Method for manufacturing phosphor panel, phosphor panel, image intensifier, and scanning electron microscope

By forming an organic film and a metal reflective film on the fluorescent body panel and covering the oxide film using the atomic layer deposition method, the metal reflective film peeling problem is solved, the stability and quality of the product are improved, and the life of the image intensifier is extended.

CN113454750BActive Publication Date: 2024-11-12HAMAMATSU PHOTONICS KK
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201980092544.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-02-20
Filing Date
2019-11-22
Publication Date
2024-11-12
Estimated Expiration
2039-11-22

AI Technical Summary

Technical Problem

The metal reflective film in the existing fluorescent body panels is prone to peel off, resulting in a decrease in product quality, especially in image enhancers, which may lead to a decrease in image quality and may cause deterioration of the photoelectric surface.

Method used

By forming an organic film on the phosphor layer, then forming a metal reflective film on the organic film, and removing the organic film by firing, then covering the surfaces of the metal reflective film and phosphor particles by atomic layer deposition method to form an oxide film. The strength of the metal reflective film and its clinging ability to the phosphor layer are enhanced, thereby suppressing the peeling of the metal reflective film.

Benefits of technology

It effectively suppresses the peeling of the metal reflective film, improves the operability and quality of the product, extends the life of the image intensifier, reduces gas adsorption and ion feedback phenomena, and improves the stability of the photoelectric surface.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113454750B_ABST
    Figure CN113454750B_ABST
Patent Text Reader

Abstract

The manufacturing method of the phosphor panel includes: a process of forming a phosphor layer having a plurality of phosphor particles on an exit window; a process of forming an organic film on the phosphor layer; a process of forming a metal reflective film on the organic film; a process of removing the organic film by firing; and a process of forming an oxide film that integrally covers the surface of the metal reflective film and the surface of the phosphor particles by atomic layer deposition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for manufacturing a phosphor panel, a phosphor panel, an image intensifier and a scanning electron microscope. Background Art

[0002] In the prior art, for example, in image intensifiers and scanning electron microscopes, phosphor panels are used as electron detection units for detecting photoelectrons. For example, Patent Document 1 discloses that a phosphor layer (fluorescent film) is formed of granular phosphors, and a metal reflection film (aluminum layer) is provided on the electron incident surface side of the phosphor layer to prevent charging of the phosphor layer. In addition, Patent Document 1 discloses a method in which a nitrocellulose film is formed on the phosphor layer, a metal reflection film is formed on the nitrocellulose film, and the nitrocellulose film is removed, thereby forming a metal reflection film on the phosphor layer.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Laid-Open No. 1-243345 Summary of the invention

[0006] The technical problem that the invention is intended to solve

[0007] In the above-mentioned method for forming the metal reflection film, since a nitrocellulose film is interposed between the phosphor layer and the metal reflection film, the metal reflection film is not formed directly on the phosphor layer. Therefore, it cannot be said that the metal reflection film is sufficiently closely attached to the phosphor layer and is in a state where it is relatively easy to peel off from the phosphor layer. In addition, the peeling of the metal reflection film may cause the quality of a product having a phosphor panel as an electronic detection unit to be degraded. For example, in an image intensifier, the peeling of the metal reflection film may cause the image quality to be degraded.

[0008] Therefore, an object of the present disclosure is to provide a method for manufacturing a phosphor panel, a phosphor panel, an image intensifier, and a scanning electron microscope capable of effectively suppressing the peeling of a metal reflection film.

[0009] Means for solving technical problems

[0010] A method for manufacturing a phosphor panel according to one aspect of the present invention includes: a process of forming a phosphor layer having a plurality of phosphor particles on a light-transmitting substrate; a process of forming an organic film on the phosphor layer; a process of forming a metal reflective film on the organic film; a process of removing the organic film by firing; and a process of forming an oxide film that integrally covers the surface of the metal reflective film and the surface of the phosphor particles by atomic layer deposition.

[0011] In the above-mentioned method for manufacturing a phosphor panel, a metal reflective film is formed on an organic film formed on a phosphor layer. As a result, it is possible to prevent metal molecules constituting the metal reflective film from being mixed into the phosphor layer, and the metal reflective film can be appropriately provided on the phosphor layer. In addition, after the organic film is removed by firing, an oxide film is formed by atomic layer deposition in a manner that integrally covers the surface of the metal reflective film and the surface of the phosphor particles. Since the surface of the metal reflective film is protected by the oxide film, the strength of the metal reflective film is improved. Furthermore, since the adhesion between the metal reflective film and the phosphor layer (phosphor particles) is improved via the oxide film, the metal reflective film is difficult to peel off from the phosphor layer. Therefore, according to the above-mentioned manufacturing method, a phosphor panel that effectively suppresses the peeling of the metal reflective film can be manufactured.

[0012] The organic film may be a nitrocellulose film. In this way, an organic film suitable for forming a metal reflective film can be appropriately formed.

[0013] The process of forming the metal reflective film can be performed by evaporation or sputtering. Thus, the metal reflective film can be appropriately formed on the organic film. In addition, by evaporation or sputtering, a metal reflective film with openings (pinholes) appropriately provided is formed. Thus, in the film formation of the oxide film based on the atomic layer deposition method, the gas used to form the oxide film can intrude into the phosphor layer through the opening of the metal reflective film. As a result, the oxide film can be appropriately formed.

[0014] The manufacturing method may further include a step of forming a second metal reflective film on the first metal reflective film as the metal reflective film on the phosphor layer after removing the organic film, and in the step of forming the oxide film, the oxide film may be formed in a manner covering the first metal reflective film, the second metal reflective film and the phosphor particles. In the manufacturing method, sometimes a portion of the metal reflective film (first metal reflective film) initially formed on the organic film is changed into a metal oxide film or damaged by the firing step. As a result, the function of the metal reflective film, such as preventing the phosphor layer from charging, may not be fully exerted by the first metal reflective film alone. On the other hand, according to the manufacturing method, the function of the metal reflective film can be ensured by the first metal reflective film and the second metal reflective film.

