Semiconductor structure and method for forming the same

By forming a sacrificial layer on the fins of the semiconductor structure and oxidizing treatment, the problem of large fin losses is solved, and precise control of fin size and improvement of electrical performance is achieved.

CN112928163BActive Publication Date: 2024-11-19SEMICON MFG INT (SHANGHAI) CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201911235973.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-12-05
Publication Date
2024-11-19
Estimated Expiration
2039-12-05

AI Technical Summary

Technical Problem

In semiconductor manufacturing, the loss of the fin is large, making it difficult to accurately control the size, affecting the satisfaction of process requirements.

Method used

The sacrificial layer is formed on the top surface and side walls of the fins and the substrate surface, and is converted into an oxide layer by oxidation treatment to form the gate oxide layer, thereby reducing consumption and loss to the fins.

Benefits of technology

Through this method, the size of the fin can be accurately controlled, the loss can be reduced, the process requirements can be met, and the electrical performance of the gate oxide layer can be improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112928163B_ABST
    Figure CN112928163B_ABST
Patent Text Reader

Abstract

A semiconductor structure and a method for forming the same, the method comprising: providing a base, the base comprising a substrate and a fin protruding from the substrate; forming a sacrificial layer on the top surface and sidewalls of the fin and the surface of the substrate; and performing an oxidation treatment on the sacrificial layer to convert the sacrificial layer into an oxide layer. In the embodiment of the present invention, by forming the sacrificial layer, in the step of forming the oxide layer, the sacrificial layer is oxidized to consume the material of the sacrificial layer to form the oxide layer, thereby facilitating the prevention of consumption of the fin and reducing the loss of the fin, and further facilitating the precise control of the size of the fin so that the size of the fin meets the process requirements.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The embodiments of the present invention relate to the field of semiconductor manufacturing, and in particular to a semiconductor structure and a method for forming the same. Background Art

[0002] In semiconductor manufacturing, with the development trend of ultra-large-scale integrated circuits, the feature size of integrated circuits continues to decrease. In order to adapt to smaller feature sizes, the channel length of metal-oxide-semiconductor field-effect transistors (MOSFETs) is also shortened accordingly. However, as the channel length of the device shortens, the distance between the source and drain of the device also shortens, so the control ability of the gate structure over the channel becomes worse, and the difficulty of pinching off the channel by the gate voltage becomes increasingly greater, making the subthreshold leakage phenomenon, the so-called short-channel effect (SCE: short-channel effects) more likely to occur.

[0003] Therefore, in order to reduce the impact of the short channel effect, semiconductor processes have gradually begun to transition from planar MOSFETs to three-dimensional transistors with higher efficiency, such as fin field effect transistors (FinFETs). In FinFETs, the gate structure can control the ultra-thin body (fin) from at least two sides. Compared with planar MOSFETs, the gate structure has a stronger control over the channel and can effectively suppress the short channel effect; and FinFETs have better compatibility with existing integrated circuit manufacturing than other devices. Summary of the invention

[0004] The problem solved by the embodiments of the present invention is to provide a semiconductor structure and a method for forming the same, so as to reduce the loss of the fin.

[0005] To solve the above problems, an embodiment of the present invention provides a method for forming a semiconductor structure, comprising: providing a base, the base comprising a substrate and a fin protruding from the substrate; forming a sacrificial layer on the top surface and side walls of the fin, and the surface of the substrate; and oxidizing the sacrificial layer to convert the sacrificial layer into an oxide layer.

[0006] Optionally, after providing the substrate and before forming the sacrificial layer, the method for forming the semiconductor structure further includes: forming a buffer layer on the top surface and side walls of the fin and the surface of the substrate; in the step of forming the sacrificial layer, the sacrificial layer is formed on the buffer layer; after forming the oxide layer, the oxide layer and the buffer layer are used to constitute a gate oxide layer.

[0007] Optionally, it is characterized in that an atomic layer deposition process is used to form a buffer layer on the top surface and side walls of the fin and the surface of the substrate.

[0008] Optionally, a plasma enhanced atomic layer deposition process is used to form a buffer layer on the top surface and sidewalls of the fin and the surface of the substrate.

