shell is cylindrical;

[0008] The inner wall of the shell is cylindrical, and the bottom of the shell is arc-shaped; there is an annular boss at the intersection of the bottom and the inner wall, and the bosses are evenly distributed on the boss in a stepped manner, and the columns are connected to the inner wall of the shell as a whole or fixedly connected together;

[0009] The air holes are evenly distributed in the cylindrical wall of the shell; the upper openings of the air holes are arranged on the upper end surface of the shell, and the lower openings of the air holes are arranged on the side wall of the annular boss;

[0010] The bottom and wall of the sub-crucible are made of sieve plates, and the sub-crucible is placed on the steps of the pillars; the pillars are used as the support of the sub-crucible;

[0011] The protection groove is arranged along the outer edge of the upper opening of the shell, and the upper opening of the protection groove is higher than the contact surface between the upper cover and the shell; the protection groove is used to contain the silicon-carbon mixed protection material; the contact surface between the upper cover and the shell is buried in the silicon-carbon mixed protection material;

[0012] An internal thread is provided at the upper opening of the air hole in the cylinder wall of the shell, and the upper opening of the air hole corresponds to the position of the internal thread hole of the upper cover, and both are matched with the external thread of the externally threaded graphite tube; the externally threaded graphite tube connects the upper cover with the shell, and can be connected with the air hole through the cavity of the externally threaded graphite tube.

[0013] The method of preparing polycrystalline silicon carbide powder by using a special-shaped graphite crucible of the present invention is as follows:

[0014] Place 7N~9N high purity silicon particles or silicon blocks at the bottom of the shell;

[0015] The carbon powder is placed in the sub-crucible, and the sub-crucible is then placed on the step of the column; the column serves to fix the sub-crucible and to leave a certain space between the inner wall of the shell and the sub-crucible, which is convenient for silicon vapor to diffuse;

[0016] Put the upper cover on the shell, and keep the upper opening of the air hole of the shell corresponding to the position of the internal thread hole of the upper cover, and then tighten it with the external thread graphite tube;

[0017] The protective special-shaped graphite crucible is placed in a high-temperature furnace;

[0018] Connect the externally threaded graphite tube to a gas source; the gas source is argon or hydrogen;

[0019] Put the silicon-carbon mixed protective material into the protective groove of the crucible body and the upper cavity of the upper cover;

[0020] 7. Open the gas source valve to introduce gas into the bottom of the shell through the external threaded graphite tube, raise the temperature of the high-temperature furnace to 1600~2100℃, maintain for 6~12h, and obtain high-purity silicon carbide polycrystalline powder.

[0021] The protective special-shaped graphite crucible of the present invention utilizes the wide-mouth upper cover and the protective groove of the crucible to contain the silicon-carbon mixed protective material; utilizes the stepped lowered columns to support the sieve plate sub-crucible, the stepped columns can ensure that the silicon vapor fills the interior of the crucible, and a gas channel is provided deep in the cylinder wall of the shell 2-1, so that the Si vapor and the C powder are fully in contact with each other through gas disturbance; the bottom of the shell adopts an arc shape, which can not only make the stress that can be borne greater, but also make the heating faster and more uniform, so as to ensure the gasification speed of silicon and the concentration of silicon vapor; the sieve plate sub-crucible adopts a honeycomb porous structure, so as to ensure the mechanical properties of the sub-crucible and the air permeability at the same time, and is convenient to use tools to pull; one or more sub-crucibles can be placed in the shell, so that the contact of the raw materials is more uniform, and a certain space is left between the inner wall of the shell and the sub-crucible, so as to facilitate the diffusion of silicon vapor. After the production is completed, the sub-crucible is taken out to collect the product, so that the purity of the product is improved and the wear rate of the graphite crucible is reduced, the number of uses is increased, and the production cost is reduced. At the same time, the use of silicon particles or silicon blocks with higher purity is conducive to the use of high vacuum in the early stage of the reaction to remove impurities introduced during the loading process, which can ensure that the impurity content in the system is less than 1ppm, further improving the purity of SiC polycrystalline powder.

