Production process and structure of crack-free and long-life composite desulfurization powder spray gun
Through the process of split assembly and high-strength cement bonding, combined with spring pressure device and tile pressing of resistant machine, the problems of horizontal cracks and longitudinal cracks and thermal shock during the use of desulfurization spray guns are solved, which extends the service life and simplifies the production process, realizing the An efficient desulfurization spray gun design.
Patent Information
- Application Number
- CN202110136182.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-02-01
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2041-02-01
AI Technical Summary
Existing desulfurization spray guns are prone to transverse cracks, longitudinal cracks, thermal shock damage and chemical corrosion during use, resulting in short service life, long production cycle, and complex production process, which is difficult to control.
The production process of crack-free long-life composite desulfurization powder spray gun is adopted. The gun head and gun body are assembled through split assembly, high-strength cement bonding and spring pressure devices are used, and machine-pressed bricks and prefabricated gun heads are used, combined with high aluminum Massive self-flow material and refractory machine press bricks to reduce internal stress release and thermal expansion differences.
It significantly extends the service life of the desulfurization spray gun, shortens the production cycle, reduces the difficulty and cost of production, improves the resistance to erosion and erosion resistance, and reduces the risks of high-altitude operations.
Smart Images

Figure CN112941268B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of desulfurization equipment and materials in molten iron pretreatment, and in particular to a production process and a powder spraying gun structure of a crack-free and long-life composite desulfurization powder spraying gun. Background Art
[0002] The sulfur content in steel directly affects the performance of steel. The off-furnace desulfurization technology is an important means of modern steelmaking. The desulfurization spray gun is an important part of the molten iron pre-desulfurization equipment. Its working principle is to use the desulfurization spray gun to spray desulfurizers such as passivation lime powder and passivation magnesium powder into the molten iron ladle with high-pressure inert gas argon or nitrogen as the carrier, so that the molten iron is stirred violently to achieve the purpose of molten iron pre-desulfurization.
[0003] During the hot metal desulfurization process, the desulfurization gun is repeatedly and intermittently used, so it has to withstand high temperature, erosion of hot metal and slag, chemical erosion and thermal shock damage; its damage is manifested as: large longitudinal and transverse cracks on the gun body surface, erosion and fracture of the slag line, and damage to the gun head; its specific damage mechanism is described as follows:
[0004] 1. Wear from high-pressure stirring and repeated hot and cold alternations cause transverse cracks, longitudinal cracks and spalling of the castable. During the desulfurization process, the high-pressure gas drives the stirring of the molten iron, causing the amplitude of the desulfurization gun body to fluctuate greatly, resulting in more transverse cracks in the desulfurization gun castable, and the cracks will continue to extend and expand in the places where cracks have appeared, and then the castable will spall under the scouring of the molten iron; with the use, the cracks become larger and larger, eventually leading to spalling and falling off, especially when the castable is intermittently used, it is easy to suffer from thermal shock damage and cracks, or cracks during baking, the intrusion of steel slag and the scouring of molten iron will increase the cracks and cause more serious spalling and falling off, and even the gun head will melt.
[0005] 2. Corrosion and damage due to chemical reaction between castable and flux. Castable is easy to react with Fe2O3 in slag to generate low melting point, which causes melting loss of castable during use. The closer to slag line, the greater the loss. In addition, after cracks are generated or low melting point is generated, castable is easy to be washed away by molten iron and damaged.
[0006] 3. Due to the expansion of the metal tube, the castable cracks and the cracks spread and damage, which is one of the most important destructive factors generated during use. During use, the gun body is quickly heated by the high-temperature metal, and the high-speed flow of carrier gas and desulfurizer in the gun core tube cools the gun body by convection cooling. Under the combined effect of heating and cooling, the temperature distribution of the gun body gradually changes from uniform distribution at room temperature to continuous decrease from outside to inside, and as the injection and immersion time increases, the temperature of the outside of the refractory casting layer of the gun body continues to rise sharply due to the heating of high-temperature molten iron, and the core of the gun body is convectively cooled by carrier gas and desulfurizer in the main tube, and the temperature rise rate is relatively slow, causing the temperature difference between the inside and outside of the gun body to continue to increase; after use, the surface temperature of the castable decreases, while the temperature of the internal metal tube does not decrease and even has an upward trend, which causes the expansion between the metal tube and the anchor and the castable to shift, and the thermal expansion between the castable and the metal tube is quite different, so it causes cracks in the castable, causing damage, and ultimately limiting the service life of the desulfurization gun.