[0009] Optionally, the plasma enhanced atomic layer deposition process uses an output power of 0 to 200W.

[0010] Optionally, in the step of forming the buffer layer, the thickness of the buffer layer is

[0011] Optionally, in the step of forming the buffer layer, the material of the buffer layer includes silicon oxide.

[0012] Optionally, the oxide layer is made of the same material as the buffer layer.

[0013] Optionally, after forming the buffer layer and before forming the sacrificial layer, the method for forming the semiconductor structure further includes: performing plasma treatment on the buffer layer in an oxygen-containing gas atmosphere, which is suitable for improving the density of the buffer layer.

[0014] Optionally, after forming the buffer layer and before forming the sacrificial layer, the method for forming the semiconductor structure further includes: performing microwave treatment on the buffer layer, which is suitable for improving the density of the buffer layer.

[0015] Optionally, the output power used in the plasma treatment is 0-100W.

[0016] Optionally, the sacrificial layer is formed by a furnace tube process.

[0017] Optionally, the temperature of the furnace tube process is 300-400°C.

[0018] Optionally, the sacrificial layer is oxidized by a thermal oxidation process.

[0019] Correspondingly, an embodiment of the present invention also provides a semiconductor structure, comprising: a base, the base comprising a substrate and a fin protruding from the substrate; a sacrificial layer, located on the top and side walls of the fin, and the surface of the substrate, the sacrificial layer being suitable for being converted into an oxide layer through oxidation treatment.

[0020] Optionally, the semiconductor structure further includes: a buffer layer located between the substrate and the sacrificial layer.

[0021] Optionally, the material of the buffer layer includes silicon oxide.

[0022] Optionally, the thickness of the buffer layer is

[0023] Optionally, the material of the sacrificial layer is the same as that of the fin.

[0024] Optionally, the thickness of the sacrificial layer is

[0025] Compared with the prior art, the technical solution of the embodiment of the present invention has the following advantages:

[0026] In the method for forming a semiconductor structure provided by an embodiment of the present invention, before forming an oxide layer, a sacrificial layer is also formed on the top surface and side wall of the fin and the surface of the substrate. Therefore, in the step of forming the oxide layer, the sacrificial layer is oxidized to consume the material of the sacrificial layer to form the oxide layer, which is beneficial to prevent consumption of the fin and reduce the loss of the fin, and further beneficial to accurately control the size of the fin so that the size of the fin meets the process requirements. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 It is a schematic structural diagram corresponding to each step in a method for forming a semiconductor structure;

[0028] Figures 2 to 4 It is a schematic structural diagram corresponding to each step in another method for forming a semiconductor structure;

[0029] Figures 5 to 9 is a schematic structural diagram corresponding to each step in an embodiment of a method for forming a semiconductor structure of the present invention;

[0030] Fig.10 It is a schematic diagram of the partial structure of the fin and the gate oxide layer formed by the formation method of the embodiment of the present invention and the consumption of the fin. DETAILED DESCRIPTION

[0031] At present, the consumption of the fins is relatively large when the gate oxide layer is formed. Now, the reason why the consumption of the fins is relatively large when the gate oxide layer is formed is analyzed in combination with a method for forming a semiconductor structure.

[0032] Figure 1 A structural schematic diagram corresponding to each step in a method for forming a semiconductor structure is shown.

[0033] refer to Figure 1 , providing a substrate, the substrate comprising a substrate 1 and a fin 2 protruding from the substrate 1 .

[0034] Continue to refer Figure 1 A plasma enhanced atomic layer deposition process is used to form a gate oxide layer 3 on the surface of the substrate 1 and on the top surface and sidewalls of the fin 2.

[0035] In the formation method, a plasma enhanced atomic layer deposition process is directly used to form a gate oxide layer 3 on the surface of the substrate 1 and on the top surface and side walls of the fin 2. The oxygen plasma used in the plasma enhanced atomic layer deposition process directly contacts the fin 2, thereby consuming part of the fin 2, which easily leads to a large loss of the fin 2, and further makes it difficult to accurately control the size of the fin 2, resulting in the size of the fin 2 being difficult to meet the process requirements.

