Thermoplastic resin composition, resin molded product

By using an appropriate amount of glass fiber and glass flakes as reinforcing fillers in the thermoplastic resin, combined with polyamide resin and laser direct molding additives, the problems of decreased strength and increased warpage of the thermoplastic resin composition after heating are solved, and high mechanical strength is achieved and low-warpage resin molded products, and form plating suitable for portable electronic device components.

CN113292849BActive Publication Date: 2024-10-29MITSUBISHI CHEM CORP +1
View PDF 18 Cites 0 Cited by

Patent Information

Application Number
CN202110452754.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2018-09-28
Publication Date
2024-10-29
Estimated Expiration
2038-09-28

AI Technical Summary

Technical Problem

The mechanical strength of existing thermoplastic resin compositions decreases and warpage increases after heating. Especially when laser direct molding additives are used, the mechanical strength of resin molded products is poor and warpage is serious.

Method used

By adding 10 to 100 parts by mass of reinforcing fillers to the thermoplastic resin, including glass flakes and glass fibers with a thickness of 0.1 to 2 μm, the mass ratio of reinforcing fibers to glass flakes is 0.1 to 1, combined with polyamide resin and laser direct forming additives, Resin molded products with high mechanical strength and low warpage are formed.

Benefits of technology

It achieves high mechanical strength while reducing warpage after heating, and can form a coating that maintains performance, making it suitable for portable electronic equipment components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113292849B_ABST
    Figure CN113292849B_ABST
Patent Text Reader

Abstract

The present invention can provide a thermoplastic resin composition and a resin molded product, wherein the thermoplastic resin composition can provide a resin molded product that maintains high mechanical strength and reduces warping after heating. In addition, the present invention provides a thermoplastic resin composition, a resin molded product, a method for manufacturing a resin molded product with a plated layer, and a method for manufacturing a portable electronic device component, wherein, for a thermoplastic resin composition formulated with an LDS additive, the thermoplastic resin composition can provide a resin molded product that can form a plated layer, maintains high mechanical strength, and reduces warping after heating. In the above-mentioned thermoplastic resin composition, 10 to 100 parts by mass of reinforcing filler is contained relative to 100 parts by mass of crystalline thermoplastic resin, and the reinforcing filler includes reinforcing fibers and glass sheets with a thickness of 0.1 to 2 μm, and the mass ratio of reinforcing fibers to glass sheets, i.e., reinforcing fibers / glass sheets, is 0.1 to 1.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present application is a divisional application of an application filed on September 28, 2018, with application number 201880061671.5 and invention name “thermoplastic resin composition, resin molded article, method for manufacturing resin molded article with coating, and method for manufacturing portable electronic device components”. Technical Field

[0002] The present invention relates to a thermoplastic resin composition, a resin molded product, a method for producing a resin molded product with a plated layer, and a method for producing a portable electronic device component. Background Art

[0003] Crystalline thermoplastic resins have excellent mechanical properties and other physical and chemical characteristics. Therefore, they are widely used in vehicle parts, electrical and electronic equipment parts, and other precision equipment parts.

[0004] In addition, various additives are blended into thermoplastic resins to impart desired functions.

[0005] For example, Patent Document 1 discloses a polyamide resin composition comprising (A) a polyamide resin, (B) an inorganic filler, and (C) carbon black, wherein at least a portion of the (A) polyamide resin is (a1) an aromatic polyamide, and the (C) carbon black has an average primary particle size of 20 nm or more, and a ratio of specific surface area to DBP (dibutyl phthalate) oil absorption, i.e., specific surface area / DBP oil absorption, of 1.0 or less.

[0006] In addition, Patent Document 2 discloses a polyamide resin composition, which contains 20 to 150 parts by mass of glass fiber and 1 to 30 parts by mass of a laser direct structuring additive relative to 100 parts by mass of a polyamide resin component containing 50% by mass or more of a polyamide resin (A) having a saturated water absorption rate of 4% by mass or less when immersed in water.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent Application Publication No. 2017-014388

[0010] Patent Document 2: Japanese Patent Application Publication No. 2015-048440 Summary of the invention

[0011] Problems to be solved by the invention

[0012] As described above, various thermoplastic resin compositions are known. Here, it is known that if the mechanical strength is to be maintained at a high level, the warpage after heating may increase. The object of the present invention is to provide a thermoplastic resin composition and a resin molded product that solve the above-mentioned problems, and the thermoplastic resin composition can provide a resin molded product that maintains high mechanical strength and reduces the warpage after heating.

[0013] In addition, in recent years, laser direct structuring (hereinafter sometimes referred to as "LDS") technology has attracted attention as one of the technologies for forming three-dimensional antennas. LDS technology is a technology that activates the surface of a resin molded product containing an LDS additive by irradiating a laser, and then applying a metal to the activated portion to form a coating. However, LDS additives are generally very hard, so if they are mixed with reinforcing fibers, the reinforcing fibers will be damaged, and sometimes the mechanical strength of the resulting resin molded product will be poor. In addition, the resin molded product is also required to reduce warping after heating.

[0014] The second object of the present invention is to solve the above-mentioned problems in the above-mentioned LDS technology combined with an LDS additive, and to provide a thermoplastic resin composition, a resin molded product, a method for manufacturing a resin molded product with a plated layer, and a method for manufacturing a portable electronic device component that can form a plated layer and maintain high mechanical strength while reducing warping after heating.

[0015] Solutions to the problem

[0016] Based on the above problems, the present inventors have conducted intensive studies and found that the above problems can be solved by mixing reinforcing fibers and glass flakes having a thickness within a given range as reinforcing fillers at a given mixing ratio.

[0017] Specifically, the above-mentioned problems are solved by the following means <1>, preferably <2> to <22>.

[0018] <1> A thermoplastic resin composition comprising 10 to 100 parts by mass of a reinforcing filler based on 100 parts by mass of a crystalline thermoplastic resin, wherein the reinforcing filler comprises reinforcing fibers and glass flakes having a thickness of 0.1 to 2 μm, and the mass ratio of the reinforcing fibers to the glass flakes, i.e., reinforcing fibers / glass flakes, is 0.1 to 1.

[0019] <2> The thermoplastic resin composition according to <1>, wherein

[0020] The crystalline thermoplastic resin includes a polyamide resin.

[0021] <3> The thermoplastic resin composition according to <2>, wherein

[0022] The polyamide resin is a semi-aromatic polyamide resin.

[0023] <4> The thermoplastic resin composition according to <2>, wherein

[0024] The polyamide resin is composed of structural units derived from diamine and structural units derived from dicarboxylic acid, wherein 50 mol % or more of the structural units derived from diamine are derived from xylylenediamine, and 50 mol % or more of the structural units derived from dicarboxylic acid are derived from α,ω-straight-chain aliphatic dicarboxylic acid having 4 to 20 carbon atoms.

[0025] <5> The thermoplastic resin composition according to <4>, wherein

[0026] 50 mol% or more of the structural units derived from dicarboxylic acid are derived from sebacic acid.

[0027] <6> The thermoplastic resin composition according to <4> or <5>, wherein

[0028] 50 mol % or more of the structural units derived from diamine are derived from p-xylylenediamine.

[0029] <7> The thermoplastic resin composition according to <4>, wherein

[0030] 70 mol % or more of the structural units derived from dicarboxylic acid are derived from sebacic acid, and 70 mol % or more of the structural units derived from diamine are derived from p-xylylenediamine.

[0031] <8> The thermoplastic resin composition according to any one of <2> to <7>, wherein

[0032] 90% by mass or more of the polyamide resin is a polyamide resin having a saturated water absorption rate of 4.0% by mass or less after immersion in water.

[0033] <9> The thermoplastic resin composition according to <1>, wherein

[0034] The crystalline thermoplastic resin includes a polyamide resin and a polybutylene terephthalate resin.

[0035] <10> The thermoplastic resin composition according to <9>, wherein

[0036] The polyamide resin includes an aliphatic polyamide resin, the polybutylene terephthalate resin includes 70 to 30% by mass of a polybutylene terephthalate resin and 30 to 70% by mass of a modified polybutylene terephthalate resin, and the total does not exceed 100% by mass, and the polybutylene terephthalate resin is formed by a dicarboxylic acid component mainly composed of terephthalic acid or an ester derivative thereof, and a diol component mainly composed of 1,4-butanediol.

[0037] <11> The thermoplastic resin composition according to any one of <1> to <10>, wherein

[0038] The reinforcing fibers include glass fibers.

[0039] <12> The thermoplastic resin composition according to any one of <1> to <11>, further comprising 0.1 to 20 parts by mass of talc based on 100 parts by mass of the crystalline thermoplastic resin.

[0040] <13> The thermoplastic resin composition according to any one of <1> to <12>, further comprising 1 to 30 parts by mass of a laser direct structuring additive based on 100 parts by mass of the crystalline thermoplastic resin.