[0007] In the actual production process of desulfurization spray guns, the overall length of the desulfurization spray gun is generally about 8-10 meters. Vertical pouring is usually used during pouring. Due to its length limitation, the pouring site of its refractory materials requires a factory building with sufficient height and sufficient space. In addition, during the transportation and hoisting process, it is required to have sufficient strength at room temperature. Since its pouring construction and curing and drying are often controlled by temperature and environmental changes, it is difficult to control. In addition, the pouring construction is limited by factors such as the amount of water added to the castable, the stirring time, and the vibration effect of the motor. The poured desulfurization spray gun also requires a long curing time, which seriously delays the production cycle of the desulfurization spray gun.
[0008] Based on the above shortcomings and problems in the production and use of the cast-type desulfurization spray gun, there is an urgent need for a new desulfurization spray gun and a manufacturing method to minimize the horizontal and vertical cracks in the gun body castable, while simplifying the production process, reducing the production cycle, and reducing the difficulty of manufacturing. Summary of the invention
[0009] The purpose of the present invention is to provide a production process and a powder spray gun structure for a crack-free and long-life composite desulfurization powder spray gun. The present invention changes the original production method of directly pouring steel structural parts and castables, and adopts a split assembly form. For the first time, a gun head prefabricated part and a gun body machine-pressed brick form are used to assemble the desulfurization spray gun. Bricks and prefabricated parts are bonded with high-strength glue, and a spring pressure device is used to press each refractory part, and high-aluminum self-flowing material is used for pouring between the machine-pressed bricks and the steel structural parts.
[0010] The present invention has newly designed a composite desulfurization powder spray gun scheme and manufacturing process, the purpose of which is to improve the transverse cracks that occur in the desulfurization spray gun during use. According to the different use conditions at different positions, a composite scheme is adopted to specifically improve its use effect, reduce costs, and shorten the production cycle.
[0011] In order to achieve the above object, the present invention adopts the following technical solutions:
[0012] A production process of a crack-free, long-life composite desulfurization powder spray gun comprises the following steps:
[0013] 1) Assemble and weld the steel structure, and weld the spring positioning plate to the outer square tube of the steel structure;
[0014] 2) Apply polyurethane on the surface of the outer square tube of the steel structure with a thickness of not less than 2mm;
[0015] 3) The spring and spring baffle are sleeved on the steel structure from the bottom of the steel structure in sequence, and then the refractory machine-pressed brick is sleeved on the steel structure and connected with the spring baffle. High-strength glue is applied between the refractory machine-pressed bricks to seal them. Finally, the prefabricated gun head is installed at the end of the steel structure, and the refractory machine-pressed bricks and the prefabricated gun head are bonded with high-strength glue;
[0016] 4) Inject the self-flowing castable material through the grouting port on the refractory machine-pressed brick.
[0017] The refractory machine-pressed bricks at the slag line position in the refractory machine-pressed bricks are prepared from the following raw materials in parts by weight: 15-25 parts of alumina particle size 5-3mm, 15-25 parts of alumina particle size 3-1mm, 5-10 parts of brown corundum particle size 3-1mm, 10-20 parts of brown corundum particle size 1-0mm, 5-10 parts of silicon carbide particle size 1-0mm, 2.8-3.0 parts of thermoplastic resin, 8-13 parts of -195 graphite, 0.5-2 parts of metal aluminum powder 200 mesh, 3-8 parts of silicon carbide 200 mesh, 8-15 parts of brown corundum 200 mesh, and 0.2-0.4 parts of urotropine.
[0018] The refractory machine-pressed bricks in the non-slag line part of the refractory machine-pressed bricks are prepared from the following raw materials in parts by weight: 10-20 parts of alumina particle size 5-3mm, 20-30 parts of alumina particle size 3-1mm, 20-30 parts of alumina particle size 1-0mm, 2.8-3.0 parts of thermoplastic resin, 8-15 parts of -194 graphite, 1-3 parts of metal aluminum powder 200 mesh, 8-15 parts of silicon carbide 200 mesh, 8-15 parts of brown corundum 200 mesh, and 0.2-0.4 parts of urotropine.
