Hydrophilic hollow fiber membrane and preparation method and application thereof

By designing a hydrophilic hollow fiber membrane with a multi-layer structure, combined with membrane-making polymers and spinning processes, the problem of heat transfer and steam penetration in traditional membrane humidifiers being difficult to achieve at the same time has been solved, and the air tightness and transmission efficiency have been improved. Extends the service life of the fuel cell humidification system.

CN113522051BActive Publication Date: 2024-10-01NINGBO INST OF MATERIALS TECH & ENG CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110631904.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-06-07
Publication Date
2024-10-01
Estimated Expiration
2041-06-07

AI Technical Summary

Technical Problem

In membrane humidifiers, it is difficult for traditional hollow fiber membranes to achieve rapid heat transfer and rapid steam penetration at the same time, while preventing the leakage of lower-temperature gases, leading to structural design conflicts.

Method used

Design a hydrophilic hollow fiber membrane, including a dense layer, a transition layer and a macroporous layer from the membrane center to the membrane surface. The dense layer contains the first pores, the transition layer contains the second pores, and the macroporous layer contains the third pores. The average pore diameter of the second pores is larger than the first pores and smaller than the third pores, and the initial contact angle between the hollow fiber membrane and the water droplets is less than or equal to 65 degrees and can be quickly reduced to 0 degrees. Film-making polymers, hydrophilic polymers and The polymer-reinforced film casting solution was prepared through a phase inversion spinning process.

Benefits of technology

It achieves rapid transmission and exchange of heat and humidity, reduces transmission and exchange resistance, improves air tightness and anti-leakage performance, and extends the service life of the fuel cell humidification system.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113522051B_ABST
    Figure CN113522051B_ABST
Patent Text Reader

Abstract

The present invention relates to a hydrophilic hollow fiber membrane and a preparation method and application thereof. The hydrophilic hollow fiber membrane comprises a dense layer, a transition layer and a macroporous layer arranged in sequence from the center of the membrane to the surface of the membrane, the dense layer contains first pores, the transition layer contains second pores, the macroporous layer contains third pores, the average pore size of the second pores is greater than the average pore size of the first pores and smaller than the average pore size of the third pores, the initial contact angle between the hollow fiber membrane and water droplets is less than or equal to 65 degrees, and the contact angle is reduced to 0 degrees within 20 seconds. The hydrophilic hollow fiber membrane of the present invention can realize rapid heat transfer and rapid steam penetration, and has excellent air tightness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of membrane humidification, in particular to a hydrophilic hollow fiber membrane and a preparation method and application thereof. Background Art

[0002] In the application process of membrane humidifiers designed with hollow fiber membranes in the humidification field, dry, low-temperature gas flows through the inner cavity of the hollow fiber membrane, and high-temperature steam flows through the outer surface of the hollow fiber membrane. At this time, the steam needs to transfer heat to the low-temperature gas in the inner cavity of the hollow fiber membrane to achieve heating of the low-temperature gas. At the same time, the steam also needs to penetrate into the inner cavity through the pores of the hollow fiber membrane to achieve humidification of the dry gas. Therefore, when designing the hollow fiber membrane structure, it is necessary to consider both the rapid transfer of heat and the rapid penetration of steam, and at the same time prevent the leakage of the low-temperature gas in the inner cavity of the hollow fiber membrane.

[0003] However, in order to achieve rapid heat transfer and rapid steam penetration, traditional technologies need to improve the hydrophilicity of the hollow fiber membrane and make the membrane wall of the hollow fiber membrane very thin, often reaching 100 microns or less. In addition, the pores of the hollow fiber membrane need to be made as large as possible to reduce the transmission exchange resistance; however, to prevent the leakage of lower-temperature gases in the inner cavity of the hollow fiber membrane, the hollow fiber membrane needs to be sufficiently thick and dense, and the two are contradictory. Summary of the invention

[0004] Based on this, it is necessary to provide a hydrophilic hollow fiber membrane and a preparation method and application thereof to address the above problems; the hydrophilic hollow fiber membrane can achieve rapid heat transfer and rapid steam penetration, and at the same time has excellent air tightness.