[0041] <14> The thermoplastic resin composition according to <13>, wherein

[0042] The laser direct structuring additive is selected from oxides containing copper and chromium, oxides containing antimony and tin, and oxides containing at least two metals and having a resistivity of 5×10 3 Conductive oxides with a resistance of Ω·cm or less.

[0043] <15> A resin molded article formed from the thermoplastic resin composition according to any one of <1> to <14>.

[0044] <16> A resin molded article formed from the thermoplastic resin composition according to <13> or <14>.

[0045] <17> The resin molded article according to <16>, further comprising a plated layer on the surface.

[0046] <18> The resin molded article according to <17>, wherein

[0047] The plating layer maintains the performance as an antenna.

[0048] <19> The resin molded article according to any one of <15> to <18>, which is a portable electronic device component.

[0049] <20> A method for manufacturing a resin molded article with a plated layer, the method comprising:

[0050] After irradiating the surface of the resin molded article described in <16> with laser light, a metal is applied to form a plating layer.

[0051] <21> The method for producing a plated resin molded article according to <20>, wherein:

[0052] The plating layer is a copper plating layer.

[0053] <22> A method for manufacturing a portable electronic device component having an antenna, the method comprising the method for manufacturing a plated resin molded article according to <20> or <21>.

[0054] Effects of the Invention

[0055] According to the present invention, a thermoplastic resin composition and a resin molded product can be provided, wherein the thermoplastic resin composition can provide a resin molded product that maintains high mechanical strength and reduces warpage after heating. In addition, a thermoplastic resin composition, a resin molded product, a method for producing a resin molded product with a plated layer, and a method for producing a portable electronic device component can be provided, wherein the thermoplastic resin composition can form a plated layer, maintains high mechanical strength, and reduces warpage after heating, even if the thermoplastic resin composition is a thermoplastic resin composition blended with an LDS additive. BRIEF DESCRIPTION OF THE DRAWINGS

[0056] Figure 1 This is a schematic diagram showing the process of providing a plating layer on the surface of a resin molded product.

[0057] Explanation of symbols

[0058] 1 Resin molded products

[0059] 2 Laser

[0060] 3 Part irradiated with laser

[0061] 4 Plating solution

[0062] 5 Plating DETAILED DESCRIPTION

[0063] Hereinafter, the content of the present invention will be described in detail. It should be noted that in the present specification, "to" is used to mean that the numerical values ​​described before and after it are included as the lower limit and the upper limit.

[0064] The thermoplastic resin composition of the present invention (hereinafter sometimes referred to as "the resin composition of the present invention") is characterized in that it contains 10 to 100 parts by mass of a reinforcing filler relative to 100 parts by mass of a crystalline thermoplastic resin, the reinforcing filler comprising reinforcing fibers and glass flakes having a thickness of 0.1 to 2 μm, and the mass ratio of the reinforcing fibers to the glass flakes, i.e., reinforcing fibers / glass flakes, is 0.1 to 1.

[0065] By setting it as such a structure, high mechanical strength can be maintained and warping after heating can be effectively suppressed. In addition, even if the LDS additive is added, these effects can be effectively achieved and a plating layer can be formed.

[0066] Hereinafter, the present invention will be described in detail.

[0067] <Crystalline thermoplastic resin>

[0068] Resin combination of the present invention comprises crystalline thermoplastic resin. As crystalline thermoplastic resin, polyamide resin, polyacetal resin, polybutylene terephthalate resin etc. can be exemplified, preferably polyamide resin and polybutylene terephthalate resin, more preferably polyamide resin. If crystalline polyamide resin is used, then when resin molding is molded, it can be cured faster, so it can be more effectively formed on the surface of resin molding. Therefore, the adhesion of resin molding and coating can be further improved.

[0069] In the resin composition of the present invention, the crystalline thermoplastic resin preferably accounts for 30% by mass or more, more preferably 35% by mass or more, further preferably 40% by mass or more, and further preferably 50% by mass or more. In addition, the upper limit of the content of the crystalline thermoplastic resin in the resin composition is preferably 80% by mass or less, more preferably 75% by mass or less, further preferably 70% by mass or less, and may also be 65% by mass or less.

[0070] The resin composition of the present invention may contain only one crystalline thermoplastic resin or two or more crystalline thermoplastic resins. When containing two or more crystalline thermoplastic resins, the total amount is preferably within the above range.

[0071] 《Polyamide resin》

[0072] The polyamide resin used in the present invention is not particularly limited, and a known polyamide resin can be used. For example, as the polyamide resin, reference can be made to the description in paragraphs 0011 to 0013 of JP-A-2011-132550.

[0073] The polyamide resin used in the present invention is preferably a semi-aromatic polyamide resin. Here, the semi-aromatic polyamide resin is composed of a structural unit derived from a diamine and a structural unit derived from a dicarboxylic acid, and 30 to 70 mol% of all structural units of the structural unit derived from the diamine and the structural unit derived from the dicarboxylic acid are structural units containing aromatic rings, and preferably 40 to 60 mol% of all structural units of the structural unit derived from the diamine and the structural unit derived from the dicarboxylic acid are structural units containing aromatic rings. By using such a semi-aromatic polyamide resin, the mechanical strength of the obtained resin molded product can be improved. As semi-aromatic polyamide resins, terephthalic acid polyamide resins (polyamide 6T, polyamide 9T), xylenediamine polyamide resins described later, etc. can be exemplified.

[0074] It is preferred that at least one of the polyamide resins used in the present invention is a polyamide resin (hereinafter sometimes referred to as a "xylylenediamine-based polyamide resin") which is composed of structural units derived from diamine and structural units derived from dicarboxylic acid, wherein 50 mol% or more of the structural units derived from diamine are derived from xylylenediamine, and 50 mol% or more of the structural units derived from dicarboxylic acid are derived from an α,ω-straight-chain aliphatic dicarboxylic acid having 4 to 20 carbon atoms.

[0075] More preferably, 70 mol% or more, further preferably 80 mol% or more, further preferably 90 mol% or more, and further preferably 95 mol% or more of the structural units derived from diamine in the xylylenediamine-based polyamide resin are derived from xylylenediamine. More preferably, 70 mol% or more, further preferably 80 mol% or more, further preferably 90 mol% or more, and further preferably 95 mol% or more of the structural units derived from dicarboxylic acid in the xylylenediamine-based polyamide resin are derived from α,ω-straight-chain aliphatic dicarboxylic acid having 4 to 20 carbon atoms.

[0076] The xylylenediamine is preferably p-xylylenediamine and m-xylylenediamine, and more preferably contains at least p-xylylenediamine.

[0077] As a preferred embodiment of the xylylenediamine-based polyamide resin of the present invention, there can be exemplified a resin in which 50 mol % or more (preferably 70 mol % or more, more preferably 90 mol % or more) of the structural units derived from diamine are derived from p-xylylenediamine.

[0078] Examples of diamines other than meta-xylylenediamine and para-xylylenediamine that can be used as the raw material diamine component of the xylylenediamine-based polyamide resin include aliphatic diamines such as tetramethylenediamine, pentamethylenediamine, 2-methylpentamethylenediamine, hexamethylenediamine, heptamethylenediamine, octamethylenediamine, nonamethylenediamine, decamethylenediamine, dodecamethylenediamine, 2,2,4-trimethyl-hexamethylenediamine, and 2,4,4-trimethylhexamethylenediamine, and 1,3-bis(1,3-diamine); Alicyclic diamines such as bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane, 1,3-diaminocyclohexane, 1,4-diaminocyclohexane, bis(4-aminocyclohexyl)methane, 2,2-bis(4-aminocyclohexyl)propane, bis(aminomethyl)decalin, and bis(aminomethyl)tricyclodecane, and diamines having an aromatic ring such as bis(4-aminophenyl)ether, p-phenylenediamine, and bis(aminomethyl)naphthalene can be used alone or in combination of two or more.

[0079] Examples of α,ω-straight-chain aliphatic dicarboxylic acids having 4 to 20 carbon atoms, which are preferably used as the raw material dicarboxylic acid component of the xylylenediamine-based polyamide resin, include succinic acid, glutaric acid, pimelic acid, suberic acid, azelaic acid, adipic acid, sebacic acid, undecanedioic acid, dodecanedioic acid and the like. One kind or a mixture of two or more kinds can be used. Among them, since the melting point of the polyamide resin is in a range suitable for molding processing, adipic acid or sebacic acid is more preferred, and sebacic acid is still more preferred.

[0080] As a preferred embodiment of the xylylenediamine-based polyamide resin in the present invention, there is exemplified a resin in which 50 mol % or more (preferably 70 mol % or more, more preferably 90 mol % or more) of the structural units derived from dicarboxylic acid are derived from sebacic acid.

[0081] In addition, as another preferred embodiment of the xylylenediamine-based polyamide resin in the present invention, there can be exemplified a mixture of a polyamide resin in which 50 mol % or more (preferably 70 mol % or more, more preferably 90 mol % or more) of the structural units derived from dicarboxylic acid are derived from sebacic acid, and a polyamide resin in which 50 mol % or more (preferably 70 mol % or more, more preferably 90 mol % or more) of the structural units derived from dicarboxylic acid are derived from adipic acid.