[0019] The prefabricated casting material of the prefabricated gun head is prepared from the following raw materials in parts by weight: 20-30 parts of fused mullite with a particle size of 5-10mm, 10-20 parts of fused mullite with a particle size of 3-6mm, 10-15 parts of coke stone with a particle size of 1-3mm, 10-20 parts of coke stone with a particle size of 0-1mm, 3-6 parts of activated alumina micropowder 5μm, 3-8 parts of pure calcium aluminate cement, 5-8 parts of silicon carbide 200 mesh, 4-8 parts of kyanite 40 mesh, 3-5 parts of white corundum 240 mesh, 0.5-0.8 parts of high-efficiency water reducer, and 0.08-0.12 parts of zirconia fiber.
[0020] A powder spray gun structure produced by adopting the production process of a crack-free, long-life composite desulfurization powder spray gun, comprising a steel structure, a spring pressure device, a prefabricated gun head, and a refractory machine-pressed brick. The refractory machine-pressed brick is sleeved on the outside of the steel structure, the prefabricated gun head is installed at the bottom of the steel structure, the spring pressure device is arranged at the upper end of the refractory machine-pressed brick, so that the refractory machine-pressed brick and the prefabricated gun head are pressed and sealed, and a self-flowing castable material layer is filled between the refractory machine-pressed brick and the steel structure.
[0021] The steel structure comprises an inner circular tube and an outer square tube. The inner circular tube is arranged inside the outer square tube, and a polyurethane layer is coated on the outer wall surface of the outer square tube.
[0022] The spring pressure device includes a spring positioning plate, a spring, and a spring baffle. The spring positioning plate is fixedly connected to the steel structure. The spring is sleeved outside the steel structure and under the spring positioning plate. The spring baffle is arranged at the bottom of the spring and is slidably sleeved with the steel structure.
[0023] The refractory machine pressed bricks are sealed by means of annular grooves and protrusions, and the refractory machine pressed bricks and the prefabricated gun head are also sealed by means of annular grooves and protrusions.
[0024] Several of the refractory machine-pressed bricks are provided with grouting ports.
[0025] The prefabricated gun head comprises a steel nozzle and a prefabricated casting material, wherein the prefabricated casting material is wrapped around the outside of the steel nozzle, and the steel nozzle is connected to a steel structural member through a thread.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] 1) The refractory material of the gun body is assembled in the form of machine-pressed bricks for the first time. Compared with the traditional cast desulfurization spray gun, it has stronger resistance to erosion and scouring; due to the assembly form, compared with the traditional cast desulfurization spray gun, the thermal expansion coefficient of the steel structure and the traditional cast refractory is quite different. Although a certain amount of kyanite, sillimanite and other raw materials are usually added to the castable to increase its thermal expansion coefficient, the actual use process is always unsatisfactory, and more or less transverse cracks caused by the release of internal stress will appear, thus affecting its service life. The present invention effectively avoids the cracks and expansion caused by the release of internal stress through split assembly, and alleviates it through a spring pressure device, so as to effectively solve the problem of crack generation and expansion, and releases the energy of stress damage caused by the thermal shock process through the spring pressure device. Taking the 240-ton molten iron tank of the fourth branch of a large steel plant in Northeast China as an example, the average life of the original casting desulfurization spray gun is 26 times, and the proportion of desulfurization spray guns that were offline due to excessive transverse and longitudinal cracks is 38.46%; while the average life of the desulfurization spray guns made by the present invention is 41 times, and there are almost no desulfurization spray guns that were offline due to transverse and longitudinal cracks.
[0028] 2) High efficiency in production. Traditional desulfurization spray guns all adopt a vertical pouring method. Due to the long length of the castable, it is difficult to ensure the pouring quality by only using devices such as vibration motors and vibration rods to assist pouring, and the production cycle is long. Most of the present invention uses machine-pressed bricks, the brick shape is relatively fixed, the production is efficient and convenient, and only assembly is required, which greatly shortens the production cycle. Usually, the production cycle of a pouring desulfurization spray gun is about 20 days, while the present invention only takes 7 days.
[0029] 3) Effectively release the height limit of the factory building and avoid high-altitude operations. Traditional desulfurization spray guns all adopt the vertical casting method, and the overall length of the desulfurization spray gun is generally about 8-10 meters, which requires a high-height factory building and high-altitude operations; the present invention only needs to be produced and assembled on the ground, which is safer to operate.
[0030] 4) The nozzle structure is fixed with several tie plates, which can make each tube of the structure bear 360° force, making the structure more stable during use.