[0036] Figures 2 to 4 A structural schematic diagram corresponding to each step in another method for forming a semiconductor structure is shown.

[0037] refer to Figure 2 , providing a substrate, the substrate comprising a substrate 10 and a fin 11 protruding from the substrate 10 .

[0038] refer to Figure 3 A plasma enhanced atomic layer deposition process is used to form a first oxide layer 12 on the surface of the substrate 10 and on the top and sidewalls of the fin 11.

[0039] refer to Figure 4 A thermal oxidation growth process is used to convert a portion of the fin 11 material into a second gate oxide layer 13 , the second gate oxide layer 13 is located between the remaining fin 11 and the first oxide layer 12 , and the second oxide layer 13 and the first oxide layer 12 constitute a gate oxide layer 14 .

[0040] In the formation method, a first oxide layer 12 and a second oxide layer 13 are formed respectively to constitute a gate oxide layer 14 through two process steps. Compared with the first method, the thickness of the first oxide layer 12 formed by the plasma enhanced atomic layer deposition process is smaller, and the consumption of the fin 11 when the first oxide layer 12 is formed by the plasma enhanced atomic layer deposition process is correspondingly less.

[0041] However, in the formation method, when a thermal oxidation growth process is used to form the second oxide layer 13, the thermal oxidation growth process is to introduce oxygen-containing gas in a high temperature environment to oxidize the fins 11, which will also consume more fins 11 and cause a size loss of the fins 11, thereby causing the size of the fins 11 to be difficult to meet the process requirements.

[0042] In order to solve the technical problem, an embodiment of the present invention provides a method for forming a semiconductor structure, including: providing a base, the base including a substrate and a fin protruding from the substrate; forming a sacrificial layer on the top surface and side wall of the fin, and the surface of the substrate; and oxidizing the sacrificial layer to convert the sacrificial layer into an oxide layer.

[0043] In the method for forming a semiconductor structure provided by an embodiment of the present invention, before forming an oxide layer, a sacrificial layer is also formed on the top surface and side wall of the fin and the surface of the substrate. Therefore, in the step of forming the oxide layer, the sacrificial layer is oxidized to consume the material of the sacrificial layer to form the oxide layer, which is beneficial to prevent consumption of the fin and reduce the loss of the fin, and further beneficial to accurately control the size of the fin so that the size of the fin meets the process requirements.

[0044] In order to make the above-mentioned purposes, features and advantages of the embodiments of the present invention more obvious and understandable, specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.

[0045] Figures 5 to 9 It is a schematic structural diagram corresponding to each step in an embodiment of a method for forming a semiconductor structure of the present invention.

[0046] refer to Figure 5 , providing a substrate, the substrate comprising a substrate 100 and a fin 110 protruding from the substrate 100 .

[0047] The substrate 100 provides a process platform for the process.

[0048] In this embodiment, the substrate 100 is a silicon substrate. In other embodiments, the material of the substrate may also be other materials such as germanium, silicon germanium, silicon carbide, gallium arsenide or indium gallium, and the substrate may also be other types of substrates such as a silicon on insulator substrate or a germanium on insulator substrate.

[0049] The fin 110 is used to provide a conductive channel when the fin field effect transistor (FinFET) is working.

[0050] In this embodiment, the material of the fin 110 is the same as that of the substrate 100, and the material of the fin 110 is silicon. In other embodiments, the material of the fin may also be a semiconductor material suitable for forming a fin, such as germanium, silicon germanium, silicon carbide, gallium arsenide, or indium gallium, and the material of the fin may also be different from that of the substrate.

[0051] Combined with reference Figure 6 In this embodiment, after providing the substrate, the method for forming the semiconductor structure further includes: forming a buffer layer 120 on the top surface and sidewalls of the fin 110 and the surface of the substrate 100 .

[0052] The buffer layer 120 is used to improve the interface quality of the surface of the fin 110, so as to facilitate the subsequent formation of the sacrificial layer on the surface of the fin 110 and improve the formation quality of the sacrificial layer. Moreover, after the sacrificial layer is subsequently formed, the step of oxidizing the sacrificial layer to convert the sacrificial layer into an oxide layer is also included. The buffer layer 120 is also used to form a gate oxide layer with the oxide layer.