[0005] A hydrophilic hollow fiber membrane comprises a dense layer, a transition layer and a macroporous layer arranged in sequence from the center of the membrane to the surface of the membrane, the dense layer contains first pores, the transition layer contains second pores, the macroporous layer contains third pores, the average pore size of the second pores is larger than the average pore size of the first pores and smaller than the average pore size of the third pores, the initial contact angle of the hollow fiber membrane with water droplets is less than or equal to 65 degrees, and the contact angle drops to 0 degrees within 20 seconds.

[0006] In one embodiment, the average pore size of the first pores is less than or equal to 20 nm;

[0007] And / or, the average pore diameter of the third pores is greater than or equal to 100 nm.

[0008] In one embodiment, the thickness of the dense layer is less than or equal to 3 μm, and the membrane wall thickness of the hydrophilic hollow fiber membrane is 90 μm-110 μm.

[0009] In one embodiment, the thickness of the transition layer is 4 to 8 times the thickness of the dense layer, the pore size of the second pores gradually increases from the center of the membrane to the surface of the membrane, and the transition layer is a continuous sponge pore structure.

[0010] In one embodiment, the material of the hydrophilic hollow fiber membrane includes a membrane-forming polymer, a hydrophilic polymer and a reinforcing polymer, the membrane-forming polymer includes at least one of polyethersulfone or polyphenylsulfone, the hydrophilic polymer includes polyvinylpyrrolidone, and the reinforcing polymer includes polyurethane resin.

[0011] The hydrophilic hollow fiber membrane of the present invention has a dense layer, a transition layer and a macroporous layer arranged in sequence from the center of the membrane to the surface of the membrane, and the average pore size of the first pores distributed in the dense layer is the smallest, and the average pore size of the third pores distributed in the macroporous layer is the largest, so that the hydrophilic hollow fiber membrane has excellent airflow sealing performance, and at the same time, the transmission and exchange resistance of the hydrophilic hollow fiber membrane to humidity and energy is minimized.

[0012] In addition, the hydrophilic hollow fiber membrane of the present invention not only has a low initial contact angle, but also can quickly achieve the infiltration of water droplets into the hydrophilic hollow fiber membrane, effectively improving the humidity exchange efficiency between the inner cavity and the outside of the hydrophilic hollow fiber membrane during the humidification process. Moreover, rapid infiltration can achieve condensation of water to close the pores of the hydrophilic hollow fiber membrane, further improving the anti-leakage performance of the hydrophilic hollow fiber membrane for gases other than steam.

[0013] A method for preparing the hydrophilic hollow fiber membrane as described above comprises the following steps:

[0014] Providing a casting solution, wherein the casting solution comprises a film-forming polymer, a hydrophilic polymer, a first hydrophilic organic solvent, a structure regulator and a reinforcing polymer;

[0015] The casting solution and the inner gel bath are extruded through a spinneret and enter the outer gel bath for phase inversion spinning to obtain a hydrophilic hollow fiber membrane.

[0016] In one embodiment, the mass fraction of the film-forming polymer in the casting solution is 17%-22%;

[0017] And / or, the mass fraction of the hydrophilic polymer in the casting solution is 6%-14%;

[0018] And / or, the mass fraction of the first hydrophilic organic solvent in the casting solution is 30%-40%;

[0019] And / or, the structure regulator comprises oligoethylene glycol, and the mass fraction of the structure regulator in the casting solution is 25%-40%;

[0020] And / or, the mass fraction of the reinforcing polymer in the casting solution is 0.5%-3%.

[0021] In one embodiment, in the step of extruding the casting liquid and the inner gel bath through a spinneret and entering into an outer gel bath for phase inversion spinning, the distance between the spinneret and the liquid surface of the outer gel bath is 8 cm-25 cm, the spinning speed of the phase inversion spinning is 5 m / min-15 m / min, and the humidity of the air between the spinneret and the liquid surface of the outer gel bath is 60%-100%.

[0022] In one embodiment, the inner gel bath comprises a second hydrophilic organic solvent and water, and the mass fraction of the second hydrophilic organic solvent in the inner gel bath is less than or equal to 5%.

[0023] The present invention, through the reasonable formulation of the casting liquid and the application of the phase conversion spinning process, enables the components such as the structure regulator in the casting liquid to synergistically regulate the phase conversion process, thereby obtaining a hydrophilic hollow fiber membrane with a low initial contact angle and capable of quickly achieving water droplet infiltration of the hydrophilic hollow fiber membrane. The method is simple and suitable for industrial production.

[0024] An application of the hydrophilic hollow fiber membrane as described above in a membrane humidification component.