[0082] Examples of the dicarboxylic acid component other than the above-mentioned α,ω-straight-chain aliphatic dicarboxylic acid having 4 to 20 carbon atoms include phthalic acid compounds such as isophthalic acid, terephthalic acid, and phthalic acid, and isomers of naphthalene dicarboxylic acid such as 1,2-naphthalene dicarboxylic acid, 1,3-naphthalene dicarboxylic acid, 1,4-naphthalene dicarboxylic acid, 1,5-naphthalene dicarboxylic acid, 1,6-naphthalene dicarboxylic acid, 1,7-naphthalene dicarboxylic acid, 1,8-naphthalene dicarboxylic acid, 2,3-naphthalene dicarboxylic acid, 2,6-naphthalene dicarboxylic acid, and 2,7-naphthalene dicarboxylic acid. One kind or a mixture of two or more kinds thereof can be used.

[0083] It should be noted that, although the main components are composed of structural units derived from diamines and structural units derived from dicarboxylic acids, structural units other than these are not completely excluded, and structural units derived from lactams such as ε-caprolactam and lauryl lactam, and structural units derived from aliphatic aminocarboxylic acids such as aminocaproic acid and aminoundecanoic acid may also be included. Here, the main component means that among the structural units constituting the xylenediamine-based polyamide resin, the total number of structural units derived from diamines and structural units derived from dicarboxylic acids is the largest among all structural units. In the present invention, the total number of structural units derived from diamines and structural units derived from dicarboxylic acids in the xylenediamine-based polyamide resin preferably accounts for more than 90% of all structural units, and more preferably accounts for more than 95%.

[0084] As an example of the mixed form of the polyamide resin of the present invention, a mixture of a xylylenediamine-based polyamide resin and a terephthalic acid-based polyamide resin can also be exemplified.

[0085] The resin composition of the present invention is preferably a polyamide resin having a saturated water absorption of 4.0% or less after immersion in water, in which 90% or more of the polyamide resin contained in the composition is a polyamide resin. By adopting such a polyamide resin, the water absorption dimensional change after molding is reduced, and a plating layer can be properly formed. Moreover, after saturation in water, heating and cooling, the adhesion between the plating layer and the resin molded product can also be maintained. The saturated water absorption of the polyamide resin (A) used in the present invention is preferably 3.5% or less, more preferably 2.5 to 3.3% by mass.

[0086] The saturated water absorption is measured by the method described in Examples described later.

[0087] The melting point of the polyamide resin is preferably 150 to 350°C, more preferably 180 to 330°C, further preferably 200 to 330°C, and further preferably 200 to 320°C.

[0088] The melting point is measured by the method described in Examples described later.

[0089] The lower limit of the number average molecular weight (Mn) of the polyamide resin is preferably 6,000 or more, more preferably 8,000 or more, further preferably 10,000 or more, further preferably 15,000 or more, further preferably 20,000 or more, further preferably 22,000 or more. The upper limit of the above Mn is preferably 35,000 or less, more preferably 30,000 or less, further preferably 28,000 or less, further preferably 26,000 or less. In such a range, heat resistance, elastic modulus, dimensional stability, and molding processability become better.

[0090] As one embodiment of the resin composition of the present invention, a method that substantially does not contain thermoplastic resins other than polyamide resins can be cited. Substantially not containing means that the content of thermoplastic resins other than polyamide resins is preferably less than 5% by mass of the resin composition of the present invention, more preferably less than 3% by mass, and further preferably less than 1% by mass.

[0091] 《Polybutylene terephthalate resin》

[0092] The polybutylene terephthalate resin used in the resin composition of the present invention is a polyester resin having a structure in which a terephthalic acid unit and a 1,4-butanediol unit form an ester bond, and includes, in addition to the polybutylene terephthalate resin (homopolymer), a polybutylene terephthalate copolymer containing other copolymer components except the terephthalic acid unit and the 1,4-butanediol unit, and a mixture of the homopolymer and the copolymer.

[0093] The polybutylene terephthalate resin may also contain dicarboxylic acid units other than terephthalic acid. Specific examples of other dicarboxylic acids include aromatic dicarboxylic acids such as isophthalic acid, phthalic acid, 1,5-naphthalene dicarboxylic acid, 2,5-naphthalene dicarboxylic acid, 2,6-naphthalene dicarboxylic acid, biphenyl-2,2'-dicarboxylic acid, biphenyl-3,3'-dicarboxylic acid, biphenyl-4,4'-dicarboxylic acid, bis(4,4'-carboxyphenyl)methane, anthracene dicarboxylic acid, and 4,4'-diphenyl ether dicarboxylic acid; alicyclic dicarboxylic acids such as 1,4-cyclohexane dicarboxylic acid and 4,4'-dicyclohexyl dicarboxylic acid; and aliphatic dicarboxylic acids such as adipic acid, sebacic acid, azelaic acid, and dimer acid.

[0094] As the diol unit, in addition to 1,4-butanediol, other diol units may be included. Specific examples of other diol units include aliphatic or alicyclic diols having 2 to 20 carbon atoms, bisphenol derivatives, etc. Specific examples include ethylene glycol, propylene glycol, 1,5-pentanediol, 1,6-hexanediol, neopentyl glycol, decamethylene glycol, cyclohexanedimethanol, 4,4'-dicyclohexylhydroxymethane, 4,4'-dicyclohexylhydroxypropane, ethylene oxide addition diols of bisphenol A, etc. In addition, in addition to the above-mentioned bifunctional monomers, trifunctional monomers such as trimellitic acid, trimesic acid, pyromellitic acid, pentaerythritol, trimethylolpropane, etc., for introducing a branched structure, or monofunctional compounds such as fatty acids for adjusting the molecular weight may be used in combination in small amounts.

[0095] It should be noted that the copolymerization amount of the diol units other than 1,4-butanediol is preferably 1 mol% or more and less than 50 mol% of the total segments of the polybutylene terephthalate resin. Among them, the copolymerization amount is preferably 2 mol% or more and less than 50 mol%, more preferably 3 to 40 mol%, and particularly preferably 5 to 20 mol%.

[0096] The polybutylene terephthalate resin is preferably a polybutylene terephthalate homopolymer obtained by polycondensing terephthalic acid and 1,4-butanediol, and may also be a polybutylene terephthalate copolymer containing one or more dicarboxylic acids other than the above-mentioned terephthalic acid as carboxylic acid units and / or containing one or more diols other than the above-mentioned 1,4-butanediol as diol units.

[0097] For polybutylene terephthalate resin, it can be produced by melt polymerization of a dicarboxylic acid component with terephthalic acid as the main component or its ester derivatives and a diol component with 1,4-butanediol as the main component in a batch or continuous manner. The dicarboxylic acid component with terephthalic acid as the main component means that the component with the largest content among the dicarboxylic acids is terephthalic acid, preferably 70 mol% or more of terephthalic acid, more preferably 80 mol% or more of terephthalic acid, and further preferably 90 mol% or more of terephthalic acid. In addition, the diol component with 1,4-butanediol as the main component means that the component with the largest content among the diol components is 1,4-butanediol, preferably 70 mol% or more of 1,4-butanediol, more preferably 80 mol% or more of 1,4-butanediol, and further preferably 90 mol% or more of 1,4-butanediol.

[0098] Furthermore, after a low molecular weight polybutylene terephthalate resin is produced by melt polymerization, the degree of polymerization (or molecular weight) can be increased to a desired value by further performing solid phase polymerization in a nitrogen stream or under reduced pressure.

[0099] The polybutylene terephthalate resin is preferably obtained by a production method in which a dicarboxylic acid component mainly composed of terephthalic acid and a diol component mainly composed of 1,4-butanediol are continuously melt-polycondensed.

[0100] The catalyst used in the esterification reaction may be a conventionally known catalyst, and examples thereof include titanium compounds, tin compounds, magnesium compounds, and calcium compounds. Among them, titanium compounds are particularly preferred. Specific examples of titanium compounds as esterification catalysts include titanium alkoxides such as tetramethyl titanate, tetraisopropyl titanate, and tetrabutyl titanate, and titanium phenolates such as tetraphenyl titanate.

[0101] The polybutylene terephthalate resin can be a polybutylene terephthalate resin modified by copolymerization. As its specific preferred copolymer, polyalkylene glycols, in particular polyester ether resins, dimer acid copolymerized polybutylene terephthalate resins, isophthalic acid copolymerized polybutylene terephthalate resins formed by copolymerization of polytetramethylene glycol, are listed, preferably isophthalic acid copolymerized polybutylene terephthalate resin. It should be noted that the copolymerization amount of these copolymers is more than 1 mol% and less than 50 mol% in all segments of the polybutylene terephthalate resin. Among them, the copolymerization amount is preferably 2 to 50 mol%, more preferably 3 to 40 mol%, and particularly preferably 5 to 20 mol%.