[0031] 5) Steel structures can be reused many times. The desulfurization spray gun that has been offline is usually dismantled by a pneumatic pick; however, the present invention can be dismantled by simply opening the spring clamping device, which greatly reduces the labor intensity. The dismantled steel structures can be reused many times, which achieves the purpose of saving costs and protecting the environment. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 The utility model is a schematic diagram of the overall structure of a crack-free and long-life composite desulfurization powder spray gun of the present invention.
[0033] Figure 2 It is a structural diagram of steel structural parts and spring pressure device.
[0034] Figure 3 It is a schematic diagram of the assembly structure of refractory machine-pressed bricks and prefabricated gun heads.
[0035] Figure 4 This is an enlarged view of the structure of the prefabricated gun head.
[0036] Figure 5 It is a schematic diagram of the structure of a steel nozzle.
[0037] Figure 6 This is a top view of the refractory machine-pressed bricks.
[0038] Figure 7 It is a top view of a refractory machine-pressed brick with a grouting port.
[0039] Figure 8 It is a production process flow chart of the present invention.
[0040] In the figure: 1. Outer square tube; 2. Inner round tube; 3. Spring positioning plate; 4. Spring baffle; 5. Spring; 6. Refractory machine-pressed brick; 7. High-strength cement; 8. Self-flowing castable material layer; 9. Prefabricated gun head; 9-1 Steel nozzle; 9-2 Tie plate; 9-3 Prefabricated casting material; 10. Refractory machine-pressed brick with grouting port; 10-1 Grouting port. DETAILED DESCRIPTION
[0041] The specific embodiments of the present invention are further described below:
[0042] like Figure 1-Figure 8 As shown, a production process of a crack-free and long-life composite desulfurization powder spray gun comprises the following steps:
[0043] 1) Assemble and weld the steel structure, and weld and fix the spring positioning plate 3 to the outer square tube of the steel structure.
[0044] The desulfurization spray gun steel structure adopts a double-layer steel structure design, with an inner round tube 2 and an outer square tube 1. The bottom of the two tubes are welded and fixed, while the top is not welded to adapt to the expansion and contraction caused by temperature changes. It is necessary to ensure that the center lines of the outer square tube 1 and the inner round tube 2 coincide.
[0045] 2) Apply polyurethane on the surface of the outer square tube 1 of the steel structure with a thickness of not less than 2mm; the purpose is to prevent direct contact between the high-aluminum self-flowing material and the steel structure. The polyurethane melts and disappears at high temperature, leaving a gap between the steel structure and the material, leaving space for high-temperature expansion of the steel structure.
[0046] 3) The spring 5 and the spring baffle 4 are sequentially sleeved on the steel structure from the bottom of the steel structure, so that the spring 5 is against the spring positioning plate 3, and then the refractory machine pressed brick 6 is sleeved on the steel structure and against the spring baffle 4, and high-strength glue 7 is applied between the refractory machine pressed bricks 6 to seal, and finally the prefabricated gun head 9 is installed at the end of the steel structure, and the refractory machine pressed brick 6 and the prefabricated gun head 9 are bonded with high-strength glue 7.
[0047] The welding of the spring positioning plate 3 in the above step 1) can be temporarily fixed by spot welding. When adjusting the spring pressure device, the spring positioning plate 3 can be disassembled and repositioned and fixed to adjust the spring pressure device. After locking the whole, ensure that the gap between each part is less than 2mm.
[0048] 4) Self-flowing castable is injected through the grouting port 10-1 on the refractory machine-pressed brick 10 to fill the internal gap. The self-flowing castable is a high-alumina self-flowing castable.
[0049] The refractory machine-pressed bricks at the slag line position of the refractory machine-pressed bricks 6 are prepared from the following raw materials in parts by weight: 15-25 parts of 88 alumina with a particle size of 5-3mm, 15-25 parts of 88 alumina with a particle size of 3-1mm, 5-10 parts of brown corundum with a particle size of 3-1mm, 10-20 parts of brown corundum with a particle size of 1-0mm, 5-10 parts of silicon carbide with a particle size of 1-0mm, 2.8-3.0 parts of thermoplastic resin, 8-13 parts of -195 graphite, 0.5-2 parts of metal aluminum powder 200 mesh, 3-8 parts of silicon carbide 200 mesh, 8-15 parts of brown corundum 200 mesh, and 0.2-0.4 parts of urotropine.