[0025] The membrane humidification assembly of the present invention can realize rapid transmission and exchange of humidity and energy, has excellent gas leakage prevention performance, and when applied to fuel cells, can greatly increase the service life of the humidification system and the fuel cell stack. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 A scanning electron microscope photograph of the outer surface of the polyethersulfone hollow fiber membrane provided in Comparative Example 1;

[0027] Figure 2 A scanning electron microscope photograph of the inner surface of the polyethersulfone hollow fiber membrane provided in Comparative Example 1;

[0028] Figure 3 This is a scanning electron microscope photograph of a cross section of the macroporous layer of the polyethersulfone hollow fiber membrane provided in Comparative Example 1;

[0029] Figure 4 A scanning electron microscope photograph of a cross section of the transition layer of the polyethersulfone hollow fiber membrane provided in Comparative Example 1;

[0030] Figure 5 The contact angle test data of the polyethersulfone hollow fiber membrane and water droplets provided in Comparative Example 1 is shown;

[0031] Figure 6A scanning electron microscope photograph of the outer surface of the hydrophilic hollow fiber membrane provided in Example 1;

[0032] Figure 7 A scanning electron microscope photograph of the inner surface of the hydrophilic hollow fiber membrane provided in Example 1;

[0033] Figure 8 A scanning electron microscope photograph of a cross section of a macroporous layer of the hydrophilic hollow fiber membrane provided in Example 1;

[0034] Fig. 9 A scanning electron microscope photograph of a cross section of the transition layer of the hydrophilic hollow fiber membrane provided in Example 1;

[0035] Fig.10 This is a graph showing the contact angle test data between the hydrophilic hollow fiber membrane provided in Example 1 and a water droplet. DETAILED DESCRIPTION

[0036] The hydrophilic hollow fiber membrane provided by the present invention and its preparation method and application will be further described below.

[0037] The hydrophilic hollow fiber membrane provided by the present invention comprises a dense layer, a transition layer and a macroporous layer arranged in sequence from the center of the membrane to the surface of the membrane, the dense layer contains first pores, the transition layer contains second pores, the macroporous layer contains third pores, and the average pore size of the second pores is larger than the average pore size of the first pores and smaller than the average pore size of the third pores.

[0038] The hydrophilic hollow fiber membrane of the present invention has a dense layer, a transition layer and a macroporous layer arranged in sequence from the center of the membrane to the surface of the membrane, and the average pore size of the first pores distributed in the dense layer is the smallest, and the average pore size of the third pores distributed in the macroporous layer is the largest, so that the hydrophilic hollow fiber membrane has excellent airflow sealing performance, and at the same time, the transmission and exchange resistance of the hydrophilic hollow fiber membrane to humidity and energy is minimized.

[0039] The membrane wall thickness of the hydrophilic hollow fiber membrane is equal to the sum of the thickness of the dense layer, the thickness of the transition layer and the thickness of the macroporous layer. In order to improve the bearing capacity of the hydrophilic hollow fiber membrane, while reducing the humidity and energy exchange resistance of the hydrophilic hollow fiber membrane, and increasing the heat transfer rate and the steam permeation rate, in one embodiment, the membrane wall thickness of the hydrophilic hollow fiber membrane is 90μm-110μm, and more preferably 90μm-100μm.

[0040] The thickness of the dense layer in the hydrophilic hollow fiber membrane and the average pore size of the first pores affect the humidity and energy exchange resistance and gas leakage prevention performance of the hydrophilic hollow fiber membrane. In order to prevent the leakage of lower-temperature gas in the inner cavity of the hydrophilic hollow fiber membrane and minimize the transmission and exchange resistance of humidity and energy, in one embodiment, the thickness of the dense layer is less than or equal to 3μm, and more preferably 1μm-3μm, and the average pore size of the first pores is less than or equal to 20nm, and more preferably 10nm-20nm.

[0041] In one embodiment, the thickness of the transition layer is 4 to 8 times the thickness of the dense layer, and the transition layer has a continuous sponge pore structure, which does not include poor pore structures such as finger-like pores, bag-like pores, and honeycomb closed pores. Therefore, the hydrophilic hollow fiber membrane has excellent resistance to bursting pressure, tensile breaking strength, airflow sealing, and lower humidity and energy exchange resistance.