[0102] When a copolymer is used as the polybutylene terephthalate resin, a polyester ether resin obtained by copolymerizing polytetramethylene glycol is preferably used. The proportion of the tetramethylene glycol component in the copolymerization is preferably 3 to 40% by mass, more preferably 5 to 30% by mass, and further preferably 10 to 25% by mass. By setting such a copolymerization ratio, it is easy to improve fluidity, toughness, and tracking resistance, so it is preferred.

[0103] The terminal carboxyl amount of the polybutylene terephthalate resin can be appropriately selected and determined, usually 60eq / ton or less, preferably 50eq / ton or less, more preferably 30eq / ton or less. When it exceeds 50eq / ton, gas is easily generated when the resin composition is melt-molded. The lower limit of the terminal carboxyl amount is not particularly limited, but considering the productivity of the manufacture of the polybutylene terephthalate resin, it is usually 10eq / ton.

[0104] It should be noted that the terminal carboxyl group amount of the polybutylene terephthalate resin is a value measured by dissolving 0.5 g of the polyalkylene terephthalate resin in 25 mL of benzyl alcohol and titrating with a 0.01 mol / l benzyl alcohol solution of sodium hydroxide. As a method for adjusting the terminal carboxyl group amount, it can be carried out by any existing known method such as a method for adjusting polymerization conditions such as a raw material addition ratio, a polymerization temperature, and a decompression method during polymerization, and a method for reacting a terminal end-capping agent.

[0105] The intrinsic viscosity of the polybutylene terephthalate resin is preferably 0.5 to 2 dL / g. From the viewpoint of moldability and mechanical properties, an intrinsic viscosity in the range of 0.6 to 1.5 dL / g is more preferred. When a polybutylene terephthalate resin having an intrinsic viscosity lower than 0.5 dL / g is used, the resulting resin composition tends to have a low mechanical strength. In addition, when it is higher than 2 dL / g, the fluidity of the resin composition sometimes deteriorates, which deteriorates the moldability.

[0106] In addition, the intrinsic viscosity of a polybutylene terephthalate resin is a value measured at 30 degreeC in the mixed solvent of tetrachloroethane and phenol of 1:1 (mass ratio).

[0107] As one embodiment of the resin component in the resin composition of the present invention, there can be exemplified an embodiment in which the polybutylene terephthalate resin and the polyamide resin account for 85% by mass or more (preferably 90% by mass or more, more preferably 95% by mass or more) of the resin component.

[0108] In the above embodiment, regarding the ratio of the polybutylene terephthalate resin to the polyamide resin, the total amount is 50 to 70% by mass of the polybutylene terephthalate resin, and preferably 50 to 30% by mass of the polyamide resin.

[0109] In the above embodiment, the polybutylene terephthalate resin preferably comprises 70 to 30% by mass of a polybutylene terephthalate resin and 30 to 70% by mass of a modified polybutylene terephthalate resin (but the total does not exceed 100% by mass), wherein the polybutylene terephthalate resin is formed of a dicarboxylic acid component with terephthalic acid as the main component or its ester derivative, and a diol component with 1,4-butanediol as the main component. More preferably, the polybutylene terephthalate resin comprises 60 to 40% by mass of a polybutylene terephthalate resin and 40 to 60% by mass of a modified polybutylene terephthalate resin, wherein the polybutylene terephthalate resin is formed of a dicarboxylic acid component with terephthalic acid as the main component or its ester derivative, and a diol component with 1,4-butanediol as the main component.

[0110] In the above embodiment, the polyamide resin is preferably an aliphatic polyamide resin, preferably polyamide 6 and polyamide 66, and more preferably polyamide 6.

[0111] <Reinforcement filler>

[0112] In the resin composition of the present invention, 10 to 100 parts by mass of reinforcing filler are included relative to 100 parts by mass of crystalline thermoplastic resin. The reinforcing filler is preferably 20 parts by mass or more, more preferably 30 parts by mass or more, further preferably 35 parts by mass or more, and further preferably 40 parts by mass or more relative to 100 parts by mass of crystalline thermoplastic resin. In addition, the reinforcing filler is preferably 90 parts by mass or less, more preferably 80 parts by mass or less, further preferably 75 parts by mass or less, and may also be 70 parts by mass or less relative to 100 parts by mass of crystalline thermoplastic resin.

[0113] In the resin composition of the present invention, the reinforcing filler preferably accounts for 10 to 45% by mass, more preferably 15 to 40% by mass, and may also account for 20 to 30% by mass.

[0114] The resin composition of the present invention may contain only one reinforcing filler or two or more reinforcing fillers. When containing two or more reinforcing fillers, the total amount is preferably within the above range.

[0115] In the resin composition of the present invention, the mass ratio of the reinforcing fiber of the reinforcing filler to the glass flake having a thickness of 0.1 to 2 μm, i.e., reinforcing fiber / glass flake, is 0.1 to 1. The mass ratio is preferably 0.2 or more, more preferably 0.3 or more, further preferably 0.4 or more, and further preferably 0.45 or more.

[0116] The resin composition of the present invention may contain only one kind of each of the reinforcing fiber and the glass flake having a thickness of 0.1 to 2 μm, or may contain two or more kinds of each. When containing two or more kinds, the total amount is preferably within the above range.

[0117] The resin composition of the present invention may contain other reinforcing fillers in addition to the reinforcing fibers and the glass flakes having a thickness of 0.1 to 2 μm, or may not contain other reinforcing materials.

[0118] Examples of other reinforcing fillers include flaky, spherical, and needle-shaped inorganic fillers, and examples of components thereof include glass, metal oxides, metal hydroxides, carbonates, and sulfates.

[0119] An example of an embodiment of the resin composition of the present invention is a resin composition that substantially does not contain any reinforcing filler other than reinforcing fibers and glass flakes having a thickness of 0.1 to 2 μm. Substantially containing no reinforcing filler means that the content of reinforcing fillers other than reinforcing fibers and glass flakes having a thickness of 0.1 to 2 μm is 5% by mass or less of the total amount of reinforcing fillers contained in the resin composition, preferably 3% by mass or less, and more preferably 1% by mass or less.

[0120] It should be noted that the reinforcing filler in the present invention does not include substances belonging to LDS additives and talc.

[0121] Reinforced Fiber

[0122] The resin composition of the present invention contains reinforcing fibers. Examples of the reinforcing fibers include carbon fibers and glass fibers, and preferably contain glass fibers.

[0123] The reinforcing fiber in the present invention refers to a fibrous inorganic material, and more specifically, preferably a chopped shape in which 1,000 to 10,000 reinforcing fibers are bundled and cut into a predetermined length.

[0124] The number average fiber length of the reinforcing fiber in the present invention is preferably 0.5 to 10 mm, more preferably 1 to 5 mm. By using reinforcing fibers with such a number average fiber length, the mechanical strength can be further improved. The number average fiber length can be calculated by randomly extracting the object reinforcing fiber whose fiber length is to be measured from the image obtained by observation under an optical microscope, measuring its long side, and calculating the number average fiber length based on the obtained measured value. The observation magnification is set to 20 times, and the number of measured roots is set to 1,000 or more. It is basically equivalent to the cut length.

[0125] In addition, the cross section of the reinforcing fiber can be any shape such as a circle, an ellipse, an oblong, a rectangle, a shape formed by combining two short sides of a semicircle and a rectangle, a cocoon shape, etc., preferably a circle. The circle here includes not only a circle in the mathematical sense, but also a shape generally referred to as a circle in the technical field of the present invention.

[0126] The lower limit of the number average fiber diameter of the reinforcing fiber is preferably 4.0 μm or more, more preferably 4.5 μm or more, and further preferably 5.0 μm or more. The upper limit of the number average fiber diameter of the reinforcing fiber is preferably 15.0 μm or less, more preferably 14.0 μm or less, and can be 12.0 μm or less. By using reinforcing fibers with a number average fiber diameter in such a range, a resin molded product with better wet heat plating properties can be obtained. In addition, in the case where the resin molded product is stored for a long time or subjected to long-term heat treatment, high plating properties can also be maintained. It should be noted that the number average fiber diameter of the reinforcing fiber is calculated as follows: for the image obtained by observation under an electron microscope, the object glass fiber whose fiber diameter is to be measured is randomly extracted, and the fiber diameter is measured at a position close to the central part, and the measured value is calculated. The observation magnification is set to 1,000 times and the number of roots is set to 1,000 or more. The number average fiber diameter of a glass fiber having a cross-section other than a circle is converted to a number average fiber diameter when the circle has the same area as the cross-section.

[0127] Next, the glass fiber preferably used in the present invention will be described.

[0128] Glass fiber can be obtained by melt spinning commonly supplied E glass (Electrical glass), C glass (Chemical glass), A glass (Alkali glass), S glass (High strength glass) and alkali-resistant glass, and any fiber can be used as long as it can be made into glass fiber without particular limitation. In the present invention, it is preferred to contain E glass.