[0015] A phosphor panel according to one aspect of the present disclosure includes: a light-transmitting substrate; a phosphor layer disposed on the light-transmitting substrate and having a plurality of phosphor particles; a metal reflective film disposed on the phosphor layer; and an oxide film formed in a manner that integrally covers the surface of the metal reflective film and the surface of the phosphor particles.

[0016] In the above-mentioned phosphor panel, the oxide film is formed in a manner that integrally covers the surface of the metal reflective film and the surface of the phosphor particles. The surface of the metal reflective film is protected by the oxide film, so that the strength of the metal reflective film is improved. Furthermore, since the close contact between the metal reflective film and the phosphor layer (phosphor particles) is improved via the oxide film, the metal reflective film is difficult to peel off from the phosphor layer. Therefore, according to the above-mentioned phosphor panel, the peeling of the metal reflective film can be effectively suppressed.

[0017] The metal reflection film may be an aluminum film, whereby the metal reflection film can appropriately function as the above-mentioned metal reflection film.

[0018] The oxide film may be an aluminum oxide film, a titanium oxide film, a zinc oxide film, or a silicon oxide film. This can appropriately improve the strength of the metal reflection film and improve the adhesion between the metal reflection film and the phosphor layer.

[0019] The phosphor particles may be gadolinium oxysulfide. Thus, a phosphor layer of a phosphor panel used as an electron detection unit in an image intensifier or the like can be appropriately formed.

[0020] The phosphor layer may contain a binding material for binding a plurality of phosphor particles together, thereby fixing the phosphor particles to each other and stabilizing the structure of the phosphor layer.

[0021] The binding material may be potassium silicate. This allows the phosphor particles to be appropriately bound to each other.

[0022] The light-transmitting substrate may be an optical fiber plate formed by bundling a plurality of optical fibers, thereby enabling the fluorescence emitted by the fluorescent layer to be transmitted to the outside with high efficiency and low distortion.

[0023] An image intensifier according to one aspect of the present disclosure includes: a photoelectric surface that emits photoelectrons according to incident light; an electron multiplying section that multiplies the photoelectrons emitted from the photoelectric surface; and the above-mentioned phosphor panel, which is configured such that the phosphor layer receives the photoelectrons multiplied by the electron multiplying section and emits fluorescence corresponding to the photoelectrons.

[0024] A scanning electron microscope according to one aspect of the present invention comprises: an electron gun which generates an electron beam; an irradiation unit which irradiates the electron beam to a sample and scans the electron beam irradiation position on the sample; and the above-mentioned phosphor panel, which is configured such that the phosphor layer receives photoelectrons generated in the sample in response to the electron beam irradiation to the sample and emits fluorescence corresponding to the photoelectrons.

[0025] The image intensifier or the scanning electron microscope is provided with the phosphor panel as an electron detection unit. As described above, in the phosphor panel, the metal reflection film is more difficult to peel off than in the prior art, so the operability of the phosphor panel during product manufacturing can be improved. That is, the handling of the phosphor panel becomes easier than in the prior art. In addition, by suppressing the peeling of the metal reflection film in the phosphor panel, the quality reduction of the product caused by the peeling of the metal reflection film can be suppressed. For example, in the image intensifier, the reduction of the image quality caused by the peeling of the metal reflection film can be suppressed. In addition, by covering the phosphor particles with an oxide film, the adsorption of gas to the phosphor particles (or the binding material attached to the phosphor particles, the same below) is suppressed, and the release of gas from the phosphor particles during the operation of the image intensifier is suppressed. As a result, the phenomenon that the gas released from the phosphor particles is ionized and reaches the photoelectric surface (ion feedback) can be suppressed, and the degradation of the photoelectric surface (degradation of cathode sensitivity) caused by this phenomenon can be suppressed. As a result, the life characteristics (product life) of the image intensifier can be improved.

[0026] Effects of the Invention

[0027] According to the present invention, a method for manufacturing a phosphor panel, a phosphor panel, an image intensifier, and a scanning electron microscope capable of effectively suppressing peeling of a metal reflection film can be provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 is a partial cross-sectional view of an image intensifier including a phosphor panel according to one embodiment.

[0029] Figure 2 yes Figure 1 An enlarged cross-sectional view of the main parts of the image intensifier is shown.

[0030] Figure 3 It is a schematic cross-sectional view showing a main part of a phosphor panel.

[0031] Figure 4 The figure shows a SEM image of a phosphor panel.

[0032] Figure 5 The diagram shows the manufacturing process of the phosphor panel.

[0033] Figure 6 The diagram shows the manufacturing process of the phosphor panel.

[0034] Figure 7 It is a figure which shows the light irradiation conditions of a life test (MTTF test).

[0035] Figure 8 (A) shows the test results of the image intensifier of the comparative example, and (B) shows the test results of the image intensifier of the embodiment.

[0036] Fig. 9 This is a schematic structural diagram of a phosphor panel according to one embodiment, taken using a scanning electron microscope.

[0037] Reference numerals:

[0038] 1…image intensifier; 3…photoelectric surface; 4…microchannel plate (electron multiplying section); 5…fluorescent surface; 12…exit window (light-transmitting substrate); 30…fluorescent panel; 51…fluorescent particles; 52…fluorescent layer; 53…metal reflective film; 54…oxide film; 61…organic film; 62…metal reflective film (first metal reflective film); 63…metal reflective film (second metal reflective film); 70…scanning electron microscope; 71…electron gun; 72…irradiation section; B…electron beam; C…binding material; E, E1, E2…photoelectrons; L1…incident light; L2…fluorescence; S…sample. DETAILED DESCRIPTION

[0039] Hereinafter, the embodiments of the present disclosure will be described with reference to the accompanying drawings. In each figure, the same or equivalent parts are marked with the same figure mark, and repeated descriptions are omitted. In addition, in the accompanying drawings, some parts are exaggerated in order to easily explain the characteristic parts of the embodiments, and the dimensions are different from the actual ones. In addition, in the following description, the terms such as "upper" and "lower" are convenient descriptions based on the states shown in the drawings.

[0040] [Structure of image intensifier]

[0041] Figure 1 and Figure 2 1 shows an image intensifier including a phosphor panel according to one embodiment. The image intensifier 1 of this embodiment includes a housing 2. The image intensifier 1 includes a photocathode 3, a microchannel plate 4 (electron multiplying unit), and a phosphor surface 5 inside the housing 2.