[0053] Specifically, the fin 110 is usually formed by etching, and the surface of the fin 110 is relatively rough. By forming the buffer layer 120, it is helpful to reduce the defects on the surface of the fin 110 and improve the roughness of the surface of the fin 110, so as to provide a good interface state for the subsequent formation of a sacrificial layer, thereby preventing the subsequent sacrificial layer from being directly formed on the surface of the fin 110 and causing defects such as dislocations and singularities.

[0054] In this embodiment, the material of the buffer layer 120 includes silicon oxide. Silicon oxide is a gate oxide layer material commonly used in semiconductor processes, which is conducive to reducing the process cost of forming the buffer layer 120 and improving process compatibility. Moreover, the material of the natural oxide layer on the surface of the fin 110 is also silicon oxide. By selecting silicon oxide as the material of the buffer layer 120, it is conducive to making the buffer layer 120 easier to form on the surface of the fin 110 and improving process compatibility. In addition, the silicon oxide material has high adhesion with other materials, which is conducive to the subsequent formation of a sacrificial layer on the buffer layer 120 and improving the interface quality between the sacrificial layer and the buffer layer 120.

[0055] In this embodiment, an atomic layer deposition (ALD) process is used to form a buffer layer 120 on the top surface and sidewall of the fin 110 and the surface of the substrate 100. The atomic layer deposition process is a self-limiting reaction process based on the atomic layer deposition process. The deposited film can reach a thickness of a single layer of atoms. Because the atomic layer deposition process can accurately deposit one atomic layer in each cycle, the use of the atomic layer deposition process is conducive to accurately controlling the thickness of the buffer layer 120 and making the thickness of the buffer layer 120 small to meet the process requirements. In addition, the film prepared by the ALD process has the characteristics of good bonding strength, consistent film thickness, good composition uniformity, good conformality, etc., which is conducive to improving the thickness uniformity and film quality of the buffer layer 120.

[0056] In this embodiment, a plasma enhanced atomic layer deposition (PEALD) process is used to form the buffer layer 120. The process temperature of the plasma enhanced atomic layer deposition process is relatively low, which can reduce the impact on the performance of the semiconductor structure and reduce the thermal budget. Moreover, the process controllability of the plasma enhanced atomic layer deposition process is higher. In addition, by selecting the plasma enhanced atomic layer deposition process, it is beneficial to further reduce the consumption of the fin 110.

[0057] The output power used in the plasma enhanced atomic layer deposition process should not be too large. The output power is used to control the energy of the plasma. If the output power is too large, the energy of the plasma reaching the surface of the fin 110 is large. On the one hand, this easily leads to excessive consumption of the fin 110. On the other hand, the plasma hitting the fin 110 is directional. If the output power is too large, the anisotropy of the plasma is stronger. Compared with the plasma in contact with the top surface of the fin 110, there is less plasma in contact with the side wall of the fin 110, which easily leads to a lower thickness uniformity of the buffer layer 120 formed on the top of the fin 110 and the side wall of the fin 110. For this reason, in this embodiment, the output power used in the plasma enhanced atomic layer deposition process is 0 to 200W, for example: 20W, 50W, 75W, 100W, 150W, etc.

[0058] The thickness of the buffer layer 120 should not be too large, otherwise a larger output power and a larger flow rate of the oxygen-containing gas are required when forming the buffer layer 120, which may easily lead to a larger consumption of the fin 110 when forming the buffer layer 120. For this reason, in the step of forming the buffer layer 120 in this embodiment, the thickness of the buffer layer 120 is For example: wait.

[0059] Combined with reference Figure 7 In this embodiment, after forming the buffer layer 120 , the method for forming the semiconductor structure further includes: performing plasma treatment 130 on the buffer layer 120 in an oxygen-containing gas atmosphere, which is suitable for improving the density of the buffer layer 120 .