[0042] In one embodiment, the pore size of the second pores gradually increases from the center of the membrane to the surface of the membrane. Further, the pore size of the second pores increases gradually from the center of the membrane to the surface of the membrane, thereby strengthening the capillary transport capacity of water from the outer surface to the center of the membrane, and at the same time, the airflow sealing performance can be improved. There is no obvious transition zone between the transition layer and the macroporous layer. It can be understood that the pore size of the second pores close to the macroporous layer is close to that of the third pores.

[0043] In one embodiment, the thickness of the macroporous layer is equal to the membrane wall thickness of the hydrophilic hollow fiber membrane minus the sum of the thickness of the dense layer and the thickness of the transition layer. In order to improve the effects of heat transfer and steam permeation, and at the same time, improve the bearing capacity of the hydrophilic hollow fiber membrane, the thickness of the macroporous layer is 75μm-90μm.

[0044] In order to reduce the humidity transmission exchange resistance and improve the mechanical properties of the hydrophilic hollow fiber membrane, in one embodiment, the average pore size of the third pores is greater than or equal to 100 nm, and more preferably 100 nm-300 nm.

[0045] Specifically, the material of the hydrophilic hollow fiber membrane includes a membrane-forming polymer, a hydrophilic polymer, and a reinforcing polymer.

[0046] In one embodiment, the membrane-forming polymer comprises at least one of polyethersulfone or polyphenylsulfone.

[0047] The addition of hydrophilic polymers can reduce the initial contact angle between the hydrophilic hollow fiber membrane and water droplets and accelerate the permeation rate of steam, thereby effectively improving the humidity exchange efficiency of the hydrophilic hollow fiber membrane. In one embodiment, the hydrophilic polymer includes polyvinyl pyrrolidone. It can be understood that polyvinyl pyrrolidone is a commonly used hydrophilic modified material. The present invention does not limit the molecular weight of polyvinyl pyrrolidone. The hydrophilic polymer is preferably at least one of polyvinyl pyrrolidone K17, polyvinyl pyrrolidone K23, polyvinyl pyrrolidone K30, and polyvinyl pyrrolidone K60.

[0048] The initial contact angle between the hydrophilic hollow fiber membrane of the present invention and water droplets is less than or equal to 65 degrees, and the contact angle drops to 0 degrees within 20 seconds, so that the water droplets can quickly infiltrate the hydrophilic hollow fiber membrane, effectively improving the humidity exchange efficiency between the inner cavity and the outer side of the hydrophilic hollow fiber membrane during humidification. In addition, the rapid infiltration can realize water condensation to close the pores of the hydrophilic hollow fiber membrane, further preventing the leakage of lower temperature gas in the inner cavity of the hydrophilic hollow fiber membrane.

[0049] In one embodiment, the reinforcing polymer includes a polyurethane resin. It is understandable that, depending on the molecular weight of the polyurethane resin, it has a very wide variety of commercial products. The function of the polyurethane resin of the present invention is to enhance the mechanical tensile properties of the hydrophilic hollow fiber membrane. Considering the flexibility, material compatibility, membrane tube strength and other requirements of the hydrophilic hollow fiber membrane, the hardness range of the polyurethane resin is preferably 70A-85A.

[0050] The hydrophilic hollow fiber membrane of the invention has an inner cavity bursting pressure greater than 250 KPa, a breaking tensile force of 2.8 N-4.2 N, and a breaking elongation of 35%-65%.

[0051] The present invention also provides a method for preparing the hydrophilic hollow fiber membrane as described above, comprising the following steps:

[0052] S1, providing a casting solution, wherein the casting solution comprises a film-forming polymer, a hydrophilic polymer, a first hydrophilic organic solvent, a structure regulator and a reinforcing polymer;

[0053] S2, extruding the casting solution and the inner gel bath agent through a spinneret, and entering the outer gel bath agent for phase inversion spinning to obtain a hollow fiber membrane.

[0054] In one embodiment, the first hydrophilic organic solvent in step S1 includes at least one of dimethylacetamide, methyl pyrrolidone and dimethyl sulfoxide.

[0055] In order to improve the hydrophilicity of the hydrophilic hollow fiber membrane and avoid the degradation of the mechanical properties of the hydrophilic hollow fiber membrane, in one embodiment, the mass fraction of the hydrophilic polymer in the casting solution is 6%-14%. It should be noted that in step S2, a portion of the hydrophilic polymer will be dissolved in the inner gel bath and the outer gel bath.