[0042] The interior of the image intensifier 1 is maintained in a high vacuum state by hermetically sealing both ends of a housing 2 having a substantially hollow cylindrical shape with a substantially disk-shaped incident window 11 and an exit window 12 (translucent substrate). The housing 2 is composed of, for example, a substantially hollow cylindrical ceramic side tube 13, a substantially hollow cylindrical silicone rubber mold member 14 covering the side of the side tube 13, and a substantially hollow cylindrical polyoxymethylene shell member 15 covering the side and bottom of the mold member 14.

[0043] For example, two through holes are formed at both ends of the molded member 14. One end of the shell member 15 is in an open state, and a through hole is formed at the other end of the shell member 15 so that the through hole on one side of the molded member 14 is consistent with its periphery. On one end side of the molded member 14, a glass incident window 11 is joined to the surface around the through hole on one side of the molded member 14. A thin film-shaped photoelectric element 3 is provided in the approximate center of the vacuum side surface of the incident window 11. The incident window 11 is, for example, a plate-shaped member made of quartz glass or the like. The photoelectric element 3 is formed on the plate-shaped member. The photoelectric element 3 is formed, for example, of a compound of antimony and alkali, a semiconductor crystal having alkali molecules such as Cs adsorbed on the surface, or the like.

[0044] On the other hand, at the other end side of the molded member 14, the exit window 12 is fitted into the through hole on the other side of the molded member 14. A thin film-like fluorescent surface 5 is provided at the approximate center portion of the vacuum side surface of the exit window 12. The exit window 12 is, for example, a fiber optic plate (FOP) formed by bundling a plurality of optical fibers. Each optical fiber of the exit window 12 is in a state where the optical axis is orthogonal to the photoelectric surface 3 and the vacuum side end faces are aligned to be in the same plane. A fluorescent surface 5 is formed on the vacuum side surface of the exit window 12. The exit window 12 and the fluorescent surface 5 constitute a phosphor panel 30.

[0045] A substantially disk-shaped microchannel plate 4 is disposed between the photoelectric surface 3 and the fluorescent surface 5. The microchannel plate 4 is supported by the inner edges of the mounting members 21 and 22 fixed to the inner wall of the side tube 13, and is in a state of being opposed to the photoelectric surface 3 and the fluorescent surface 5 at a predetermined interval. The microchannel plate 4 functions as an electron multiplying unit that multiplies the photoelectrons emitted from the photoelectric surface 3. Specifically, the microchannel plate 4 multiplies the photoelectrons emitted from the photoelectric surface 3 and outputs the multiplied photoelectrons to the fluorescent surface 5.

[0046] In the peripheral area of ​​the vacuum side surface of the incident window 11, a metal wiring layer (not shown) is electrically connected to the photoelectric surface 3. When the wiring layer is connected to the photoelectric surface 3, the mounting member 23 clamped by the side tube 13 and the incident window 11 is extended and fixed in the mold member 14. In addition, in the peripheral area of ​​the vacuum side surface of the exit window 12, another metal wiring layer (not shown) is electrically connected to the fluorescent surface 5. When the wiring layer is connected to the fluorescent surface 5, the mounting member 24 clamped by the side tube 13 and the mold member 14 is extended and fixed in the mold member 14.

[0047] One end of the lead wires 25 to 28, for example, made of Kovar metal, is connected to the end of the mounting components 21 to 24, respectively. The other ends of the lead wires 25 to 28 airtightly penetrate the molded component 14 and the shell component 15 and protrude to the outside, and are electrically connected to an external voltage source (not shown). Thus, a predetermined voltage from the external voltage source is applied to the photoelectric surface 3, the microchannel plate 4, and the fluorescent surface 5. A potential difference of, for example, about 200V is set between the photoelectric surface 3 and the input surface 4a of the microchannel plate 4. A potential difference of, for example, 500V to 1200V can be variably set between the input surface 4a and the output surface 4b of the microchannel plate 4. A potential difference of, for example, about 6kV is set between the output surface 4b of the microchannel plate 4 and the fluorescent surface 5.

[0048] Next, the operation of the image intensifier 1 is described. When the incident light L1 enters the photoelectric surface 3 through the incident window 11, the photoelectric surface 3 emits a photoelectron E1 in response to the incident light L1. When the photoelectron E1 enters the input surface 4a of the microchannel plate 4, the microchannel plate 4 multiplies the photoelectron E1 and emits the multiplied photoelectron E2 toward the fluorescent surface 5. When the photoelectron E2 enters the fluorescent surface 5, the fluorescent surface 5 emits fluorescence L2 corresponding to the photoelectron E2. The fluorescence L2 (optical image) emitted from the fluorescent surface 5 passes through the exit window 12 and is obtained by an imaging unit such as a CCD camera.

[0049] [Structure of phosphor panel]

[0050] Next, refer to Figure 3 and Figure 4 , the structure of the fluorescent panel 30 is described. Figure 3 It is a schematic cross-sectional view showing a portion of the emission window 12 where the fluorescent surface 5 is provided. Figure 4 is a SEM image showing a cross section of a portion of the phosphor panel 30. Figure 3 As shown, the phosphor panel 30 has the above-mentioned exit window 12, a phosphor layer 52 having a plurality of phosphor particles 51, a metal reflection film 53, and an oxide film 54. The above-mentioned phosphor surface 5 is composed of the phosphor layer 52, the metal reflection film 53, and the oxide film 54 covering the phosphor layer 52 and the metal reflection film 53. The exit window 12 functions as a light-transmitting substrate that allows the fluorescence L2 to pass through.