[0022] The protective special-shaped graphite crucible of the invention is used in the field of preparing silicon carbide polycrystalline powder. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 1 is a schematic diagram of the overall structure of the protective special-shaped graphite crucible of Example 1;

[0024] Figure 2 is a schematic diagram of the cross-sectional structure of the upper cover 1 of Example 1;

[0025] Figure 3 1 is a schematic structural diagram of a crucible body 2 of a protective special-shaped graphite crucible of Example 1;

[0026] Figure 4 is a schematic diagram of a three-dimensional cross-sectional structure of a protective special-shaped graphite crucible of Example 1;

[0027] Figure 5 is a schematic cross-sectional structure diagram of a protective special-shaped graphite crucible of Example 1;

[0028] Figure 6 is a schematic structural diagram of the sub-crucible of Example 1;

[0029] Figure 7 This is a schematic diagram of the cross-sectional structure of the protective special-shaped graphite crucible of Example 2.

[0030] In the figure: 1 is the upper cover, 1-1 is the cover body, 1-2 is the partition, 1-3 is the internal thread hole, 1-4 is the upper cavity, and 1-5 is the lower cavity;

[0031] 2 is the crucible body, 2-1 is the shell, 2-1-1 is the air hole, 2-2 is the column, 2-3 is the protection groove, and 2-4 is the boss;

[0032] 3 is a sub-crucible, and 4 is an externally threaded graphite tube. DETAILED DESCRIPTION

[0033] Specific implementation method 1: (see attached Figures 1 to 6 ) The protective special-shaped graphite crucible of this embodiment includes an upper cover 1, a crucible body 2, a sub-crucible 3 and an externally threaded graphite tube 4;

[0034] The upper cover 1 is composed of a cylindrical cover body 1-1 and a partition 1-2 located in the middle of the cover body. An internal threaded hole 1-3 is provided on the partition 1-2. The upper part of the partition 1-2 and the cover body form an upper cavity 1-4, and the lower part of the partition 1-2 and the cover body form a lower cavity 1-5. The upper cavity 1-4 is used to contain silicon-carbon mixed protective material.

[0035] The crucible body 2 is composed of a shell 2-1, at least three stepped columns 2-2 and a protective groove 2-3.

[0036] The bottom of the housing 2-1 is arc-shaped;

[0037] The outer wall of the housing 2-1 is cylindrical;

[0038] The inner wall of the shell 2-1 is cylindrical, and the columns 2-2 are evenly distributed on the cylindrical inner wall and are stepped down, and the columns 2-2 are connected to the inner wall of the shell as a whole or fixed together;

[0039] At least three air holes 2-1-1 are evenly distributed in the cylinder wall of the shell 2-1; the upper opening of the air hole 2-1-1 is arranged at the upper end surface of the shell 2-1, and the lower opening of the air hole 2-1-1 is arranged at the lower part of the inner wall of the shell 2-1;

[0040] The bottom and wall of the sub-crucible 3 are made of sieve plates, and the sub-crucible 3 is placed on the step of the column 2-2; the column 2-2 is used as a support body for the sub-crucible 3;

[0041] The protection groove 2-3 is arranged along the outer edge of the upper opening of the shell 2-1, and the upper opening of the protection groove 2-3 is higher than the contact surface between the upper cover 1 and the shell 2-1; the protection groove 2-1-2 is used to contain the silicon-carbon mixed protection material; the contact surface between the upper cover 1 and the shell 2-1 is buried in the silicon-carbon mixed protection material;

[0042] An internal thread is provided at the upper opening of the air hole 2-1-1 in the cylinder wall of the shell 2-1, and the upper opening of the air hole 2-1-1 corresponds to the position of the internal threaded hole 1-3 of the upper cover 1, and both are matched with the external thread of the externally threaded graphite tube 4; the externally threaded graphite tube 4 not only connects the upper cover 1 with the shell 2-1, but also can be connected with the air hole 2-1-1 through the cavity of the externally threaded graphite tube 4.