[0056] The structure regulator can ensure that the transition layer has a continuous sponge pore structure. In one embodiment, the structure regulator includes oligoethylene glycol, specifically, the oligoethylene glycol includes at least one of diethylene glycol, triethylene glycol or tetraethylene glycol. In order to prevent the appearance of undesirable pore structures such as finger-like pores, bag-like pores, and honeycomb closed pores, and to avoid stratification of the casting solution, the mass fraction of the structure regulator in the casting solution is 25%-40%.

[0057] It should be noted that the structure modifier is dissolved in the inner gel bath and the outer gel bath in step S2.

[0058] In order to enhance the mechanical tensile properties of the hydrophilic hollow fiber membrane and avoid stratification of the casting solution, the mass fraction of the reinforcing polymer in the casting solution is 0.5%-3%.

[0059] The casting liquid is obtained by blending a membrane-forming polymer, a hydrophilic polymer, a first hydrophilic organic solvent, a structure regulator and a reinforcing polymer. Considering that when there are bubbles in the casting liquid, the residual bubbles will cause macroscopic pore defects in the hydrophilic hollow fiber membrane. In one embodiment, after the membrane-forming polymer, the hydrophilic polymer, the first hydrophilic organic solvent, the structure regulator and the reinforcing polymer are blended, a defoaming treatment such as vacuum degassing and / or static degassing is also performed.

[0060] In order to make the film-forming polymer, hydrophilic polymer, structure regulator, reinforcing polymer and the first hydrophilic organic solvent blended and dissolved better, the reinforcing polymer and the first hydrophilic organic solvent are blended first, and then the film-forming polymer is added after they are completely dissolved, and finally the hydrophilic polymer and the structure regulator are added in sequence.

[0061] In order to prepare the hydrophilic hollow fiber membrane of the present invention, while providing the casting solution as mentioned above, it is also necessary to cooperate with a specific phase inversion spinning process, and it is necessary to comprehensively control parameters such as the water entry time, air humidity, inner gel bath agent, and outer gel bath agent in the phase inversion spinning process.

[0062] In step S2, the casting liquid and the inner gel bath are squeezed out from the spinneret, wherein the casting liquid is squeezed out from the annular gap of the spinneret, and the inner gel bath is squeezed out from the center of the spinneret. Before entering the outer gel bath, the water vapor in the air between the spinneret and the liquid surface of the outer gel bath will accumulate and adsorb on the outer surface of the casting liquid, thereby achieving pre-phase separation of the outer surface. At the same time, the casting liquid achieves pre-phase separation of the inner surface under the action of the inner gel bath.

[0063] The time from extrusion to the time of entering the outer gel bath is the water entry time. In order to regulate the water entry time, in one embodiment, the distance between the liquid level of the spinneret and the outer gel bath is 8cm-25cm, more preferably 10cm-20cm, and the spinning speed of the phase inversion spinning is 5m / min-15m / min, more preferably 10m / min-15m / min. It should be noted that the distance between the liquid levels of the outer gel bath is the shortest distance between the liquid levels of the outer gel bath, and the water entry time is preferably 1 second-3 seconds. In one embodiment, the humidity of the air between the liquid level of the spinneret and the outer gel bath is 60%-100%, more preferably 70%-95%.

[0064] It should be noted that when the water entry time is shortened, the humidity of the air between the spinneret and the liquid surface of the external gel bath should be appropriately increased.

[0065] In one embodiment, the outer gel bath comprises water; and the inner gel bath comprises water and a second hydrophilic organic solvent.

[0066] In one embodiment, the second hydrophilic organic solvent includes at least one of dimethylacetamide, methyl pyrrolidone and dimethyl sulfoxide. Specifically, the mass fraction of the second hydrophilic organic solvent in the inner gel bath is less than or equal to 5%, and the greater the mass fraction of the second hydrophilic organic solvent in the inner gel bath, the greater the average pore size of the first pores.

[0067] In one embodiment, the temperature of the outer gel bath is 20°C-50°C, and the temperature of the inner gel bath is 20°C-40°C.

[0068] The present invention, through the reasonable formulation of the casting liquid and the application of the phase conversion spinning process, enables the components such as the structure regulator in the casting liquid to synergistically regulate the phase conversion process, thereby obtaining a hydrophilic hollow fiber membrane with a low initial contact angle and capable of quickly achieving water droplet infiltration of the hydrophilic hollow fiber membrane. The method is simple and suitable for industrial production.