[0050] The refractory machine-pressed bricks in the non-slag line part of the refractory machine-pressed bricks 6 are prepared from the following raw materials in parts by weight: 10-20 parts of 88 alumina with a particle size of 5-3mm, 20-30 parts of 88 alumina with a particle size of 3-1mm, 20-30 parts of 88 alumina with a particle size of 1-0mm, 2.8-3.0 parts of thermoplastic resin, 8-15 parts of -194 graphite, 1-3 parts of metal aluminum powder 200 mesh, 8-15 parts of silicon carbide 200 mesh, 8-15 parts of brown corundum 200 mesh, and 0.2-0.4 parts of urotropine.
[0051] The prefabricated casting material 9-3 of the prefabricated gun head is prepared from the following raw materials in parts by weight: 20-30 parts of fused mullite with a particle size of 5-10mm, 10-20 parts of fused mullite with a particle size of 3-6mm, 10-15 parts of coke stone with a particle size of 1-3mm, 10-20 parts of coke stone with a particle size of 0-1mm, 3-6 parts of activated alumina micropowder 5μm, 3-8 parts of pure calcium aluminate cement, 5-8 parts of 95 silicon carbide 200 mesh, 4-8 parts of kyanite 40 mesh, 3-5 parts of white corundum 240 mesh, 0.5-0.8 parts of high-efficiency water reducer, and 0.08-0.12 parts of zirconia fiber.
[0052] See Figure 1-Figure 7 A powder spray gun structure produced by the production process of a crack-free, long-life composite desulfurization powder spray gun includes a steel structure, a spring pressure device, a prefabricated gun head 9, and a refractory machine-pressed brick 6. The refractory machine-pressed brick 6 is sleeved on the outside of the steel structure, and the prefabricated gun head 9 is installed at the bottom of the steel structure. The spring pressure device is arranged at the upper end of the refractory machine-pressed brick 6, so that the refractory machine-pressed brick 6 and the prefabricated gun head 9 are pressed and sealed, and a self-flowing castable material layer 8 is filled between the refractory machine-pressed brick 6 and the steel structure.
[0053] The steel structure comprises an inner circular tube 2 and an outer square tube 1 . The inner circular tube 2 is arranged in the outer square tube 1 , and a polyurethane layer is coated on the outer wall surface of the outer square tube 1 .
[0054] The spring pressure device includes a spring positioning plate 3, a spring 5, and a spring baffle 4. The spring positioning plate 3 is fixedly connected to the steel structure. The spring 5 is sleeved outside the steel structure and under the spring positioning plate 3. The spring baffle 4 is arranged at the bottom of the spring 5 and is slidably sleeved with the steel structure.
[0055] The refractory machine pressed bricks 6 are sealed by means of annular grooves and protrusions, and the refractory machine pressed bricks 6 and the prefabricated gun head 9 are also sealed by means of annular grooves and protrusions.
[0056] Several of the refractory machine-pressed bricks are provided with grouting ports 10-1. Figure 1 Among them, the refractory machine-pressed brick at the bottom is a refractory machine-pressed brick 10 provided with a grouting port.
[0057] The prefabricated gun head 9 includes a steel nozzle 9-1 and a prefabricated castable 9-3. The prefabricated castable 9-3 is wrapped around the outside of the steel nozzle 9-1. The steel nozzle 9-1 is connected to a steel structure through threads.
[0058] According to the position of the desulfurization spray gun in the molten iron, the present invention adopts refractory materials of different materials and different manufacturing processes: the refractory material at the nozzle of the desulfurization spray gun is in the form of a prefabricated part, the castable is mainly made of mullite-pyrotechnic stone, combined with low cement, compounded with various micropowders and fibers, with high strength, erosion resistance, and slight expansion at high temperature; the refractory material of the gun body is in the form of machine-pressed bricks, among which the machine-pressed brick refractory material at the slag line is selected from Al-SiC-C with excellent slag resistance, and the machine-pressed brick refractory material at other parts is Al-C, and the bricks are bonded with high-strength cement.
[0059] The water content of the desulfurization spray gun prefabricated gun head castable formula is 3.5-5.5wt%; its 110℃*24h dry compressive strength can reach more than 20MPa; there is no peeling phenomenon after 20 times of thermal vibration at 1100℃, and its residual compressive strength can reach more than 5MPa. This formula composition can greatly improve its high temperature strength, reduce the thermal conductivity of the refractory material, improve the anti-oxidation performance of the refractory material, and improve its anti-scouring performance in molten steel.