[0043] Specific implementation method 2: This implementation method is different from the specific implementation method 1 in that the number of the stepped lowered columns 2 - 2 is 3 to 6; the rest is the same as the specific implementation method 1.

[0044] Specific implementation method three: This implementation method is different from specific implementation method one or two in that the number of steps of the stepped lowering columns 2 - 2 is 2 to 6; the rest is the same as specific implementation method one or two.

[0045] In this embodiment, a sub-crucible 3 can be placed on each step, which can increase the output and improve the uniformity of the product.

[0046] Specific implementation method 4: This implementation method is different from specific implementation methods 1 to 3 in that the columns 2-2 and the air holes 2-1-1 are arranged alternately on the circumference of the shell 2-1; the rest is the same as specific implementation methods 1 to 3.

[0047] Specific implementation method five: This implementation method is different from specific implementation methods one to four in that the number of air holes 2-1-1 is 3 to 6; the rest is the same as specific implementation methods one to four.

[0048] Specific implementation method 6: This implementation method is different from specific implementation methods 1 to 5 in that the sieve plate of the sub-crucible is a honeycomb porous structure; the rest is the same as specific implementation methods 1 to 5.

[0049] The sieve plate of the sub-crucible in this embodiment has a honeycomb porous structure, which ensures the mechanical properties of the sub-crucible and at the same time has air permeability.

[0050] Specific embodiment 7: This embodiment is different from specific embodiments 1 to 6 in that the thickness of the side wall and the bottom of the sub-crucible 3 is 5 mm to 10 mm; the rest is the same as specific embodiments 1 to 6.

[0051] Specific embodiment eight: This embodiment is different from specific embodiments one to seven in that the diameter of the honeycomb holes of the sub-crucible 3 is 0.01-0.5 mm; the rest is the same as specific embodiments one to seven.

[0052] Specific embodiment 9: The method for using the protective special-shaped graphite crucible described in specific embodiment 1 is as follows:

[0053] Place 7N~9N high purity silicon particles or silicon blocks at the bottom of the shell;

[0054] The carbon powder is placed in the sub-crucible, and the sub-crucible is then placed on the step of the column; the column serves to fix the sub-crucible and to leave a certain space between the inner wall of the shell and the sub-crucible, which is convenient for silicon vapor to diffuse;

[0055] Put the upper cover on the shell, and keep the upper opening of the air hole of the shell corresponding to the position of the internal thread hole of the upper cover, and then tighten it with the external thread graphite tube;

[0056] The protective special-shaped graphite crucible is placed in a high-temperature furnace;

[0057] Connect the externally threaded graphite tube to a gas source; the gas source is argon or hydrogen;

[0058] Put the silicon-carbon mixed protective material into the protective groove of the crucible body and the upper cavity of the upper cover;

[0059] Open the gas source valve to introduce gas into the bottom of the shell through the externally threaded graphite tube, raise the temperature of the high-temperature furnace to 1600~2100℃, and maintain it for 6~12h to obtain high-purity silicon carbide polycrystalline powder.

[0060] Specific implementation method ten: This implementation method is different from specific implementation method nine in that the purity of the gas source is ≥ 6N, and the rest is the same as specific implementation method nine.

[0061] Use the following examples to verify the beneficial effects of the present invention:

[0062] Embodiment 1: The protective special-shaped graphite crucible of this embodiment is composed of an upper cover 1, a crucible body 2, a sub-crucible 3 and an externally threaded graphite tube 4;

[0063] The upper cover 1 is composed of a cylindrical cover body 1-1 and a partition 1-2 located in the middle of the cover body. An internal threaded hole 1-3 is provided on the partition 1-2. The upper part of the partition 1-2 and the cover body form an upper cavity 1-4, and the lower part of the partition 1-2 and the cover body form a lower cavity 1-5. The upper cavity 1-4 is used to contain silicon-carbon mixed protective material.