[0069] The present invention also provides the use of the hydrophilic hollow fiber membrane as described above in a membrane humidification component.

[0070] In one embodiment, a plurality of hydrophilic hollow fiber membranes are first packaged into a membrane bundle; the membrane bundle is then glued into a hollow fiber membrane box to prepare a membrane humidification assembly; the membrane humidification assembly can be used as a fuel cell humidifier system.

[0071] In the actual operation of the fuel cell humidifier system, low-temperature dry gas with a humidity of no more than 30% generally flows in the inner cavity of the hollow fiber membrane; high-temperature humid gas with a humidity of more than 90% flows on the outside of the hollow fiber membrane. At this time, the high-temperature humid gas on the outside transfers heat to the low-temperature dry gas in the inner cavity to heat the low-temperature dry gas; at the same time, the high-temperature humid gas penetrates into the inner cavity to humidify the low-temperature dry gas.

[0072] It should be noted that the structural design of the fuel cell humidifier system needs to be integrated with the fuel cell stack design layout and performance design requirements. The present invention only provides suggestions for fluid transmission inside and outside the hollow fiber membrane, and does not limit the final structural design of the humidifier.

[0073] The membrane humidification assembly of the present invention can realize the rapid transmission and exchange of humidity and energy, and the water vapor transmission rate is greater than 0.35g / (cm 2 ·min·MPa), excellent gas leakage prevention performance, pressure drop rate of less than 1.6KPa / minute, when used in fuel cells, can greatly improve the service life of the humidification system and fuel cell stack.

[0074] The membrane humidification assembly is used in the fuel cell humidifier system, which can controllably humidify the anode hydrogen and cathode air in the fuel cell. The fuel cell stack has mechanical and physical stability, stable humidification efficacy, efficient heat energy recovery and excellent gas leakage prevention performance, which can greatly improve the service life of the humidification system and the fuel cell stack.

[0075] Hereinafter, the hydrophilic hollow fiber membrane and its preparation method and application will be further described through the following specific examples.

[0076] Comparative Example 1

[0077] In order to better demonstrate the technical features of the present invention, the hollow fiber membrane humidifier assembly of Cologne and the polyethersulfone hollow fiber membrane therein are used as comparative examples.

[0078] like Figure 1 As shown, the membrane wall thickness of the polyethersulfone hollow fiber membrane of Comparative Example 1 is about 100 microns, and large finger-like holes are evenly distributed in the middle of the membrane wall. The average length of the finger-like holes is 40 microns, occupying about 40% of the membrane wall area; Figure 2 As shown, there is an obvious dense layer near the inner surface of the polyethersulfone hollow fiber membrane of Comparative Example 1, and the average thickness of the layer is about 2 microns; Figure 3 As shown, there is an obvious macroporous layer near the outer surface of the polyethersulfone hollow fiber membrane of Comparative Example 1, and the average thickness of the layer is about 3 microns; Figure 4 As shown, in the transitional membrane wall region between the outer surface and the inner surface of the polyethersulfone hollow fiber membrane of Comparative Example 1, in addition to the finger-like pores, there are also obvious bag-like closed pores.

[0079] Through the tensile test, the average tensile breaking force of the polyethersulfone hollow fiber membrane of Comparative Example 1 is 2.75 N. Through the contact angle test, Figure 5 As shown in the figure, the initial water drop contact angle of the polyethersulfone hollow fiber membrane is 73.5 degrees, which can be reduced to 0 degrees within 41 seconds. Through the bursting test, the bursting pressure of the polyethersulfone hollow fiber membrane is 273KPa.

[0080] The hollow fiber membrane humidifier assembly was subjected to a pressure test. After the inflation pressure reached 250KPa, it was sealed and the pressure drop was 1.79KPa / minute. The hollow fiber membrane humidifier assembly was used in a fuel cell humidifier system. Dry air at 60°C and 30% humidity was introduced into the inner cavity of the hydrophilic hollow fiber membrane; steam at 90°C and 95% humidity was introduced into the outer side of the hydrophilic hollow fiber membrane; the results showed that the air temperature at the outlet of the inner cavity of the hydrophilic hollow fiber membrane was 69°C and the humidity was 65%.