[0060] By performing plasma treatment 130 on the buffer layer 120 in an oxygen-containing gas atmosphere, the plasma treatment 130 can generate oxygen ions, break the bonds of the by-products in the buffer layer 120, and remove some impurity ions in the buffer layer 120, so that the film quality of the buffer layer 120 is close to that of the film formed by the thermal oxidation growth process, which is beneficial to improving the density and electrical properties of the buffer layer 120.

[0061] In this embodiment, oxygen is used for the plasma treatment 130, and the gas flow rate of the oxygen is 0 sccm to 500 sccm, for example, 100 sccm, 160 sccm, 300 sccm, etc. In this embodiment, the gas flow rate of oxygen used for the plasma treatment 130 is relatively small, which is beneficial to ensure that the density of the buffer layer 120 is improved while preventing the fin 110 from being consumed.

[0062] In the step of plasma processing 130 on the buffer layer 120, the output power used by the plasma processing 130 should not be too large, otherwise it is easy to consume the fin 110. Therefore, in this embodiment, the output power used by the plasma processing 130 is 0-100W, for example: 25W, 40W, 60W, etc.

[0063] In this embodiment, after the buffer layer 120 is formed, plasma treatment 130 is performed on the buffer layer 120 in an oxygen-containing gas atmosphere, which is suitable for improving the density of the buffer layer 120 as an example.

[0064] In other embodiments, after forming the buffer layer and before forming the sacrificial layer, the method for forming the semiconductor structure may further include: performing microwave treatment on the buffer layer, which is suitable for improving the density of the buffer layer.

[0065] The microwave treatment can generate high-energy microwaves to break the connecting bonds of byproducts in the buffer layer and remove impurities in the buffer layer, thereby improving the density of the buffer layer.

[0066] refer to Figure 8 A sacrificial layer 140 is formed on the top surface and sidewall of the fin 110 and the surface of the substrate 100 .

[0067] The subsequent steps also include: performing oxidation treatment on the sacrificial layer 140 to convert the sacrificial layer 140 into an oxide layer.

[0068] In this embodiment, before forming the oxide layer, a sacrificial layer 140 is formed on the top surface and side wall of the fin 110 and the surface of the substrate 100, so that in the subsequent step of forming the oxide layer, the sacrificial layer 140 is oxidized to consume the material of the sacrificial layer 140 to form the oxide layer, which is beneficial to prevent the consumption of the fin 110 and reduce the loss of the fin 110, and further helps to accurately control the size of the fin 110 so that the size of the fin 110 meets the process requirements.

[0069] In this embodiment, in the step of forming the sacrificial layer 140 , the sacrificial layer 140 is formed on the buffer layer 120 , and then the sacrificial layer 140 is oxidized to form an oxide layer, which is used to form a gate oxide layer together with the buffer layer 120 .

[0070] In this embodiment, the material of the sacrificial layer 140 is the same as that of the fin 110 . The material of the sacrificial layer 140 is silicon, so that the material of the subsequently formed oxide layer is silicon oxide, which is beneficial to improving process compatibility.

[0071] The thickness of the sacrificial layer 140 should not be too small or too large. If the thickness of the sacrificial layer 140 is too small, in the subsequent step of oxidizing the sacrificial layer 140 to form an oxide layer, the sacrificial layer 140 is easily consumed prematurely and completely converted into an oxide layer, which may easily cause the oxidation treatment to oxidize the fin 110, thereby easily consuming the fin 110; if the thickness of the sacrificial layer 140 is too large, the thickness of the subsequently formed oxide layer is also too large, which may easily cause the thickness of the formed gate oxide layer to be too large, making it difficult to meet the process requirements. For this reason, in the step of forming the sacrificial layer 140, the thickness of the sacrificial layer 140 is to For example: wait.

[0072] In this embodiment, a furnace tube process is used to form the sacrificial layer 140. The furnace tube process is simple to operate and has high process compatibility.

[0073] In this embodiment, the furnace tube process is a low-temperature furnace tube process. By selecting the low-temperature furnace tube process, it is beneficial to improve the thickness uniformity and film density of the sacrificial layer 140, especially to improve the thickness uniformity of the sacrificial layer 140 located at the top of the fin 110 and the side wall of the fin 110, and the low-temperature furnace tube process is beneficial to reduce the impact on the structure of the fin 110. Specifically, the temperature of the furnace tube process is 300-400°C, for example: 320°C, 345°C, 390°C, etc.