[0129] The glass fiber used in the present invention is preferably surface treated with a surface treatment agent such as a silane coupling agent such as γ-methacryloxypropyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-aminopropyltriethoxysilane, etc. The amount of the surface treatment agent attached is preferably 0.01 to 1% by mass of the glass fiber. In addition, it is also possible to use a fiber that has been surface treated with a resin having film-forming ability such as a lubricant such as a fatty acid amide compound, silicone oil, an antistatic agent such as a quaternary ammonium salt, an epoxy resin, a urethane resin, a mixture of a resin having film-forming ability and a heat stabilizer, a flame retardant, etc. as needed.

[0130] Glass fiber can be obtained as a commercial product, for example, T-286H, T-756H, T-289H manufactured by Nippon Electric Glass Co., Ltd., DEFT2A manufactured by Owens Corning, HP3540 manufactured by PPG, CSG3PA820 manufactured by Nittobo Co., Ltd., etc.

[0131] Glass Piece

[0132] The resin composition of the present invention contains a glass sheet with a thickness of 0.1 to 2 μm. The thickness of the glass sheet refers to the average thickness. The thickness of the glass sheet is preferably 0.3 μm or more, more preferably 0.4 μm or more, further preferably 0.5 μm or more, and further preferably 0.6 μm or more. In addition, the thickness of the glass sheet is preferably 1.8 μm or less, more preferably 1.6 μm or less, further preferably 1.4 μm or less, further preferably 1.2 μm or less, further preferably 1.0 μm or less, and further preferably 0.8 μm or less. Here, the average thickness is measured by the following method. That is, for more than 100 glass sheets, a scanning electron microscope (SEM) is used to measure the thickness of each sheet, and the measured values ​​are averaged and obtained. The sample stage of the scanning electron microscope is adjusted by a sample stage micro-motion device so that the cross section (thickness plane) of the glass sheet is perpendicular to the irradiation electron beam axis of the scanning electron microscope.

[0133] The glass composition of the glass sheet described above can be applied to various glass compositions represented by A glass, C glass, and E glass, and is not particularly limited.

[0134] <Laser Direct Structuring (LDS) Additives>

[0135] The resin composition of the present invention contains a laser direct structuring (LDS) additive. The LDS additive in the present invention refers to the following compound: relative to 100 parts by mass of a crystalline thermoplastic resin, 10 parts by mass of an additive considered to be an LDS additive is added, and irradiation is performed using a YAG laser with a wavelength of 1064 nm with an output power of 10 W, a frequency of 80 kHz, and a speed of 3 m / s. The subsequent plating process is implemented in an M-Copper85 chemical plating tank manufactured by MacDermid. When a metal is applied to the laser irradiated surface, a compound that can form a coating. The LDS additive used in the present invention may be a synthetic product or a commercial product. In addition, in addition to commercial products sold in the form of LDS additives, as long as the requirements of the LDS additive of the present invention are met, the commercial products may also be substances sold for other purposes. Only one LDS additive may be used, or two or more may be used in combination.

[0136] The first embodiment of the LDS additive used in the present invention is a compound containing copper and chromium. The LDS additive of the first embodiment preferably contains 10 to 30% by mass of copper. In addition, it preferably contains 15 to 50% by mass of chromium. The LDS additive of the first embodiment is preferably an oxide containing copper and chromium.

[0137] The copper and chromium are preferably contained in a spinel structure. The spinel structure is a complex oxide and can be regarded as AB 2 O 4 One of the representative crystal structures of type compounds (A and B are metal elements).

[0138] The LDS additive of the first embodiment may contain trace amounts of other metals in addition to copper and chromium. Examples of other metals include antimony, tin, lead, indium, iron, cobalt, nickel, zinc, cadmium, silver, bismuth, arsenic, manganese, magnesium, and calcium, preferably manganese. These metals may exist in the form of oxides.

[0139] A preferred example of the LDS additive according to the first embodiment is an LDS additive having a content of metal oxide other than copper chromium oxide of 10% by mass or less.

[0140] A second embodiment of the LDS additive used in the present invention contains at least one of antimony and phosphorus and tin oxide, and preferably contains antimony and tin oxide.

[0141] The LDS additive of the second embodiment is more preferably an additive having a tin content greater than the phosphorus and antimony contents, and the amount of tin is further preferably 80% by mass or more relative to the total amount of tin, phosphorus, and antimony.

[0142] In particular, the LDS additive of the second embodiment is preferably an oxide containing antimony and tin, more preferably an oxide containing more tin than antimony, and still more preferably an oxide containing 80 mass % or more of tin relative to the total amount of tin and antimony.

[0143] More specifically, as the LDS additive of the second embodiment, tin oxide doped with antimony, tin oxide doped with antimony oxide, tin oxide doped with phosphorus, and tin oxide doped with phosphorus oxide can be listed, preferably tin oxide doped with antimony and tin oxide doped with antimony oxide, and more preferably tin oxide doped with antimony oxide. For example, in the LDS additive containing phosphorus and tin oxide, the phosphorus content can be listed as 1 to 20% by mass. In addition, in the LDS additive containing antimony and tin oxide, the antimony content is preferably 1 to 20% by mass. In addition, in the LDS additive containing phosphorus, antimony and tin oxide, the phosphorus content is preferably 0.5 to 10% by mass, and the antimony content is preferably 0.5 to 10% by mass.

[0144] The third embodiment of the LDS additive used in the present invention preferably includes at least two metals and a resistivity of 5×10 3 The resistivity of the conductive oxide is more preferably 8×10 2 Ω·cm or less, more preferably 7×10 2 Ω·cm or less, more preferably 5×10 2 Ω·cm or less. There is no particular restriction on its lower limit, and for example, it can be set to 1×10 1 Ω·cm or more, and can be further set to 1×10 2 Ω·cm or more.

[0145] The resistivity of the conductive oxide of the present invention is generally referred to as powder resistivity, and can be measured by placing 10 g of conductive oxide powder into a cylinder with an inner diameter of 25 mm, the inner surface of which has been processed with Teflon (registered trademark), and pressurizing the cylinder to 100 kgf / cm 2 (Filling rate: 20%), measured using a "3223 type" tester manufactured by Yokogawa Electric Corporation.

[0146] The LDS additive used in the third embodiment contains a resistivity of 5×10 3 The conductive oxide with a resistance of Ω·cm or less may be used without any particular limitation, and preferably contains at least two metals, and specifically preferably contains a metal of the nth group (n is an integer of 3 to 16) and a metal of the n+1th group of the periodic table. n is more preferably an integer of 10 to 13, and further preferably 12 or 13.

[0147] For the LDS additive used in the third embodiment, when the total content of the metal of the periodic table group n (n is an integer of 3 to 16) and the content of the metal of the group n+1 in the LDS additive is set to 100 mol%, the content of one metal is preferably 15 mol% or less, more preferably 12 mol% or less, and further preferably 10 mol% or less. There is no particular restriction on its lower limit, but it is preferably 0.0001 mol% or more. By making the content of two or more metals in such a range, the plating property can be improved. In the present invention, a metal oxide of the group n doped with a metal of the group n+1 is particularly preferred.

[0148] In addition, in the LDS additive used in the third embodiment, it is preferred that 98% by mass or more of the metal component contained in the LDS additive be composed of the above-mentioned Group n metal and Group n+1 metal of the periodic table.

[0149] Examples of metals of the nth group of the periodic table include group 3 (scandium, yttrium), group 4 (titanium, zirconium, etc.), group 5 (vanadium, niobium, etc.), group 6 (chromium, molybdenum, etc.), group 7 (manganese, etc.), group 8 (iron, ruthenium, etc.), group 9 (cobalt, rhodium, iridium, etc.), group 10 (nickel, palladium, platinum), group 11 (copper, silver, gold, etc.), group 12 (zinc, cadmium, etc.), group 13 (aluminum, gallium, indium, etc.), group 14 (germanium, tin, etc.), group 15 (arsenic, antimony, etc.), and group 16 (selenium, tellurium, etc.). Among them, metals of group 12 (n=12) are preferred, and zinc is more preferred.

[0150] Examples of metals of Group n+1 of the periodic table include Group 4 (titanium, zirconium, etc.), Group 5 (vanadium, niobium, etc.), Group 6 (chromium, molybdenum, etc.), Group 7 (manganese, etc.), Group 8 (iron, ruthenium, etc.), Group 9 (cobalt, rhodium, iridium, etc.), Group 10 (nickel, palladium, platinum), Group 11 (copper, silver, gold, etc.), Group 12 (zinc, cadmium, etc.), Group 13 (aluminum, gallium, indium, etc.), Group 14 (germanium, tin, etc.), Group 15 (arsenic, antimony, etc.), and Group 16 (selenium, tellurium, etc.). Among them, metals of Group 13 (n+1=13) are preferred, aluminum or gallium is more preferred, and aluminum is further preferred.