[0064] The crucible body 2 is composed of a shell 2-1, three stepped columns 2-2 and a protective groove 2-3;

[0065] The inner wall of the shell 2-1 is cylindrical, and the bottom of the shell 2-1 is arc-shaped; there is an annular boss 2-4 at the intersection of the bottom and the inner wall, and three stepped columns 2-2 are evenly distributed on the boss 2-4, each column 2-2 has two steps, and the column 2-2 is fixedly connected to the inner wall of the shell;

[0066] Three air holes 2-1-1 are evenly distributed in the cylinder wall of the shell 2-1; the upper opening of the air hole 2-1-1 is set on the upper end surface of the shell 2-1, and the lower opening of the air hole 2-1-1 is on the side wall of the annular boss 2-4;

[0067] The bottom and wall of the sub-crucible 3 are made of a sieve plate with honeycomb holes, the thickness of the sieve plate is 5 mm, and the aperture of the honeycomb holes is 0.5 mm. The sub-crucible 3 is placed on the step of the column 2-2; the column 2-2 is used as a support body of the sub-crucible 3;

[0068] The protection groove 2-3 is arranged along the outer edge of the upper opening of the shell 2-1, and the upper opening of the protection groove 2-3 is higher than the contact surface between the upper cover 1 and the shell 2-1; the protection groove 2-1-2 is used to contain the silicon-carbon mixed protection material; the contact surface between the upper cover 1 and the shell 2-1 is buried in the silicon-carbon mixed protection material;

[0069] An internal thread is provided at the upper opening of the air hole 2-1-1 in the cylinder wall of the shell 2-1, and the upper opening of the air hole 2-1-1 corresponds to the position of the internal thread hole 1-3 of the upper cover 1, and both are matched with the external thread of the externally threaded graphite tube 4; the externally threaded graphite tube 4 not only connects the upper cover 1 with the shell 2-1, but also communicates with the air hole 2-1-1 through the cavity of the externally threaded graphite tube 4;

[0070] The protective special-shaped graphite crucible of Example 1 is used to prepare high-purity silicon carbide polycrystalline powder, and the specific steps are as follows:

[0071] 1. Place 7N high-purity silicon particles at the bottom of the shell 2-1;

[0072] 2. Place C powder in the sub-crucible 3, and then place the sub-crucible 3 on the step of the column 2-2; the column 2-2 serves to fix the sub-crucible and to leave a certain space between the inner wall of the shell 2-1 and the sub-crucible to facilitate the diffusion of silicon vapor;

[0073] 3. Cover the upper cover 1 on the shell 2-1, and keep the upper opening of the air hole 2-1-1 of the shell 2-1 corresponding to the position of the internal thread hole 1-3 of the upper cover 1, and then tighten it with the external thread graphite tube 4;

[0074] 4. The protective special-shaped graphite crucible is placed in a high-temperature furnace;

[0075] 5. Connect the externally threaded graphite tube 4 to the argon gas source;

[0076] 6. Put the silicon-carbon mixed protective material into the protective groove 2-3 of the crucible body 2 and the upper cavity 1-4 of the upper cover 1;

[0077] 7. Open the argon gas source valve to introduce argon gas with a purity of 6N into the bottom of the shell 2-1 through the externally threaded graphite tube 4, raise the temperature of the high-temperature furnace to 2000°C, and maintain it for 12 hours to obtain high-purity silicon carbide polycrystalline powder.

[0078] The purity of the high-purity silicon carbide polycrystalline powder prepared by the protective special-shaped graphite crucible of this embodiment 1 reaches 6N, and the preparation process of the high-purity silicon carbide polycrystalline powder does not wear the protective special-shaped graphite crucible, and the protective special-shaped graphite crucible can be reused many times.