[0074] refer to Fig. 9 , the sacrificial layer 140 is oxidized to transform the sacrificial layer 140 into an oxide layer 150 .

[0075] By oxidizing the sacrificial layer 140, the sacrificial layer 140 can be consumed and converted into an oxide layer 150, which is beneficial to prevent the fin 110 from being consumed, and further beneficial to accurately control the size of the fin 110, so that the size of the fin 110 meets the requirements for the electrical performance of the semiconductor structure.

[0076] In this embodiment, after the oxide layer 150 is formed, the oxide layer 150 and the buffer layer 120 are used to form a gate oxide layer 160 .

[0077] Combined with reference Fig.10 , shows a schematic diagram of the local structure of the fin and the gate oxide layer formed by the formation method of an embodiment of the present invention and the consumption of the fin 110, Fig.10 The partial structural schematic diagram of the gate oxide layer formed by the formation method of the prior art and the consumption of the fin are also shown. Take the fin material as silicon and the silicon oxide material as silicon oxide as an example, wherein Bare Si represents the fin; ALDOX in the prior art represents the gate oxide layer formed by the atomic layer deposition process in the prior art; in the embodiment of the present invention, Low Power ALDOX represents the buffer layer formed by the plasma enhanced atomic layer deposition process with a lower output power in the embodiment of the present invention, Thermal OX represents the oxide layer formed by oxidizing the sacrificial layer by the thermal oxidation process in the embodiment of the present invention, and the oxide layer and the buffer layer constitute the gate oxide layer formed in the embodiment of the present invention.

[0078] from Fig.10 It can be seen from the figure that the gate oxide layer is formed by the prior art method, and the loss of silicon (Si Loss) is That is to say, the loss of the fin caused by forming the gate oxide layer using the prior art method is When the gate oxide layer 160 is formed by the method of the embodiment of the present invention, the loss of silicon (Si Loss) is That is, the loss of the fin 110 caused by forming the gate oxide layer 160 by the method of the embodiment of the present invention is The method according to the embodiment of the present invention can significantly reduce the consumption of the fin 110 .

[0079] In this embodiment, the oxide layer 150 is made of the same material as the buffer layer 120 , that is, silicon oxide, so that the gate oxide layer 160 is made of the same material, which is beneficial to improving process compatibility and film quality of the gate oxide layer 160 .

[0080] In this embodiment, a thermal oxidation process is used to oxidize the sacrificial layer 140. The thermal oxidation process is used to form the oxide layer 150, which is beneficial to improving the film quality (eg, density) of the oxide layer 150 and reducing defects and impurities in the oxide layer 150.

[0081] Specifically, the thermal oxidation process may be an in-situ steam generation process (ISSG), a dry oxygen oxidation process, or the like.

[0082] With reference to Table 1, some electrical parameters of the gate oxide layer formed by the prior art method and some electrical parameters of the gate oxide layer 160 formed by the formation method of the embodiment of the present invention are shown. As can be seen from Table 1, compared with the gate oxide layer formed by the prior art, the gate oxide layer 160 formed by the embodiment of the present invention has a smaller equivalent electrical thickness (EOT), a smaller interface trap density (Interfacial trap density, DIT), and a higher leakage voltage (Leakage Index), thereby optimizing the electrical performance of the gate oxide layer 160.

[0083]

[0084] Table 1

[0085] The subsequent process steps will not be described in detail in this embodiment.

[0086] Accordingly, the present invention also provides a semiconductor structure. Figure 8 , showing a schematic structural diagram of an embodiment of a semiconductor structure of the present invention.

[0087] The semiconductor structure includes: a base, the base includes a substrate 100 and a fin 110 protruding from the substrate 100; a sacrificial layer 140, located on the top and sidewalls of the fin 110 and the surface of the substrate 100, and the sacrificial layer 140 is suitable for being converted into an oxide layer through oxidation treatment.