[0151] The LDS additive used in the third embodiment may contain metals other than conductive metal oxides. Examples of metals other than conductive oxides include antimony, titanium, indium, iron, cobalt, nickel, cadmium, silver, bismuth, arsenic, manganese, chromium, magnesium, and calcium. These metals may exist in the form of oxides. The content of these metals is preferably 0.01% by mass or less relative to the LDS additive.

[0152] Among the above, in the present invention, the LDS additive preferably contains at least one of copper, antimony and tin, and more preferably contains copper. Therefore, the LDS additive of the first embodiment is more preferred.

[0153] The number average particle size of the LDS additive used in the present invention is preferably 0.01 to 100 μm, more preferably 0.05 to 30 μm, and even more preferably 0.05 to 15 μm. By setting the average particle size to such a level, the surface of the plated layer can be made more uniform.

[0154] The content of the LDS additive in the resin composition is preferably 1 to 30 parts by mass, more preferably 2 to 25 parts by mass, further preferably 5 to 20 parts by mass, and further preferably 5 to 15 parts by mass, relative to 100 parts by mass of the crystalline thermoplastic resin. By setting the content of the LDS additive to such a range, the plating property of the obtained resin molded product can be made better. In addition, as described later, by combining with talc, a plating layer can be formed with a small content. When two or more LDS additives are included, the total amount is preferably in the above range.

[0155] <Mold release agent>

[0156] The resin composition of the present invention may further contain a release agent. The release agent is mainly used to improve the productivity of the resin composition during molding. Examples of the release agent include aliphatic carboxylic acid amides, aliphatic carboxylic acids, esters of aliphatic carboxylic acids and alcohols, aliphatic hydrocarbon compounds with a number average molecular weight of 200 to 15,000, and polysiloxane silicone oils.

[0157] For details of the release agent, reference can be made to paragraphs 0037 to 0042 of Japanese Patent Application Laid-Open No. 2016-196563 and paragraphs 0048 to 0058 of Japanese Patent Application Laid-Open No. 2016-078318, and these contents are incorporated herein.

[0158] In the case of coordinating a mold release agent, relative to the resin combination, the lower limit of the content of the mold release agent is preferably more than 0.001 mass %, more preferably more than 0.01 mass %, in addition, the upper limit is preferably less than 2.0 mass %, more preferably less than 1.5 mass %. By being set to such a scope, it is possible to make mold release good, and it is possible to prevent mold contamination during injection molding. A mold release agent can be used alone or in combination with more than two kinds. When using more than two kinds, the preferred total amount is the above range.

[0159] <Talc>

[0160] The resin composition of the present invention may further contain talc. By adding talc, dimensional stability and product appearance can be improved. In addition, by adding talc, the growth rate of the coating can be increased. In addition, by adding talc, the plating property of the resin molded product can be improved even if the content of the LDS additive is reduced. Talc can be talc that has been surface-treated with at least one compound selected from polyorganohydrogensiloxanes and organopolysiloxanes. In this case, the amount of siloxane compound attached to the talc is preferably 0.1 to 5% by mass of the talc.

[0161] The number average particle size of talc is preferably 1 to 50 μm, more preferably 2 to 25 μm. Talc is generally scaly, and the length of the longest part is taken as the average particle size. The number average particle size of talc is calculated as follows: for an image obtained by observation under an electron microscope, a talc of which the particle size is to be measured is randomly extracted and the particle size is measured, and the calculation is performed based on the obtained measured value. The observation magnification is set to 1,000 times and the number of measurements is set to 1,000 or more.

[0162] When talc is blended, the content of talc in the resin composition of the present invention is preferably 0.1 to 20 parts by mass based on 100 parts by mass of the crystalline thermoplastic resin.

[0163] When the LDS additive is added, the content of talc in the resin composition of the present invention is preferably 1 to 200 parts by mass, more preferably 10 to 150 parts by mass, further preferably 30 to 120 parts by mass, and further preferably 80 to 120 parts by mass relative to 100 parts by mass of the LDS additive. In addition, when the talc is surface-treated with a siloxane compound, the content of the talc surface-treated with the siloxane compound is preferably within the above range.

[0164] <Other additives>

[0165] In addition to the above, the resin composition of the present invention may also include other ingredients. As other ingredients, flame retardants, light stabilizers, heat stabilizers, alkalis, elastomers, titanium oxide, antioxidants, hydrolysis resistance improvers, matting agents, ultraviolet absorbers, nucleating agents, plasticizers, dispersants, antistatic agents, anti-coloring agents, anti-gelling agents, coloring agents, etc. can be exemplified. The details can be referred to the records of paragraphs 0130 to 0155 of the Gazette of Japanese Patent No. 4894982, which are introduced into this specification. These components are preferably less than 20% by mass of the resin composition in total. These components can be used only one kind respectively, or two or more kinds can be used in combination.

[0166] <Method for producing resin composition>

[0167] As a method for producing the resin composition of the present invention, any method may be adopted.

[0168] For example, the following method can be cited: polyamide resin, reinforcing filler (reinforcing fiber, glass flake), LDS additive, etc. are mixed with a mixing device such as a V-type mixer to prepare a total mixed product, and then melt-kneading is performed in an extruder with a vent to form pellets. Alternatively, as a two-step mixing method, the following method can be cited: after fully mixing the components other than the reinforcing filler in advance, melt-kneading is performed in an extruder with a vent to produce pellets, and then the pellets and the reinforcing filler are mixed and melt-kneaded in an extruder with a vent.

[0169] In addition, the following method can be listed: a mixture is prepared in advance by thoroughly mixing the components other than the reinforcing filler using a V-type mixer, the mixture is supplied through the first chute of a twin-screw extruder with a vent, the reinforcing filler is supplied through the second chute in the extruder, the mixture is melt-kneaded, and the mixture is pelletized.

[0170] In the screw structure of the kneading zone of the extruder, it is preferred that a component that promotes kneading is provided on the upstream side, and a component having a pressure-increasing capability is provided on the downstream side.

[0171] Examples of the element that promotes kneading include a progressive kneading disc element, an orthogonal kneading disc element, a wide kneading disc element, and a progressive mixing screw element.

[0172] The heating temperature during melt kneading can be appropriately selected from the range of 180 to 360°C. When the temperature is too high, decomposition gas is easily generated, which sometimes causes extrusion failure such as broken wires. Therefore, it is preferred to select a screw structure that takes shear heat generation into consideration. In order to suppress decomposition during kneading and molding in the subsequent process, it is preferred to use an antioxidant or a heat stabilizer.

[0173] <Resin molded products>

[0174] The present invention also discloses a resin molded article obtained by molding the resin composition of the present invention.

[0175] When the resin composition of the present invention is molded into a thickness of 4 mm, the flexural strength measured according to ISO 178 is preferably 170 MPa or more, more preferably 180 MPa or more, and further preferably 190 MPa or more. The upper limit of the flexural strength is not particularly limited, for example, it is actually 270 MPa or less, further 260 MPa or less, and particularly 250 MPa or less.

[0176] When the resin composition of the present invention is molded into a thickness of 4 mm, the bending modulus measured according to ISO 178 is preferably 7.5 GPa or more, more preferably 8.0 GPa or more, and further preferably 8.5 GPa or more. The upper limit of the above-mentioned bending modulus is not particularly limited, for example, it is actually 15 GPa or less, further 14 GPa or less, and particularly 13 GPa or less.

[0177] When the resin composition of the present invention is molded into a thickness of 4 mm, the notched Charpy impact strength measured according to ISO 179 is preferably 3 kJ / m 2 The upper limit of the notched Charpy impact strength is not particularly limited, but is, for example, 10 kJ / m 2 Below, and even less than 9kJ / m 2 , especially 7kJ / m 2 the following.

[0178] When the resin composition of the present invention is molded into a thickness of 4 mm, the unnotched Charpy impact strength measured according to ISO179 standard is preferably 25 kJ / m 2 The upper limit of the unnotched Charpy impact strength is not particularly limited, but is, for example, 50 kJ / m 2 Below, and further less than 40kJ / m 2 , especially 39kJ / m2 the following.

[0179] The above-mentioned specific gravity, flexural strength, flexural elastic modulus, notched Charpy impact strength and unnotched Charpy impact strength are measured according to the methods described in the Examples described later.

[0180] The manufacturing method of the resin molded product in the present invention is not particularly limited, and any molding method commonly used for the resin composition can be used. As examples thereof, there can be cited: injection molding, ultra-high-speed injection molding, injection compression molding, two-color molding, hollow molding such as gas-assisted molding, molding using a heat-insulating mold, molding using a rapid heating mold, foam molding (also including supercritical fluid), insert molding, IMC (in-mold coating molding), extrusion molding, sheet molding, thermoforming, rotational molding, stacking molding, compression molding, blow molding, etc. In addition, a molding method using a hot runner method can also be used.

[0181] The resin molded article obtained by molding the resin composition of the present invention is preferably used as a plated resin molded article having a plated layer on the surface of the resin molded article. The plated layer in the resin molded article of the present invention is preferably in a form that maintains the performance as an antenna.