[0051] The phosphor layer 52 is provided on the exit window 12 (the inner surface 12a which is the vacuum side surface of the exit window 12). The phosphor layer 52 is formed on the exit window 12, for example, by a manufacturing method (sedimentation method, etc.) described later. The thickness t1 of the phosphor layer 52 is, for example, about 4 μm to 8 μm. The phosphor layer 52 is constituted as an aggregate of a plurality of phosphor particles 51. The particle size of the phosphor particles 51 is, for example, about 1 μm to 4 μm. In addition, the center value of the particle size distribution of the phosphor particles 51 is about 2 μm. The phosphor particles 51 have the property of emitting fluorescence corresponding to the incident photoelectrons. The phosphor particles 51 are, for example, gadolinium oxysulfide (GOS). The phosphor layer 52 contains a binding material for binding (bonding) the plurality of phosphor particles 51 to each other. In the present embodiment, a binding material C composed of potassium silicate is attached to the surface of the phosphor particles 51. Via the binding material C, the adjacent phosphor particles 51 are bound to each other.

[0052] The metal reflection film 53 is provided on the phosphor layer 52 (on the side of the phosphor layer 52 opposite to the exit window 12 side). The metal reflection film 53 is a so-called metal back, which has a relatively high reflectivity for light passing through the microchannel plate 4, and has a relatively high transmittance for the photoelectrons E2 from the microchannel plate 4. The metal reflection film 53 is formed, for example, of an aluminum film. The thickness t2 of the metal reflection film 53 is, for example, about 50 nm to 120 nm. The metal reflection film 53 has the function of preventing the phosphor layer 52 from being charged, the function of reflecting the fluorescence from the phosphor particles 51 toward the exit window 12 side, and the like. The metal reflection film 53 is formed on the phosphor layer 52 by a process of removing the organic film after evaporating or sputtering a metal material (aluminum in this embodiment) on the organic film provided on the phosphor layer 52, and the details will be described later. The metal reflection film 53 formed in this way is dotted with openings 53a such as pinholes.

[0053] The oxide film 54 is formed so as to integrally cover the surface of the metal reflection film 53 and the surface of the phosphor particles 51. The oxide film 54 is preferably formed of a material having a relatively high electron transmittance so as not to hinder the incidence of electrons to the phosphor particles 51. From such a viewpoint, the oxide film 54 is preferably formed of an element having a relatively small atomic number.

[0054] The oxide film 54 is formed by performing film formation based on the atomic layer deposition method (ALD) on the formation body in which the exit window 12, the phosphor layer 52 and the metal reflective film 53 are formed into layers as described above. Film formation based on ALD is a technology based on the principle of gas adsorption. Therefore, by allowing the gas to invade the interior of the above-mentioned formation body from the gaps in the above-mentioned formation body (for example, the opening 53a of the above-mentioned metal reflective film 53, the gap between the phosphor layer 52 and the inner surface 12a of the exit window 12, the gap between the phosphor layer 52 and the inner surface 53c of the metal reflective film 53, etc.), film formation can also be performed inside the above-mentioned formation body. In addition, by ALD, a dense and gapless connected film can be formed even for fine concave and convex surfaces.

[0055] Therefore, if Figure 3 As shown, the oxide film 54 is formed not only on the outer surface of the above-mentioned formation (the outer surface 53b of the metal reflection film 53 and the outer surface 12b of the exit window 12), but also on the inside of the above-mentioned formation (the surface and inner surface 53c of the opening 53a of the metal reflection film 53, the inner surface 12a of the exit window 12, and the surface of the phosphor particle 51). In addition, the oxide film 54 is formed integrally (continuously) on the outer surface and the inside of the above-mentioned formation. In addition, the oxide film 54 covers the surface of the phosphor particle 51 in a manner that encloses the bonding material C attached to the surface of the phosphor particle 51. The thickness of the oxide film 54 is, for example, about 3nm to 12nm.

[0056] From the viewpoint of appropriately performing film formation based on ALD, the material of the oxide film 54 is preferably an oxide such as Be, Mg, Al, Si, Ca, Ti, Cr, Mn, Fe, Co, Ni, Cu, Zn, Ga, Ge, Sr, Y, Sn, Ba, Hf, Ta, W, Ir, etc. In addition, the oxide film 54 is preferably an aluminum oxide film (Al2O3), a titanium oxide film (TiO2), a zinc oxide film (ZnO), or a silicon oxide film (SiO2). With such a material, film formation based on ALD can be performed relatively easily, and a dense and continuous film can be appropriately formed. In the present embodiment, as an example, the oxide film 54 is an aluminum oxide film with a thickness of 5 nm formed by ALD.

[0057] [Method for manufacturing phosphor panel]

[0058] Next, refer to Figure 5 and Figure 6 , a method for manufacturing the phosphor panel 30 is described. Figure 5 and Figure 6Schematic diagram showing the manufacturing process of the phosphor panel 30. As a preparatory stage, a phosphor solution is prepared. First, a plurality of phosphor particles 51 are mixed with pure water and filtered potassium silicate. Then, the solution obtained in this way is stirred using ultrasonic waves. Thus, a solution in which a plurality of phosphor particles 51 are uniformly dispersed can be obtained. Then, the solution is further stirred on the basis of further adding barium acetate.

[0059] Next, for example, with respect to the mounting member 24 (metal flange, see Figure 1 , 2 ), a tube (not shown) is fixed. The tube is arranged in such a way that the inner surface 12a of the exit window 12 is located inside the tube. That is, the tube is fixed to the mounting member 24 in such a way that the portion where the fluorescent surface 5 is to be formed (i.e., the inner surface 12a of the exit window 12) is located inside the tube. In addition, at this time, the exit window 12 and the mounting member 24 are connected via a frit glass 29 (see Figure 2 ) and fixed to each other.

[0060] Next, the phosphor solution prepared in the above preparation stage is placed in the tube fixed to the inner surface 12a as described above. The phosphor particles 51 contained in the phosphor solution placed in the tube settle to the inner surface 12a after being left for a certain period of time. After that, the supernatant in the tube and the water attached to the surface of the phosphor particles 51 are carefully sucked. Figure 5 As shown in FIG. 1A , a phosphor layer 52 including a plurality of phosphor particles 51 is formed on the inner surface 12 a of the emission window 12 .