[0060] The nozzle hole type can be Y-type, T-type, three-hole, four-hole and other types of nozzle holes. The present invention adopts welding several reinforcing plates 9-2 for each round tube of the nozzle structure to fix it. This method can make each tube bear force in all directions, making the structure more stable during use, reducing the shaking of the desulfurization gun during use, thereby reducing the occurrence of desulfurization transverse cracking and gun bending. The embodiment takes three-hole powder spraying as an example. The angle between each steel pipe is 120°, and each pipe is fixed with several reinforcing plates 9-2 around it, so that each pipe of the structure can be subjected to force at 360°; the three-hole distribution can make the desulfurizer spray out evenly in three directions, and then make the desulfurization gun body itself bear force evenly in all directions, thereby reducing the shaking of the desulfurization gun during use and the occurrence of desulfurization transverse cracking and gun bending.
[0061] The volume density of the refractory machine-pressed bricks at the slag line can reach 3.0g / cm 3 The room temperature compressive strength can reach more than 50Mpa, and the high temperature flexural strength is greater than 5Mpa. This formula has good slag erosion resistance and thermal vibration resistance.
[0062] The volume density of refractory machine-pressed bricks in other parts can reach 2.8g / cm 3 The room temperature compressive strength can reach more than 45Mpa, and the high temperature flexural strength is greater than 5Mpa. This formula has good high temperature strength and thermal vibration performance.
[0063] Embodiment 1:
[0064] Taking a 240-ton iron molten ladle of the fourth branch of a large steel plant in Northeast China as an example, the present invention specifically describes a crack-free, long-life composite desulfurization powder spray gun and a production process.
[0065] The desulfurization process of the desulfurization lance of the fourth branch of the steel plant has been put into production for more than 20 years. Its service life has been unstable. Especially in recent years, due to the high content of S and N in the molten iron, the desulfurization time has been significantly increased, and the proportion of desulfurizer added has also increased significantly. Therefore, the proportion of desulfurization lances that have been offline due to abnormal reasons such as horizontal and vertical cracks, erosion and fracture of the slag line, and damage to the lance head has gradually increased.
[0066] Based on long-term observation and a large number of experiments, the present invention improves the traditional pouring desulfurization spray gun as follows:
[0067] 1. Change the production method of direct pouring of steel structural parts and castables, adopt a split assembly form, the gun head adopts the form of prefabricated parts, and the gun body is assembled in the form of machine-pressed bricks. The bricks and prefabricated parts are bonded with high-strength glue. The desulfurization gun used by the steel plant has a total length of 9 meters, of which the total length of the refractory part is 5 meters and the external diameter is 280mm. The gun head prefabricated part 9 used in the present invention is located at the bottom of the desulfurization gun, with a total height of 500mm, an external diameter of refractory material of 280mm, and the internal steel structural parts and the upper steel structural parts are connected by pipe threads. The refractory machine-pressed bricks 6 used in the present invention are 300mm high and 280mm in external diameter. There are 15 machine-pressed bricks in total, of which from bottom to top, the 11th to 14th are slag line parts, and the 3rd and 15th are refractory machine-pressed bricks 10 with grouting ports.
[0068] The composition of the refractory castable of the gun head prefabricated part 9 is shown in Table 1. The water addition amount of the castable formula is 4.5-4.8wt%; its 110℃*24h dry compressive strength is about 26MPa; there is no peeling phenomenon after 20 times of thermal vibration at 1100℃, and its residual compressive strength is about 6MPa. Compared with the ordinary desulfurization spray gun castable, this formula group improves its high temperature strength, reduces the thermal conductivity of the refractory material, improves the anti-oxidation performance of the refractory material, and improves its erosion resistance in molten steel. The gun head nozzle adopts three-hole powder spraying, and the angle between each steel pipe is 120°. There are several tie plates 9-2 around each pipe to fix it, so that each pipe of the structure can be stressed at 360°; the three-hole distribution can make the desulfurizer spray evenly in three directions, so that the desulfurization gun body itself is evenly stressed in all directions, thereby reducing the shaking of the desulfurization gun during use and the occurrence of desulfurization transverse cracking and gun bending. The entire process of prefabricated parts, from on-site mixing to pouring and curing, can be completed in just 6 days.