[0182] <Method for producing plated resin molded article>

[0183] Next, a method for producing a plated resin molded article is disclosed, the method comprising irradiating a surface of a resin molded article formed from the resin composition of the present invention with laser light and then forming a plated layer using a metal.

[0184] Figure 1 1 is a schematic diagram showing a process of forming a plating layer on the surface of a resin molded product 1 by laser direct structuring technology. Figure 1 In the embodiment, the resin molded product 1 is a flat substrate, but it is not necessarily a flat substrate, and may be a resin molded product with a curved surface formed partially or entirely. In addition, the obtained resin molded product with a plated layer is not limited to a final product, and also includes various parts.

[0185] Return to Figure 1 , irradiate the resin molded product 1 with a laser 2. The laser here is not particularly limited, and can be appropriately selected from known lasers such as YAG laser, excimer laser, electromagnetic ray, etc., preferably YGA laser. In addition, the wavelength of the laser is not particularly limited, and the preferred wavelength range is 200nm to 1200nm, and more preferably 800 to 1200nm.

[0186] When the laser is irradiated, only the portion 3 of the resin molded product 1 irradiated with the laser is activated. In this activated state, the plating solution 4 is applied to the resin molded product 1. The plating solution 4 is not particularly limited, and a wide range of known plating solutions can be used. Preferably, it is a plating solution containing at least one of copper, nickel, silver, gold and palladium as a metal component (especially a plating solution for chemical plating), more preferably a plating solution containing at least one of copper, nickel, silver and gold (especially a plating solution for chemical plating), and further preferably a plating solution containing copper (especially a plating solution for chemical plating). That is, the metal component of the plated layer in the present invention preferably contains at least one of the above-mentioned metals.

[0187] The method of applying the plating solution 4 to the resin molded article 1 is not particularly limited, and for example, a method of placing the resin molded article in a liquid containing the plating solution can be mentioned. The resin molded article after the plating solution is applied forms a plating layer 5 only on the portion irradiated with the laser.

[0188] In the method of the present invention, a plating layer (circuit) having a width of less than 1 mm and further having a width of less than 150 μm (the lower limit is not particularly limited, for example, 30 μm or more) can be formed. In order to suppress corrosion and degradation of the formed plating layer (circuit), for example, the plating layer can be further protected with nickel or gold after chemical plating. In addition, by using electroplating after chemical plating, the required film thickness can also be formed in a short time.

[0189] Furthermore, the method for producing a plated resin molded article is preferably used as a method for producing a portable electronic device component having an antenna, which method includes the method for producing a plated resin molded article.

[0190] The resin molded article obtained from the resin composition of the present invention can be used for various applications such as electronic parts (particularly parts of portable electronic devices) such as connectors, switches, relays, and conductive circuits.

[0191] In addition, the descriptions of Japanese Patent Application Laid-Open Nos. 2011-219620, 2011-195820, 2011-178873, 2011-168705, and 2011-148267 may be referred to without departing from the gist of the present invention.

[0192] Example

[0193] Below, enumerate embodiment and the present invention is described more specifically.As long as do not depart from the gist of the present invention, the material, dosage, ratio, processing content, processing step etc. shown in the following examples can be appropriately changed.Therefore, the scope of the present invention is not limited to the specific examples shown below.

[0194] Polyamide resin: PXD10 obtained according to the synthesis method described below was used.

[0195] <Synthesis Example of Crystalline Thermoplastic Resin (PXD10)>

[0196] In a reaction vessel with an internal volume of 50 liters equipped with a stirrer, a partial condenser, a condenser, a thermometer, a dropping device, a nitrogen inlet pipe, and a strand die, 8950 g (44.25 mol) of sebacic acid (manufactured by Ito Oil Manufacturing Co., Ltd., product name Sebacic acid TA), 12.54 g (0.074 mol) of calcium hypophosphite, and 6.45 g (0.079 mol) of sodium acetate were weighed and accurately weighed. After the reaction vessel was fully purged with nitrogen, it was pressurized to 0.4 MPa with nitrogen, and the temperature was raised from 20°C to 190°C while stirring, and the sebacic acid was uniformly melted in 55 minutes. Then, 5960 g (43.76 mol) of p-phenylenediamine (manufactured by Mitsubishi Gas Chemical Co., Ltd.) was added dropwise under stirring for 110 minutes. During this period, the temperature in the reaction vessel was continuously raised to 293°C. In the dropping process, the pressure was controlled at 0.42 MPa, and the generated water was discharged to the outside of the system through the partial condenser and the condenser. The temperature of the partial condenser was controlled in the range of 145-147°C. After the dropwise addition of p-phenylenediamine was completed, the polycondensation reaction was continued for 20 minutes at a pressure of 0.42 MPa in the reaction vessel. During this period, the temperature in the reaction vessel was raised to 296°C. Then, the pressure in the reaction vessel was reduced from 0.42 MPa to 0.12 MPa in 30 minutes. During this period, the internal temperature rose to 298°C. Then, the pressure was reduced at a rate of 0.002 MPa / min, and it took 20 minutes to reduce the pressure to 0.08 MPa, and the amount of components with a molecular weight of less than 1,000 was adjusted. The temperature in the reaction vessel at the end of the decompression was 301°C. Then, the system was pressurized with nitrogen, and the polymer was drawn out from the wire drawing die head in a linear form at a temperature of 301°C in the reaction container and a resin temperature of 301°C, and then cooled with cooling water at 20°C and pelletized to obtain about 13 kg of polyamide resin. It should be noted that the cooling time in the cooling water was 5 seconds, and the wire drawing speed was set to 100 m / min. Hereinafter, it is referred to as "PXD10".

[0197] The saturated water absorption when immersed in water, measured by the method described later, was 3.0% by mass.

[0198] <Method for measuring saturated water absorption when polyamide resin is immersed in water>

[0199] A 100×100 mm and 2 mm thick plate-shaped test piece was immersed in 80°C hot water, and the plate mass was measured every 24 hours. At this time, the moisture on the plate surface was fully blown away by blowing air. The immersion was terminated when the mass change was saturated, and the mass change rate relative to the initial mass was calculated as the saturated water absorption rate.

[0200] [Mathematical formula 1]

[0201] (Saturated water absorption rate: %) = [(mass after saturated water absorption) - (initial mass)] / (initial mass) × 100

[0202] 5007: Polybutylene terephthalate resin (PBT): "Novaduran 5008-C" manufactured by Mitsubishi Engineering-Plastics Corporation

[0203] 5605: IPA-PBT (isophthalic acid copolymer) "Novaduran 5605" manufactured by Mitsubishi Engineering-Plastics Corporation

[0204] 1010X: Polyamide 6 (PA6), manufactured by Ube Industries, Ltd.

[0205] LDS Additives:

[0206] Black1G: Made by Shepherd Japan, copper chromium oxide (CuCr 2 O 4 )

[0207] CP-5C: Antimony-doped tin oxide, manufactured by Keeling & Walker

[0208] 23K: Aluminum-doped zinc oxide, manufactured by HakusuiTech, resistivity (product standard value) 100 to 500 Ω·cm

[0209] Reinforcement Fiber:

[0210] T-756H: manufactured by Nippon Electric Glass Co., Ltd., E glass, glass fiber, urethane sizing agent, cut length (number average fiber length) 3 mm, number average fiber diameter 10 μm, glass fiber cross section is circular.

[0211] T-127: manufactured by Nippon Electric Glass Co., Ltd., E glass, glass fiber, chopped strands, number average fiber diameter 13 μm, cut length (number average fiber length) 3 mm, glass fiber cross section is circular.

[0212] Glass sheet:

[0213] Fleca REFG 313: Made by Nippon Sheet Glass Co., Ltd. (5μm thick)

[0214] Fine Flake 6145: manufactured by Nippon Glass Co., Ltd. (0.7μm thick)

[0215] Release agent:

[0216] CS8CP: Made by Nitto Kasei Kogyo Co., Ltd., calcium montanate

[0217] PED522: Oxidized polyethylene wax, manufactured by Clariant Chemical

[0218] talc:

[0219] MW (Micron White) 5000S: manufactured by Hayashi Chemicals Co., Ltd., average diameter 4.7 μm

[0220] Examples 1 to 6, Comparative Examples 1 to 7

[0221] <Mixture>

[0222] Each component was weighed to a composition as shown in Table 1 below, and the components other than glass fiber and glass flake were mixed in a tumble mixer, and introduced from the end of a twin-screw extruder (TEM26SS manufactured by Toshiba Machine Co., Ltd.), and the glass fiber and glass flake were fed sideways after melting to produce pellets. The temperature of the twin-screw extruder was set to 300° C. In Example 6 and Comparative Example 7, the setting temperature of the twin-screw extruder was 260° C.