[0061] Next, after the exit window 12 and the phosphor particles 51 are dried, the surface of each phosphor particle 51 is immersed in potassium silicate. As a result, the binding material C composed of potassium silicate is attached to the surface of the phosphor particles 51, and the phosphor particles 51 are firmly bonded to each other via the binding material C. Figure 5 As shown in (B), an organic film 61 is formed on the phosphor layer 52 (on the side opposite to the exit window 12 side). In this embodiment, the organic film 61 is a nitrocellulose film. The organic film 61 is provided on the phosphor layer 52 in a substantially flat shape. That is, the organic film 61 is not provided along the surface shape of the phosphor particles 51, but is provided above the plurality of phosphor particles 51 while maintaining a substantially flat shape.

[0062] Then, if Figure 5As shown in (C), a metal reflection film 62 (first metal reflection film) is formed on the organic film 61. In the present embodiment, as an example, the metal reflection film 62 is an aluminum film. The thickness of the metal reflection film 62 is, for example, about 10 nm to 20 nm. The metal reflection film 62 is provided on the organic film 61 by evaporation or sputtering. As described above, by providing the organic film 61 on the phosphor layer 52 in a substantially flat shape, the metal reflection film 62 can be formed in a substantially flat shape along the shape of the organic film 61.

[0063] Next, proceed as follows Figure 5 The formed body composed of the exit window 12, the phosphor layer 52, the organic film 61 and the metal reflective film 62 as shown in (C) is fired. The above-mentioned formed body is fired, for example, at 350°C in the atmosphere. By firing, the organic film 61 is burned and removed. As a result, Figure 6 As shown in (A) of FIG. 5 , the metal reflection film 62 is disposed on the phosphor layer 52. In addition, the metal reflection film 62 formed by the above-mentioned vapor deposition or sputtering has dotted openings 62a such as pinholes.

[0064] Then, if Figure 6 As shown in (B), after the organic film 61 is removed, a metal reflection film 63 (second metal reflection film) is formed on the metal reflection film 62 located on the phosphor layer 52. This is based on the following reasons. That is, there is a case where a part of the metal reflection film 62 is changed into a metal oxide film (aluminum oxide in this embodiment) or damaged due to the firing for removing the organic film 61. As a result, a metal reflection film (here, an aluminum film) with a sufficient layer thickness cannot be ensured, and the function as the above-mentioned metal pad cannot be fully exerted by the metal reflection film 62 alone. Therefore, in order to ensure a metal reflection film with a sufficient layer thickness, a metal reflection film 63 is formed on the metal reflection film 62. The above-mentioned metal reflection film 53 is composed of the metal reflection film 62 and the metal reflection film 63 formed in this way.

[0065] The metal reflection film 63 may be formed of the same material as the metal reflection film 62, or may be formed of a metal material different from the metal reflection film 62. In the present embodiment, as an example, the metal reflection film 63 is formed of aluminum, which is the same as the metal reflection film 62. The metal reflection film 63 is formed on the metal reflection film 62 by evaporation or sputtering. The thickness of the metal reflection film 63 is, for example, about 40 nm to 100 nm. An opening 63a connected to the opening 62a is formed in the metal reflection film 63 at a portion corresponding to the opening 62a of the metal reflection film 62. The opening 53a of the above-mentioned metal reflection film 53 is composed of the opening 62a and the opening 63a.

[0066] Next, an oxide film 54 (see FIG. 1 ) is formed by atomic layer deposition (ALD) to integrally cover the surface of the metal reflection film 53 (the metal reflection film 62 and the metal reflection film 63) and the surface of the phosphor particles 51. Figure 3 ). In this embodiment, Figure 6 The entire structure (the exit window 12, the phosphor layer 52, and the metal reflection film 53) in the state shown in (B) is subjected to film formation based on ALD. As a result, Figure 3 As shown, the oxide film 54 is formed on the outer surface of the above-mentioned formation (the outer surface 53b of the metal reflection film 53 and the outer surface 12b of the exit window 12) and the interior of the above-mentioned formation (the surface and inner surface 53c of the opening 53a of the metal reflection film 53, the inner surface 12a of the exit window 12, and the surface of the phosphor particles 51).

[0067] It should be noted that when the surface of the metal reflection film 62 is changed into a metal oxide film during the firing process, the metal reflection film 53 and the oxide film 54 after the above-mentioned ALD film formation can have the following structure: a metal oxide film produced by firing is formed on the outside of the aluminum film, and an oxide film 54 formed by ALD is further formed on the outside of the metal oxide film.

[0068] [Effects of phosphor panel]

[0069] In the phosphor panel 30 described above, the oxide film 54 is formed so as to integrally cover the surface of the metal reflection film 53 (the outer surface 53b and the inner surface 53c) and the surface of the phosphor particles 51. Since the surface of the metal reflection film 53 is protected by the oxide film 54, the strength of the metal reflection film 53 is improved. Furthermore, the adhesion between the metal reflection film 53 and the phosphor layer 52 (phosphor particles 51) is improved via the oxide film 54, so that the metal reflection film 53 is difficult to be peeled off from the phosphor layer 52. Therefore, according to the phosphor panel 30, the peeling of the metal reflection film 53 can be effectively suppressed.

[0070] In the present embodiment, the metal reflection film 53 is an aluminum film, so that the metal reflection film 53 can appropriately function as the metal spacer (ie, the function of preventing the phosphor layer 52 from being charged up, the function of reflecting the fluorescence L2 from the phosphor particles 51, etc.).

[0071] In addition, in the present embodiment, the oxide film 54 is formed of an aluminum oxide film. This can appropriately improve the strength of the metal reflection film 53 and improve the adhesion between the metal reflection film 53 and the phosphor layer 52. In addition, when the oxide film 54 is formed of a titanium oxide film, a zinc oxide film, or a silicon oxide film, the same effect as described above is achieved.

[0072] In the present embodiment, the phosphor particles 51 are gadolinium oxysulfide. This allows the phosphor layer 52 of the phosphor panel 30 used as an electron detection unit in an image intensifier or the like to be appropriately formed.

[0073] Furthermore, the phosphor layer 52 contains a bonding material C that bonds the plurality of phosphor particles 51 to each other. This fixes the phosphor particles 51 to each other, and stabilizes the structure of the phosphor layer 52 .

[0074] In the present embodiment, the bonding material C is potassium silicate. This allows the phosphor particles 51 to be appropriately bonded to each other.