[0079] Example 2: (See attached Figure 7) The protective special-shaped graphite crucible of this embodiment is composed of an upper cover 1, a crucible body 2, two sub-crucibles 3 and an externally threaded graphite tube 4;

[0080] The upper cover 1 is composed of a cylindrical cover body 1-1 and a partition 1-2 located in the middle of the cover body. An internal threaded hole 1-3 is provided on the partition 1-2. The upper part of the partition 1-2 and the cover body form an upper cavity 1-4, and the lower part of the partition 1-2 and the cover body form a lower cavity 1-5. The upper cavity 1-4 is used to contain silicon-carbon mixed protective material.

[0081] The crucible body 2 is composed of a shell 2-1, three stepped columns 2-2 and a protective groove 2-3;

[0082] The inner wall of the shell 2-1 is cylindrical, and the bottom of the shell 2-1 is arc-shaped; there is an annular boss 2-4 at the intersection of the bottom and the inner wall, and three stepped columns 2-2 are evenly distributed on the boss 2-4, each column 2-2 has three steps, and the column 2-2 is fixedly connected to the inner wall of the shell;

[0083] Three air holes 2-1-1 are evenly distributed in the cylinder wall of the shell 2-1; the upper opening of the air hole 2-1-1 is set on the upper end surface of the shell 2-1, and the lower opening of the air hole 2-1-1 is on the side wall of the annular boss 2-4;

[0084] The bottom and wall of the sub-crucible 3 are made of a sieve plate with honeycomb holes, the thickness of the sieve plate is 5 mm, and the aperture of the honeycomb holes is 0.5 mm. The two sub-crucibles 3 are placed on two steps of the column 2-2 respectively; the column 2-2 is used as a support body for the sub-crucible 3;

[0085] The protection groove 2-3 is arranged along the outer edge of the upper opening of the shell 2-1, and the upper opening of the protection groove 2-3 is higher than the contact surface between the upper cover 1 and the shell 2-1; the protection groove 2-1-2 is used to contain the silicon-carbon mixed protection material; the contact surface between the upper cover 1 and the shell 2-1 is buried in the silicon-carbon mixed protection material;

[0086] An internal thread is provided at the upper opening of the air hole 2-1-1 in the cylinder wall of the shell 2-1, and the upper opening of the air hole 2-1-1 corresponds to the position of the internal thread hole 1-3 of the upper cover 1, and both are matched with the external thread of the externally threaded graphite tube 4; the externally threaded graphite tube 4 not only connects the upper cover 1 with the shell 2-1, but also communicates with the air hole 2-1-1 through the cavity of the externally threaded graphite tube 4;

[0087] The protective special-shaped graphite crucible of Example 1 is used to prepare high-purity silicon carbide polycrystalline powder, and the specific steps are as follows:

[0088] 1. Place 7N high-purity silicon particles at the bottom of the shell 2-1;

[0089] 2. Place C powder in two sub-crucibles 3, and then place the two sub-crucibles 3 on two steps of the column 2-2 respectively; the column 2-2 serves to fix the sub-crucibles and to leave a certain space between the inner wall of the shell 2-1 and the sub-crucibles to facilitate the diffusion of silicon vapor;

[0090] 3. Cover the upper cover 1 on the shell 2-1, and keep the upper opening of the air hole 2-1-1 of the shell 2-1 corresponding to the position of the internal thread hole 1-3 of the upper cover 1, and then tighten it with the external thread graphite tube 4;

[0091] 4. The protective special-shaped graphite crucible is placed in a high-temperature furnace;

[0092] 5. Connect the externally threaded graphite tube 4 to the argon gas source;

[0093] 6. Put the silicon-carbon mixed protective material into the protective groove 2-3 of the crucible body 2 and the upper cavity 1-4 of the upper cover 1;

[0094] 7. Open the argon gas source valve to introduce argon gas with a purity of 6N into the bottom of the shell 2-1 through the externally threaded graphite tube 4, raise the temperature of the high-temperature furnace to 2100°C, and maintain it for 12 hours to obtain high-purity silicon carbide polycrystalline powder.