[0223] <Flexural strength and flexural modulus>

[0224] After drying the pellets obtained by the above-mentioned production method at 70°C for 3 hours, an ISO tensile test piece (4 mm thick) was injection molded using an injection molding machine (manufactured by Toshiba Machine Co., Ltd., "EC75SX") under the conditions of a cylinder temperature of 300°C, a mold temperature of 130°C, and a molding cycle of 50 seconds. In Example 6 and Comparative Example 7, the conditions were set to a cylinder temperature of 260°C, a mold temperature of 120°C, and a molding cycle of 50 seconds.

[0225] The flexural strength (unit: MPa) and flexural modulus (unit: GPa) were measured at a temperature of 23° C. using the above-mentioned ISO tensile test piece (4 mm thick) in accordance with ISO178.

[0226] <Charpy impact strength>

[0227] After drying the pellets obtained by the above-mentioned production method at 70°C for 3 hours, an ISO tensile test piece (4 mm thick) was injection molded using an injection molding machine (manufactured by Toshiba Machine Co., Ltd., "EC75SX") under the conditions of a cylinder temperature of 300°C, a mold temperature of 130°C, and a molding cycle of 50 seconds. In Example 6 and Comparative Example 7, the conditions were set to a cylinder temperature of 260°C, a mold temperature of 120°C, and a molding cycle of 50 seconds.

[0228] Charpy impact strength (with notch and without notch) was measured according to ISO179 standard.

[0229] <Warp evaluation>

[0230] After the pellets obtained by the above-mentioned manufacturing method were dried at 70°C for 3 hours, they were injection molded using an injection molding machine ("EC75SX" manufactured by Toshiba Machine Co., Ltd.) under the conditions of a barrel temperature of 300°C, a mold temperature of 130°C, and a molding cycle of 50 seconds to form a plate-shaped test piece with a thickness of 60mm×60mm×2mm. As a warpage evaluation, the warpage amount of the obtained molded product was measured. In addition, annealing treatment was performed under the following conditions, and the warpage amount of the obtained molded product was measured. Among them, in Example 6 and Comparative Example 7, the conditions of a barrel temperature of 260°C, a mold temperature of 120°C, and a molding cycle of 50 seconds were set to form a plate-shaped test piece with a thickness of 100mm×100mm×2mm.

[0231] As annealing conditions, the obtained test piece was heated for 90 seconds using a surface-type far-infrared heater set at 300° C. The surface temperature of the test piece was measured by thermal imaging, and the result showed that the highest reached temperature was 270° C. In Example 6 and Comparative Example 7, the obtained test piece was heated for 12 hours using a hot air oven set at 140° C.

[0232] The plate-shaped test piece was scanned using Keyence's 3D measuring instrument VR-3000, and the warpage was calculated based on the difference between the maximum and minimum heights detected.

[0233] The amount of change indicates the difference between the warpage after annealing and the warpage before annealing.

[0234] <Plating Appearance>

[0235] The pellets obtained by the above-mentioned production method were dried at 70°C for 3 hours, and then injection molded into a 3 mm thick plate using an injection molding machine (manufactured by Toshiba Machine Co., Ltd., "EC75SX") under the conditions of a cylinder temperature of 300°C, a mold temperature of 130°C, and a molding cycle of 50 seconds. In Example 6 and Comparative Example 7, the conditions were set to a cylinder temperature of 260°C, a mold temperature of 120°C, and a molding cycle of 50 seconds.

[0236] The obtained plate was irradiated with a YAG laser having a wavelength of 1064 nm at an output power of 10 W, a speed of 80 m / s, and a frequency of 3 μs. The test piece was degreased with sulfuric acid, treated with THP Alkaliacti and THP Alkaliacce manufactured by Kizai, and copper-plated with SEL Copper manufactured by Kizai. Evaluation was performed as follows.

[0237] A: The plated layer is attached.

[0238] B: No plating layer attached.

[0239]

[0240]

[0241] According to the above results, for the resin composition of the present invention, by mixing glass fibers and glass sheets of a given thickness as reinforcing fillers at a given ratio, a resin molded product with small warpage after heating is obtained (Examples 1 to 7). In addition, the mechanical strength is also excellent. In addition, when the LDS additive is added (Examples 3 to 6), a coating can be formed while keeping the warpage after heating at a low level and the mechanical strength at a high level.

[0242] In contrast, when no glass sheet was included, the warpage after heating was large (Comparative Example 1, Comparative Example 5, Comparative Example 7).

[0243] In addition, even if the glass fiber and the glass sheet are mixed at a given ratio, when the thickness of the glass sheet is outside the given range, the warping after heating is large (Comparative Example 2, Comparative Example 6). In addition, the mechanical strength is also very poor. In addition, even if the glass fiber and the glass sheet of a given thickness are mixed, when the ratio is outside the given range, the warping after heating is still large (Comparative Example 3). On the other hand, when the glass fiber is not mixed, the warping after heating is small, but the mechanical strength is poor (Comparative Example 4).

Claims

1. A thermoplastic resin composition, wherein: The reinforcing filler is contained in an amount of 10 to 100 parts by mass relative to 100 parts by mass of the crystalline thermoplastic resin. The crystalline thermoplastic resin is at least one selected from polyamide resin and polybutylene terephthalate resin. The reinforcing filler includes reinforcing fibers and glass flakes with a thickness of 0.1 to 1.8 μm. The mass ratio of the reinforcing fiber to the glass sheet, i.e., reinforcing fiber / glass sheet, is 0.1 to 1. The content of the reinforcing filler other than the reinforcing fibers and the glass flakes having a thickness of 0.1 to 1.8 μm is 5% by mass or less of the total amount of the reinforcing filler contained in the resin composition.

2. The thermoplastic resin composition according to claim 1, wherein The crystalline thermoplastic resin includes a polyamide resin.

3. The thermoplastic resin composition according to claim 1 or 2, wherein The crystalline thermoplastic resin comprises a polyamide resin, The content of the thermoplastic resin other than the polyamide resin is 5% by mass or less of the thermoplastic resin composition.

4. The thermoplastic resin composition according to claim 2, wherein The polyamide resin is a semi-aromatic polyamide resin.

5. The thermoplastic resin composition according to claim 2, wherein The polyamide resin is composed of structural units derived from diamine and structural units derived from dicarboxylic acid, wherein 50 mol % or more of the structural units derived from diamine are derived from xylylenediamine, and 50 mol % or more of the structural units derived from dicarboxylic acid are derived from α,ω-straight-chain aliphatic dicarboxylic acid having 4 to 20 carbon atoms.

6. The thermoplastic resin composition according to claim 5, wherein 50 mol% or more of the structural units derived from dicarboxylic acid are derived from sebacic acid.

7. The thermoplastic resin composition according to claim 5 or 6, wherein 50 mol % or more of the structural units derived from diamine are derived from p-xylylenediamine.

8. The thermoplastic resin composition according to claim 5, wherein At least 70 mol% of the structural units derived from dicarboxylic acid are derived from sebacic acid, 70 mol % or more of the structural units derived from diamine are derived from p-xylylenediamine.

9. The thermoplastic resin composition according to claim 2, wherein 90% by mass or more of the polyamide resin is a polyamide resin having a saturated water absorption rate of 4.0% by mass or less after immersion in water.

10. The thermoplastic resin composition according to claim 1, wherein The crystalline thermoplastic resin includes a polyamide resin and a polybutylene terephthalate resin.

11. The thermoplastic resin composition according to claim 10, wherein The polyamide resin comprises an aliphatic polyamide resin, The polybutylene terephthalate resin comprises: 70 to 30% by mass of a polybutylene terephthalate resin composed of a dicarboxylic acid component mainly composed of terephthalic acid or an ester derivative thereof and a diol component mainly composed of 1,4-butanediol; and Modified polybutylene terephthalate resin 30-70% by mass And the total does not exceed 100 mass%.

12. The thermoplastic resin composition according to claim 1 or 2, wherein The reinforcing fibers include glass fibers.

13. The thermoplastic resin composition according to claim 1 or 2, wherein: The present invention further comprises 0.1 to 20 parts by mass of talc based on 100 parts by mass of the crystalline thermoplastic resin.

14. The thermoplastic resin composition according to claim 1 or 2, which does not contain a flame retardant.

15. The thermoplastic resin composition according to claim 3, which does not contain a flame retardant. 16 . The resin composition according to claim 1 , which does not contain a laser direct structuring additive.

17. The thermoplastic resin composition according to claim 1 or 2, wherein: The crystalline thermoplastic resin includes a polybutylene terephthalate resin and / or a polyamide resin, and the polybutylene terephthalate resin and the polyamide resin account for 85% by mass or more of the resin components included in the resin composition.

18. A resin molded article formed from the thermoplastic resin composition according to any one of claims 1 to 17.

19. The resin molded article according to claim 18, which is a portable electronic device component.

Citation Information

Patent Citations

  • JP1973094982A

  • Hot water temperature setting device for hot water supply

    JP1989300155A

  • Polyamide resin composition and conductive shaft-like molding

    JP2011132550A

  • Manufacturing method of polyamide resin molded article

    JP2011148267A

  • Polycarbonate resin composition and molding

    JP2011168705A