[0075] In the present embodiment, the emission window 12 is a fiber optic plate (FOP) formed by bundling a plurality of optical fibers, thereby enabling the fluorescence L2 emitted from the fluorescent layer 52 to be transmitted to the outside with high efficiency and low distortion.

[0076] [Effects of image intensifier]

[0077] In addition, the image intensifier 1 includes a photoelectric surface 3 that emits photoelectrons E1 according to incident light L1, a microchannel plate 4 that multiplies the photoelectrons E1 emitted from the photoelectric surface 3, and a phosphor panel 30. The phosphor panel 30 is configured such that the phosphor layer 52 receives the photoelectrons E2 multiplied by the microchannel plate 4 and emits fluorescence L2 corresponding to the photoelectrons E2. Figure 2 As shown, the fluorescent surface 5 is arranged to face the microchannel plate 4. In the image intensifier 1, the metal reflection film 53 of the fluorescent panel 30 is more difficult to peel off than in the prior art, so the handling property of the fluorescent panel 30 during product manufacturing can be improved. That is, the handling of the fluorescent panel 30 becomes easier than in the prior art.

[0078] Furthermore, by suppressing the peeling of the metal reflection film 53 in the phosphor panel 30, it is possible to suppress the degradation of the quality of the image intensifier 1 caused by the peeling of the metal reflection film 53. Specifically, it is known that in an image intensifier, the peeling of the metal reflection film (metal backing) may cause the degradation of the image quality obtained by the image intensifier. Therefore, according to the above-mentioned image intensifier 1, it is possible to suppress the degradation of the image quality caused by the peeling of the metal reflection film 53.

[0079] Furthermore, since the phosphor particles 51 are covered with the oxide film 54, the adsorption of gas to the phosphor particles 51 (or the binding material C attached to the phosphor particles 51, the same below) can be suppressed, and the release of gas from the phosphor particles 51 during the operation of the image intensifier 1 can be suppressed. As a result, the phenomenon that the gas released from the phosphor particles 51 is ionized and reaches the photoelectric surface 3 (ion feedback) can be suppressed, and the degradation of the photoelectric surface 3 (degradation of cathode sensitivity) caused by this phenomenon can be suppressed. As a result, the life characteristics (product life) of the image intensifier 1 can be improved. In particular, potassium silicate used as the binding material C has the property of being relatively easy to adsorb gas. Therefore, when potassium silicate is used as the binding material C as in the present embodiment, it can be said that the above-mentioned effect brought about by the covering of the phosphor particles 51 by the oxide film 54 is particularly large.

[0080] Reference Figure 7 and Figure 8 , the effect of improving the life characteristics in the image intensifier 1 is described in detail. Figure 7 It is a figure which shows the light irradiation conditions of a life test (MTTF test). Figure 8 (A) shows the test results of the image intensifier of the comparative example (hereinafter referred to as the "comparative example"). Figure 8 (B) shows the test results of the image intensifier of the embodiment (hereinafter referred to as "the embodiment"). Here, the embodiment is an image intensifier having the same structure as the above-mentioned image intensifier 1. Specifically, the embodiment has the above-mentioned phosphor panel 30 as the phosphor panel. On the other hand, the comparative example is an image intensifier having a phosphor panel in which the film formation of the above-mentioned oxide film 54 by ALD is omitted.

[0081] More specifically, the embodiment is an image intensifier obtained as follows. That is, in the manufacturing process of the embodiment, the state before film formation by the above-mentioned ALD (that is, Figure 6 The phosphor panel (in the state shown in (B)) was subjected to a baking treatment at 350°C for 8 hours in a vacuum. Then, the oxide film 54 was formed on the phosphor panel based on the above-mentioned ALD. Then, the phosphor panel 30 obtained in this way was sealed in the housing 2 together with the photoelectric element 3 and the microchannel plate 4, thereby obtaining the embodiment. On the other hand, in the manufacturing process of the comparative example, Figure 6 The phosphor panel in the state shown in (B) was subjected to a baking treatment at 350° C. for 20 hours in a vacuum. Then, the phosphor panel immediately after the baking treatment was sealed in a housing together with the photoconductor and the microchannel plate, thereby obtaining a comparative example.

[0082] In the life test, for each of the incident windows 11 of the above-mentioned embodiments and comparative examples, Figure 7The light irradiation is repeated under the light irradiation conditions shown. Figure 7 As shown, light whose light intensity varied regularly within a range of 0.00054 lux to 54 lux was intermittently irradiated to each of the example and the comparative example for 12 minutes.

[0083] As a result, we get Figure 8 The test results shown. Figure 8 In the figure, Sk is the radiation sensitivity of the photoelectric surface (cathode sensitivity), MCP gain is the gain of the microchannel plate, and LG (luminescence gain) is an indicator corresponding to the amount of fluorescence emitted from the phosphor (phosphor layer). LG is a value obtained by the product of Sk, MCP gain and luminance efficiency. Figure 8 The horizontal axis represents the elapsed time from the start time of light irradiation. Figure 8 The vertical axis represents the state based on the state at the beginning of the test (100%). Figure 8 As shown in (A), in the comparative example, Sk and LG decreased to about 10% at the time of about 300 hours from the start of the life test (light irradiation). Figure 8 As shown in (B), in the embodiment, even after 1000 hours from the start of the life test, Sk and LG also maintain a state of more than 40%. That is, in the comparative example, LG decreases due to the decrease in Sk. On the other hand, in the embodiment, since the degradation rate of Sk is slower than that of the comparative example, LG can maintain a relatively high state even after a long time. Based on the above, it can be considered that in the embodiment, the above-mentioned oxide film 54 is formed in a manner of enclosing the phosphor particles 51 and the binding material C, thereby suppressing the gas release from the phosphor particles 51 and the binding material C. As a result, it can be considered that in the embodiment, the above-mentioned ion feedback is suppressed and the degradation of Sk is suppressed.