[0069] Table 1: Example 1 Gun head prefabricated refractory castable formula
[0070]
[0071]
[0072] The formula composition of the refractory machine-pressed bricks in the slag line is shown in Table 2: The machine-pressed bricks with the modified formula have a volume density of 3.1g / cm 3 The room temperature compressive strength is 56Mpa, and the high temperature flexural strength is 6.8Mpa. This formula has good slag erosion resistance and thermal vibration resistance.
[0073] Table 2: Refractory machine-pressed brick formula for the slag line portion of Example 1
[0074]
[0075] The refractory machine-pressed bricks in other parts are made of Al-C, and the formula composition is shown in Table 3: Its volume density can reach 2.8g / cm 3 The room temperature compressive strength can reach more than 45Mpa, and the high temperature flexural strength is greater than 5Mpa. This formula has good high temperature strength and thermal vibration performance.
[0076] Table 3: Refractory machine-pressed brick formula for non-slag line area in Example 1
[0077]
[0078]
[0079] The production cycle of machine-pressed bricks, from batching to mixing and pressing bricks, and then to drying, can be completed in just 3 days.
[0080] 2. The surface of the outer square tube 1 is coated with polyurethane with a thickness greater than 2 mm to prevent direct contact between the high-aluminum self-flowing material and the steel structure. The polyurethane melts and disappears at high temperature, leaving a gap between the steel structure and the material, leaving space for the high-temperature expansion of the steel structure.
[0081] 3. The refractory materials assembled in each part are compressed by the spring pressure device to effectively solve the problem of crack generation and expansion. The energy of stress damage caused by the thermal shock process is released by the spring pressure device to effectively avoid cracks and expansion caused by the release of internal stress.
[0082] Implementation effect:
[0083] 1. Greatly shorten the production cycle. Usually, the production cycle of the pouring desulfurization spray gun is about 20 days. However, the various parts of the present invention can be made simultaneously. Most of them are machine-pressed bricks. The brick shape is relatively fixed. The production is efficient and convenient. Only assembly is required. The whole process only takes 7 days. High production efficiency. Traditional desulfurization spray guns all adopt the vertical pouring method. Due to the long length of the castable, only the vibrating motor vibrating rod and other devices are used to assist the pouring. It is difficult to ensure the pouring quality, and the production cycle is long.
[0084] 2. It significantly improves the abnormal offline conditions such as large longitudinal and transverse cracks on the surface of the gun body, erosion and fracture of the slag line, damage to the gun head, bending of the gun body, and internal gun blockage. During the statistical period from March to June this year, the average life of the pouring desulfurization spray gun was 26 times, and the proportion of desulfurization spray guns offline due to excessive transverse and longitudinal cracks was 38.46%; while the average life of the desulfurization spray gun made by the present invention was 41 times, and there were almost no desulfurization spray guns offline due to abnormal phenomena such as transverse and longitudinal cracks.
[0085] As can be seen from the above table, various measures have been taken to improve the abnormal offline conditions such as large longitudinal and transverse cracks on the surface of the gun body, erosion and fracture at the slag line, damage to the gun head, bending of the gun body, and internal gun blockage, so that the service life of the desulfurization gun has been significantly improved, with an increase of 57.7%. This not only meets the smelting requirements of the steel plant, but also creates considerable benefits for refractory manufacturers.