[0095] The purity of the high-purity silicon carbide polycrystalline powder prepared by the protective special-shaped graphite crucible of this embodiment 1 reaches 6N, and the preparation process of the high-purity silicon carbide polycrystalline powder does not wear the protective special-shaped graphite crucible, and the protective special-shaped graphite crucible can be reused many times.

Claims

1. A special-shaped graphite crucible, characterized in that The graphite crucible comprises an upper cover (1), a crucible body (2), a sub-crucible (3) and an externally threaded graphite tube (4); The upper cover (1) is composed of a cylindrical cover body (1-1) and a partition layer (1-2) located in the middle of the cover body, an internal threaded hole (1-3) is provided on the partition layer (1-2), the upper part of the partition layer (1-2) and the cover body form an upper cavity (1-4), and the lower part of the partition layer (1-2) and the cover body form a lower cavity (1-5); The crucible body (2) is composed of a shell (2-1), 3 to 6 columns (2-2) that are lowered in a step-like manner, and a protective groove (2-3); The outer wall of the shell (2-1) is cylindrical; The inner wall of the shell (2-1) is cylindrical, and the bottom of the shell (2-1) is arc-shaped; an annular boss (2-4) is provided at the intersection of the bottom and the inner wall; columns (2-2) are evenly distributed on the boss (2-4) and are stepped down; the columns (2-2) are connected to the inner wall of the shell as a whole or fixedly connected together; the number of steps of the columns (2-2) is 2 to 6; Three to six air holes (2-1-1) are evenly distributed in the cylindrical wall of the shell (2-1); the upper opening of the air hole (2-1-1) is arranged on the upper end surface of the shell (2-1), and the lower opening of the air hole (2-1-1) is on the side wall of the annular boss (2-4); the upright columns (2-2) and the air holes (2-1-1) are arranged alternately on the circumference of the shell (2-1); The bottom and wall of the sub-crucible (3) are made of a sieve plate with a honeycomb porous structure, the aperture of the honeycomb holes is 0.01-0.5 mm, the side wall and bottom thickness of the sub-crucible (3) are 5 mm-10 mm, and the sub-crucible (3) is placed on the step of the column (2-2); the column (2-2) serves as a support body for the sub-crucible (3); The protection groove (2-3) is arranged along the outer edge of the upper opening of the shell (2-1), and the upper opening of the protection groove (2-3) is higher than the contact surface between the upper cover (1) and the shell (2-1); An internal thread is provided at the upper opening of the air hole (2-1-1) in the cylinder wall of the shell (2-1); the upper opening of the air hole (2-1-1) corresponds to the position of the internal thread hole (1-3) of the upper cover (1), and both are matched with the external thread of the externally threaded graphite tube (4).

2. A method for preparing polycrystalline silicon carbide powder using the special-shaped graphite crucible according to claim 1, characterized in that The method proceeds as follows: Place 7N~9N silicon particles or silicon blocks at the bottom of the shell; The carbon powder is placed in the sub-crucible, and the sub-crucible is then placed on the step of the column; the column serves to fix the sub-crucible and to leave a certain space between the inner wall of the shell and the sub-crucible, which is convenient for silicon vapor to diffuse; Put the upper cover on the shell, and keep the upper opening of the air hole of the shell corresponding to the position of the internal thread hole of the upper cover, and then tighten it with the external thread graphite tube; The protective special-shaped graphite crucible is placed in a high-temperature furnace; Connect the externally threaded graphite tube to a gas source; the gas source is argon or hydrogen; Put the silicon-carbon mixed protective material into the protective groove of the crucible body and the upper cavity of the upper cover; Open the gas source valve to introduce gas into the bottom of the shell through the externally threaded graphite tube, raise the temperature of the high-temperature furnace to 1600~2100 ℃, and maintain it for 6~12 hours to obtain high-purity silicon carbide polycrystalline powder.

3. The method for preparing polycrystalline silicon carbide powder by using the special-shaped graphite crucible according to claim 1 according to claim 2, characterized in that The purity of the gas source is ≥6N.