[0088] The oxide layer is used to form a gate oxide layer.

[0089] The semiconductor structure of this embodiment also includes a sacrificial layer 140 located on the top and side walls of the fin 110 and the surface of the substrate 100. The sacrificial layer 140 is suitable for being converted into an oxide layer through oxidation treatment, so that the material of the sacrificial layer 140 can be consumed and converted into an oxide layer by subsequently performing oxidation treatment on the sacrificial layer 140, which is beneficial to prevent consumption of the fin 110 and reduce the loss of the fin 110, and further beneficial to accurately control the size of the fin 110 so that the size of the fin 110 meets the process requirements.

[0090] The substrate 100 provides a process platform for the process.

[0091] In this embodiment, the substrate 100 is a silicon substrate. In other embodiments, the material of the substrate may also be other materials such as germanium, silicon germanium, silicon carbide, gallium arsenide or indium gallium, and the substrate may also be other types of substrates such as a silicon on insulator substrate or a germanium on insulator substrate.

[0092] The fin 110 is used to provide a conductive channel when the fin field effect transistor (FinFET) is working.

[0093] In this embodiment, the substrate 100 is a silicon substrate. In other embodiments, the material of the substrate may also be other materials such as germanium, silicon germanium, silicon carbide, gallium arsenide or indium gallium, and the substrate may also be other types of substrates such as a silicon on insulator substrate or a germanium on insulator substrate.

[0094] The sacrificial layer 140 is suitable for being transformed into an oxide layer through an oxidation process.

[0095] In this embodiment, the material of the sacrificial layer 140 is the same as that of the fin 110 . The material of the sacrificial layer 140 is silicon, so that the material of the subsequently formed oxide layer is silicon oxide, which is beneficial to improving process compatibility.

[0096] The thickness of the sacrificial layer 140 should not be too small or too large. If the thickness of the sacrificial layer 140 is too small, when the sacrificial layer 140 is subsequently oxidized to form an oxide layer, the sacrificial layer 140 is easily consumed prematurely and completely converted into an oxide layer, which can easily cause the oxidation treatment to also oxidize the fin 110, thereby easily causing the consumption of the fin 110; if the thickness of the sacrificial layer 140 is too large, the thickness of the oxide layer formed subsequently is also too large, which can easily cause the thickness of the gate oxide layer formed to be too large, making it difficult to meet the process requirements. For this reason, in this embodiment, the thickness of the sacrificial layer 140 is to For example: wait..

[0097] In this embodiment, the semiconductor structure further includes a buffer layer 120 located between the substrate and the sacrificial layer 140 .

[0098] The buffer layer 120 is used to improve the interface quality of the surface of the fin 110, so as to facilitate the formation of the sacrificial layer 140 on the surface of the fin 110 and improve the formation quality of the sacrificial layer 140. Moreover, the sacrificial layer 140 is subsequently oxidized to form an oxide layer, and the buffer layer 120 is also used to form a gate oxide layer with the oxide layer.

[0099] Specifically, the fin 110 is usually formed by etching, and the surface of the fin 110 is relatively rough. The buffer layer 120 is helpful to reduce the defects on the surface of the fin 110 and improve the roughness of the surface of the fin 110, thereby providing a good interface state for forming the sacrificial layer 140, thereby preventing the sacrificial layer 140 from being directly formed on the surface of the fin 110 and causing some defects such as singularities.

[0100] In this embodiment, the material of the buffer layer 120 includes silicon oxide. Silicon oxide is a gate oxide layer material commonly used in semiconductor processes, which is conducive to reducing the process cost of forming the buffer layer 120 and improving process compatibility. Moreover, the material of the natural oxide layer on the surface of the fin 110 is also silicon oxide. By selecting silicon oxide as the material of the buffer layer 120, it is conducive to making the buffer layer 120 easier to form on the surface of the fin 110 and improving process compatibility. In addition, the silicon oxide material has high adhesion with other materials, which is conducive to the formation of the sacrificial layer 140 on the buffer layer 120 and improving the interface quality between the sacrificial layer 140 and the buffer layer 120.