[0084] [Effects of the method for manufacturing phosphor panel]

[0085] The method for manufacturing the phosphor panel 30 of the present embodiment includes the steps of forming a phosphor layer 52 having a plurality of phosphor particles 51 on the emission window 12 (see Figure 5 (A)); a step of forming an organic film 61 on the phosphor layer 52 (refer to Figure 5 (B)); forming a metal reflection film 62 (a portion of the metal reflection film 53) on the organic film 61 (refer to Figure 5 (C)); the process of removing the organic film 61 by firing (refer to Figure 6 and forming an oxide film 54 integrally covering the surface of the metal reflection film 53 and the surface of the phosphor particles 51 by ALD (refer to Figure 3 ).

[0086] In the above-mentioned manufacturing method, the metal reflection film 62 is formed on the organic film 61 formed on the phosphor layer 52. As a result, it is possible to prevent the metal molecules constituting the metal reflection film 62 from being mixed into the phosphor layer 52, and the metal reflection film 53 can be appropriately provided on the phosphor layer 52. In addition, after the organic film 61 is removed by firing, the oxide film 54 is formed by ALD in a manner that integrally covers the surface of the metal reflection film 53 and the surface of the phosphor particles 51. As a result, as described above, the strength of the metal reflection film 53 is improved. Furthermore, the adhesion between the metal reflection film 53 and the phosphor layer 52 (phosphor particles 51) is improved via the oxide film 54, so that the metal reflection film 53 is difficult to peel off from the phosphor layer 52. Therefore, according to the above-mentioned manufacturing method, the phosphor panel 30 in which the peeling of the metal reflection film 53 is effectively suppressed can be manufactured.

[0087] In addition, if the above-mentioned effect is to be supplemented, it is known that a covering layer such as aluminum oxide is provided to continuously cover the surface of a plurality of phosphor particles, for example, as described in Japanese Patent Application Laid-Open No. 2013-216800. However, it should be noted that the above-mentioned effect of the present embodiment cannot be obtained simply by continuously covering the surface of a plurality of phosphor particles. That is, in the above-mentioned manufacturing method, in a state where the metal reflection film 53 is formed on the phosphor layer 52, the oxide film 54 is continuously formed across the metal reflection film 53 and the phosphor layer 52 by performing film formation based on ALD. As a result, the adhesion between the above-mentioned metal reflection film 53 and the phosphor layer 52 can be improved, and damage such as peeling of the metal reflection film 53 can be effectively suppressed.

[0088] In addition, the organic film 61 is a nitrocellulose film. Thus, the organic film 61 suitable for forming the metal reflection film 53 can be appropriately formed. In addition, the process of forming the metal reflection film 53 is performed by evaporation or sputtering. Thus, the metal reflection film 53 can be appropriately formed on the organic film 61. In addition, by evaporation or sputtering, a metal reflection film 53 with openings 53a (pinholes) appropriately provided is formed. Thus, in the film formation of the oxide film 54 based on ALD, the gas used to form the oxide film 54 can be appropriately intruded into the phosphor layer 52 through the openings 53a of the metal reflection film 53. As a result, the oxide film 54 can be appropriately formed.

[0089] The manufacturing method further includes a step of forming a metal reflection film 63 on the metal reflection film 62 as the metal reflection film on the phosphor layer 52 after removing the organic film 61 (see Figure 6(B)). In addition, in the process of forming the oxide film 54, the oxide film 54 is formed in a manner that covers the metal reflective film 53 (i.e., the metal reflective film 62 and the metal reflective film 63) and the phosphor particles 51. In the above-mentioned manufacturing method, a portion of the metal reflective film 62 initially formed on the organic film 61 may sometimes be changed into a metal oxide film (aluminum oxide in this embodiment) or damaged due to the firing process. As a result, the function of the metal reflective film, such as preventing the phosphor layer 52 from charging up, may not be fully exerted only by the metal reflective film 62 initially formed on the organic film 61. On the other hand, according to the above-mentioned manufacturing method, the function as the above-mentioned metal reflective film can be ensured by the metal reflective film 62 and the metal reflective film 63.

[0090] In addition, the thickness of metal reflection film 62 (15 nm in this embodiment) is smaller than the thickness of metal reflection film 63 (70 nm in this embodiment). In this way, by forming metal reflection film 62 formed on organic film 61 before the firing step to be relatively thin, organic film 61 can be appropriately removed in the firing step. In addition, by forming relatively thick metal reflection film 62 after removing organic film 61, the thickness of the entire metal reflection film (thickness t2 of metal reflection film 53) can be sufficiently ensured.

[0091] [Structure of a scanning electron microscope]

[0092] The phosphor panel 30 described above can be used in various optical devices in addition to the image intensifier. For example, the phosphor panel 30 can also be used as an electron detection unit in a scanning electron microscope. Fig. 9 1 is a schematic diagram of the structure of a scanning electron microscope according to an embodiment. Fig. 9 As shown in FIG. 1 , the scanning electron microscope 70 of the present embodiment includes: an electron gun 71 for generating an electron beam; an irradiation unit 72 for irradiating an electron beam B to a sample S and scanning the electron beam irradiation position on the sample S; and a phosphor panel 30. The phosphor panel 30 is configured such that the phosphor layer 52 receives photoelectrons E generated in the sample S in response to the electron beam irradiation to the sample S, and emits fluorescence in response to the photoelectrons E. That is, as shown in FIG. Fig. 9As shown, the fluorescent surface 5 is arranged in a manner opposite to the sample S. In the scanning electron microscope 70, similarly to the above-mentioned image intensifier 1, the metal reflection film 53 of the fluorescent panel 30 is difficult to peel off compared with the conventional technology, so the handling of the fluorescent panel 30 during product manufacturing can be improved. That is, compared with the conventional technology, the handling of the fluorescent panel 30 becomes easier. In addition, the scanning electron microscope 70 is a so-called transmission type scanning electron microscope in which the incident surface of the electron beam B in the sample S and the exit surface of the photoelectron E are located on opposite sides to each other, but the fluorescent panel 30 can also be used as an electron detection unit of a so-called reflection type scanning electron microscope in which the incident surface of the electron beam in the sample and the exit surface of the photoelectron are the same.

[0093] An embodiment of the present invention has been described above, but the present invention is not limited to the above embodiment. For example, the material and shape of each structure are not limited to the above materials and shapes, and various materials and shapes can be used. For example, the exit window 12 may not be composed of FOP, but may be composed of a glass substrate.