Claims
1. A production process for a crack-free, long-life composite desulfurization powder spray gun, characterized in that: The steps include: 1) Assemble and weld the steel structure, and weld the spring positioning plate to the outer square tube of the steel structure; 2) Apply polyurethane on the surface of the outer square tube of the steel structure with a thickness of not less than 2mm; 3) The spring and spring baffle are sleeved on the steel structure from the bottom of the steel structure in sequence, and then the refractory machine-pressed brick is sleeved on the steel structure and connected with the spring baffle. High-strength glue is applied between the refractory machine-pressed bricks to seal them. Finally, the prefabricated gun head is installed at the end of the steel structure, and the refractory machine-pressed bricks and the prefabricated gun head are bonded with high-strength glue; 4) Inject the self-flowing castable material through the grouting port on the refractory machine-pressed brick; The refractory machine-pressed bricks at the slag line of the refractory machine-pressed bricks are prepared from the following raw materials in parts by weight: 15-25 parts of alumina with a particle size of 5-3mm, 15-25 parts of alumina with a particle size of 3-1mm, 5-10 parts of brown corundum with a particle size of 3-1mm, 10-20 parts of brown corundum with a particle size of 1-0mm, 5-10 parts of silicon carbide with a particle size of 1-0mm, 2.8-3.0 parts of thermoplastic resin, 8-13 parts of -195 graphite, 0.5-2 parts of metal aluminum powder 200 mesh, 3-8 parts of silicon carbide 200 mesh, 8-15 parts of brown corundum 200 mesh, and 0.2-0.4 parts of methenamine; The refractory machine-pressed bricks at the non-slag line part of the refractory machine-pressed bricks are prepared from the following raw materials in parts by weight: 10-20 parts of alumina with a particle size of 5-3mm, 20-30 parts of alumina with a particle size of 3-1mm, 20-30 parts of alumina with a particle size of 1-0mm, 2.8-3.0 parts of thermoplastic resin, 8-15 parts of -194 graphite, 1-3 parts of metal aluminum powder 200 mesh, 8-15 parts of silicon carbide 200 mesh, 8-15 parts of brown corundum 200 mesh, and 0.2-0.4 parts of hexamethylenetetramine; The prefabricated casting material of the prefabricated gun head is prepared from the following raw materials in parts by weight: 20-30 parts of fused mullite with a particle size of 5-10mm, 10-20 parts of fused mullite with a particle size of 3-6mm, 10-15 parts of coke gemstone with a particle size of 1-3mm, 10-20 parts of coke gemstone with a particle size of 0-1mm, 3-6 parts of activated alumina micropowder 5μm, 3-8 parts of pure calcium aluminate cement, 5-8 parts of silicon carbide 200 mesh, 4-8 parts of kyanite 40 mesh, 3-5 parts of white corundum 240 mesh, 0.5-0.8 parts of high-efficiency water reducer, and 0.08-0.12 parts of zirconia fiber; The prefabricated gun head comprises a steel nozzle and a prefabricated casting material, wherein the prefabricated casting material is wrapped around the outside of the steel nozzle, and the steel nozzle is connected to the steel structure through a thread; The nozzle hole type is Y-type or T-type or three-hole or four-hole nozzle hole type, and each round tube of the nozzle structural part is fixed by welding several tie plates.
2. A powder spray gun structure produced by the production process of the crack-free long-life composite desulfurization powder spray gun according to claim 1, characterized in that: It includes a steel structure, a spring pressure device, a prefabricated gun head, and a refractory machine-pressed brick. The refractory machine-pressed brick is sleeved on the outside of the steel structure, the prefabricated gun head is installed at the bottom of the steel structure, and the spring pressure device is arranged at the upper end of the refractory machine-pressed brick so that the refractory machine-pressed brick and the prefabricated gun head are pressed and sealed, and a self-flowing castable material layer is filled between the refractory machine-pressed brick and the steel structure.
3. The powder spray gun structure produced by the production process of the crack-free long-life composite desulfurization powder spray gun according to claim 2 is characterized in that: The steel structure comprises an inner circular tube and an outer square tube. The inner circular tube is arranged inside the outer square tube, and a polyurethane layer is coated on the outer wall surface of the outer square tube.
4. The powder spray gun structure produced by the production process of the crack-free long-life composite desulfurization powder spray gun according to claim 2 is characterized in that: The spring pressure device includes a spring positioning plate, a spring, and a spring baffle. The spring positioning plate is fixedly connected to the steel structure. The spring is sleeved outside the steel structure and under the spring positioning plate. The spring baffle is arranged at the bottom of the spring and is slidably sleeved with the steel structure.
5. The powder spray gun structure produced by the production process of the crack-free long-life composite desulfurization powder spray gun according to claim 2 is characterized in that: The refractory machine pressed bricks are sealed by means of annular grooves and protrusions, and the refractory machine pressed bricks and the prefabricated gun head are also sealed by means of annular grooves and protrusions.
6. The powder spray gun structure produced by the production process of the crack-free long-life composite desulfurization powder spray gun according to claim 5 is characterized in that: Several of the refractory machine-pressed bricks are provided with grouting ports.
7. The powder spray gun structure produced by the production process of the crack-free long-life composite desulfurization powder spray gun according to claim 2 is characterized in that: The prefabricated gun head comprises a steel nozzle and a prefabricated casting material, wherein the prefabricated casting material is wrapped around the outside of the steel nozzle, and the steel nozzle is connected to a steel structural member through a thread.