[0101] The thickness of the buffer layer 120 should not be too large, otherwise a larger output power and a larger flow rate of the oxygen-containing gas are required when forming the buffer layer 120, which may easily lead to a larger consumption of the fin 110 when forming the buffer layer 120. For example: wait.

[0102] The semiconductor structure can be formed by the formation method described in the above embodiment, or by other formation methods. For the specific description of the semiconductor structure described in this embodiment, reference can be made to the corresponding description in the above embodiment, and this embodiment will not be repeated here.

[0103] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.

Claims

1. A method for forming a semiconductor structure, characterized in that: include: Providing a substrate, the substrate comprising a substrate and a fin protruding from the substrate; A sacrificial layer is formed on the top surface and sidewall of the fin and the surface of the substrate, wherein the material of the sacrificial layer is the same as the material of the fin; the sacrificial layer is formed by a furnace tube process, wherein the temperature of the furnace tube process is 300-400° C.; The sacrificial layer is oxidized by a thermal oxidation process to convert the sacrificial layer into an oxide layer, wherein the surface of the sacrificial layer is exposed during the thermal oxidation process; The thermal oxidation process is an in-situ steam generation process; After providing the substrate and before forming the sacrificial layer, the method for forming the semiconductor structure further includes: forming a buffer layer on the top surface and side walls of the fin and the surface of the substrate; in the step of forming the sacrificial layer, the sacrificial layer is formed on the buffer layer; after forming the oxide layer, the oxide layer and the buffer layer are used to constitute a gate oxide layer.

2. The method for forming a semiconductor structure according to claim 1, wherein: An atomic layer deposition process is adopted to form a buffer layer on the top surface and sidewall of the fin and the surface of the substrate.

3. The method for forming a semiconductor structure according to claim 1, wherein: A plasma enhanced atomic layer deposition process is adopted to form a buffer layer on the top surface and sidewall of the fin and the surface of the substrate.

4. The method for forming a semiconductor structure according to claim 3, wherein: The output power used in the plasma enhanced atomic layer deposition process is 0-200W.

5. The method for forming a semiconductor structure according to claim 1, wherein: In the step of forming the buffer layer, the thickness of the buffer layer is 6. The method for forming a semiconductor structure according to claim 1, wherein: In the step of forming the buffer layer, the material of the buffer layer includes silicon oxide.

7. The method for forming a semiconductor structure according to claim 1, wherein: The oxide layer and the buffer layer are made of the same material.

8. The method for forming a semiconductor structure according to claim 1, wherein: After forming the buffer layer and before forming the sacrificial layer, the method for forming the semiconductor structure further includes: performing plasma treatment on the buffer layer in an oxygen-containing gas atmosphere, which is suitable for improving the density of the buffer layer.

9. The method for forming a semiconductor structure according to claim 1, wherein: After forming the buffer layer and before forming the sacrificial layer, the method for forming the semiconductor structure further includes: performing microwave treatment on the buffer layer, which is suitable for improving the density of the buffer layer.

10. The method for forming a semiconductor structure according to claim 8, wherein: The output power used in the plasma treatment is 0-100W.

11. A semiconductor structure, characterized in that: The semiconductor structure is formed by the method for forming a semiconductor structure according to any one of claims 1 to 10, comprising: A base, the base comprising a substrate and a fin protruding from the substrate; a sacrificial layer, located on the top and sidewalls of the fin and the surface of the substrate, the sacrificial layer being formed by a furnace tube process, the temperature of the furnace tube process being 300-400° C., the sacrificial layer being suitable for being converted into an oxide layer by oxidation treatment, the oxidation treatment being an in-situ steam generation process; The semiconductor structure further includes a buffer layer located between the substrate and the sacrificial layer. The oxide layer and the buffer layer are used to form a gate oxide layer.

12. The semiconductor structure according to claim 11, wherein: The material of the buffer layer includes silicon oxide.

13. The semiconductor structure according to claim 11, wherein: The thickness of the buffer layer is 14. The semiconductor structure according to claim 11, wherein: The material of the sacrificial layer is the same as that of the fin.

15. The semiconductor structure according to claim 11, wherein: The thickness of the sacrificial layer is