[0094] In addition, mainly in the image intensifier, in order to improve the above-mentioned ion feedback suppression effect, the following film forming process may be additionally performed. That is, after the phosphor layer 52 is formed on the exit window 12 ( Figure 5 In the state shown in (A) of FIG. 5 ), an oxide film (e.g., aluminum oxide) is formed by ALD to integrally cover the surface of the phosphor layer 52 (i.e., the surface of each phosphor particle 51). Alternatively, an oxide film may be formed on the surface of each phosphor particle 51 in the previous stage of preparing the phosphor solution. That is, the phosphor solution may be prepared using phosphor particles 51 on which an oxide film has been pre-formed. According to the above process, the phosphor particles 51 can be covered with an oxide film as early as possible in the manufacturing process of the phosphor panel 30, so that the adsorption of gas to the phosphor particles 51 can be effectively suppressed. In addition, in the case of performing ALD-based film formation on the surface of the phosphor layer 52 as described above, that is, in the case of fixing the phosphor particles 51 to each other by the oxide film formed by the film formation, the binding material C (potassium silicate) in the above embodiment may also be omitted. That is, in Figure 5 In the state shown in (A), the step of immersing the surface of each phosphor particle 51 in potassium silicate may be omitted.

[0095] In the above embodiment, the metal reflection film 63 is formed on the metal reflection film 62 (see Figure 6 (B)), but when the metal reflection film 62 after removing the organic film 61 can fully function as the above-mentioned metal pad, the formation of the metal reflection film 63 can also be omitted. In this case, the metal reflection film 53 in the above-mentioned embodiment is composed of only the metal reflection film 62.

Claims

1. A method for manufacturing a phosphor panel, characterized in that: include: forming a phosphor layer having a plurality of phosphor particles on a light-transmitting substrate; forming an organic film on the phosphor layer; forming a metal reflective film on the organic film; A step of removing the organic film by firing; and A step of forming an oxide film that integrally covers the surface of the metal reflection film and the surface of the phosphor particles by atomic layer deposition.

2. The method for manufacturing a phosphor panel according to claim 1, wherein: The organic membrane is a nitrocellulose membrane.

3. The method for manufacturing a phosphor panel according to claim 1, wherein: The step of forming the metal reflection film is performed by vapor deposition or sputtering.

4. The method for manufacturing a phosphor panel according to claim 2, wherein: The step of forming the metal reflection film is performed by vapor deposition or sputtering.

5. The method for manufacturing a phosphor panel according to any one of claims 1 to 4, characterized in that: After removing the organic film, the method further includes forming a second metal reflection film on the first metal reflection film which is the metal reflection film located on the phosphor layer. In the step of forming the oxide film, the oxide film is formed so as to cover the first metal reflection film, the second metal reflection film, and the phosphor particles.

6. A phosphor panel, characterized in that: have: Light-transmitting substrate; A phosphor layer, which is disposed on the light-transmitting substrate and has a plurality of phosphor particles; a metal reflective film disposed on the phosphor layer; and An oxide film is formed so as to integrally cover the surface of the metal reflection film and the surface of the phosphor particles.

7. The phosphor panel according to claim 6, wherein: The metal reflective film is an aluminum film.

8. The phosphor panel according to claim 6, wherein: The oxide film is an aluminum oxide film, a titanium oxide film, a zinc oxide film, or a silicon oxide film.

9. The phosphor panel according to claim 7, wherein: The oxide film is an aluminum oxide film, a titanium oxide film, a zinc oxide film, or a silicon oxide film.

10. The phosphor panel according to claim 6, wherein: The phosphor particles are gadolinium oxysulfide.

11. The phosphor panel according to claim 7, wherein: The phosphor particles are gadolinium oxysulfide.

12. The phosphor panel according to claim 8, wherein: The phosphor particles are gadolinium oxysulfide.

13. The phosphor panel according to claim 9, wherein: The phosphor particles are gadolinium oxysulfide.

14. The phosphor panel according to claim 6, wherein: The phosphor layer contains a bonding material that bonds the plurality of phosphor particles to each other.

15. The phosphor panel according to claim 7, wherein: The phosphor layer contains a bonding material that bonds the plurality of phosphor particles to each other.

16. The phosphor panel according to claim 8, wherein: The phosphor layer contains a bonding material that bonds the plurality of phosphor particles to each other.

17. The phosphor panel according to claim 9, wherein: The phosphor layer contains a bonding material that bonds the plurality of phosphor particles to each other.

18. The phosphor panel according to claim 10, wherein: The phosphor layer contains a bonding material that bonds the plurality of phosphor particles to each other.

19. The phosphor panel according to claim 11, wherein: The phosphor layer contains a bonding material that bonds the plurality of phosphor particles to each other.

20. The phosphor panel according to claim 12, wherein: The phosphor layer contains a bonding material that bonds the plurality of phosphor particles to each other.

21. The phosphor panel according to claim 13, wherein: The phosphor layer contains a bonding material that bonds the plurality of phosphor particles to each other.

22. The phosphor panel according to any one of claims 14 to 21, wherein: The bonding material is potassium silicate.

23. The phosphor panel according to any one of claims 6 to 21, characterized in that: The light-transmitting substrate is an optical fiber board formed by bundling a plurality of optical fibers.

24. The phosphor panel according to claim 22, wherein: The light-transmitting substrate is an optical fiber board formed by bundling a plurality of optical fibers.

25. An image intensifier, characterized in that: have: A photoelectric surface that emits photoelectrons in response to incident light; an electron multiplying section that multiplies the photoelectrons emitted from the photoelectric element; and The phosphor panel according to any one of claims 6 to 24 is configured such that the phosphor layer receives the photoelectrons multiplied by the electron multiplying section and emits fluorescence corresponding to the photoelectrons.

26. A scanning electron microscope, characterized in that: include: an electron gun, which generates an electron beam; an irradiation unit that irradiates the electron beam to the sample and scans the electron beam irradiation position on the sample; as well as The phosphor panel according to any one of claims 6 to 24 is configured such that the phosphor layer receives photoelectrons generated in the sample in response to irradiation of the sample with an electron beam, thereby emitting fluorescence in response to the photoelectrons.