[0081] Example 1

[0082] Based on the total weight of the casting solution, 1 wt% of polyurethane (Shore hardness 82A) was added to 39 wt% of dimethylacetamide, and stirred at 80°C for complete dissolution; the temperature was lowered to 50°C, and then 20 wt% of polyethersulfone was added, and stirring was continued for complete dissolution; 10 wt% of polyvinylpyrrolidone K30 was added, and stirring was continued for complete dissolution; 30 wt% of triethylene glycol was added, and stirring was continued for uniform blending; then vacuum degassing was carried out for 30 minutes, and the degassing was allowed to stand for 12 hours.

[0083] Prepare water at 25°C and water at 30°C as the inner gel bath and the outer gel bath respectively, adjust the liquid level distance between the spinneret and the outer gel bath to 15 cm, and the air humidity to 90%; extrude the inner gel bath and the casting solution through the spinning head at a speed of 10 m / min, enter the outer gel bath for phase inversion spinning, and obtain a hydrophilic hollow fiber membrane.

[0084] like Figure 6 As shown in FIG. , the membrane wall thickness of the hydrophilic hollow fiber membrane is about 100 microns. Figure 7 As shown, the thickness of the dense layer of the hydrophilic hollow fiber membrane is about 2.5 microns, the aperture of the second pores gradually increases from the center of the membrane to the surface of the membrane, and the thickness of the transition layer is 12 microns. Figure 8 As shown in FIG. 1 , in the macroporous layer of the hydrophilic hollow fiber membrane, the pore size of the third pore does not have an obvious gradient distribution. Fig. 9 As shown, the transition layer of the hydrophilic hollow fiber membrane has a continuous sponge pore structure, and no undesirable bag-like closed pores are found.

[0085] The average pore size of the first pores in the dense layer was 13.4 nm as measured by a liquid-liquid porosimeter. The average pore size of the third pores in the macroporous layer was 173 nm as measured by microscopic observation and counting analysis.

[0086] Through tensile testing, such as Fig.10 As shown, the average tensile breaking force of the hydrophilic hollow fiber membrane is 3.3 Newtons, and the average elongation at break is 47%. Through the contact angle test, the initial water drop contact angle of the hydrophilic hollow fiber membrane is 57 degrees, which can be reduced to 0 degrees within 10 seconds. Through the burst test, the burst pressure of the hydrophilic hollow fiber membrane is 311KPa.

[0087] After the hydrophilic hollow fiber membrane is further packaged into a membrane humidification assembly, the membrane humidification assembly is subjected to a pressure test. After the inflation pressure reaches 250KPa, it is sealed and the pressure drop is 1.13KPa / minute. The membrane humidification assembly is used in the fuel cell humidifier system. Dry air at 60°C and 30% humidity is introduced into the inner cavity of the hydrophilic hollow fiber membrane; steam at 90°C and 95% humidity is introduced into the outer side. The results show that the membrane humidification assembly has excellent humidification and heating effects on the air flowing through the inner cavity of the hydrophilic hollow fiber membrane. The air temperature at the outlet of the inner cavity of the hydrophilic hollow fiber membrane is measured to be 75°C and the humidity is 72%, which meets the operation requirements of the fuel cell stack.

[0088] Example 2

[0089] Based on the total weight of the casting solution, 3 wt% of polyurethane (Shore hardness 70A) was added to 34 wt% of dimethyl sulfoxide, and stirred at 70°C for complete dissolution; the temperature was lowered to 45°C, and then 17 wt% of polyphenylsulfone was added, and stirring was continued for complete dissolution; 6 wt% of polyvinylpyrrolidone K60 was added, and stirring was continued for complete dissolution; 40 wt% of diethylene glycol was added, and stirring was continued for uniform blending; then vacuum degassing was carried out for 60 minutes, and the degassing was allowed to stand for 15 hours.

[0090] Prepare a 1% dimethyl sulfoxide aqueous solution at 20°C as an inner gel bath agent, prepare tap water at 20°C as an outer gel bath agent, adjust the liquid surface distance between the spinneret and the outer gel bath agent to 10 cm; the air humidity is 70%; extrude the inner gel bath agent and the casting solution through the spinning head at a speed of 5 m / min, enter the outer gel bath agent for phase inversion spinning, and obtain a hydrophilic hollow fiber membrane.

[0091] After cross-sectional scanning electron microscopy analysis, the membrane wall thickness of the hydrophilic hollow fiber membrane is about 90 microns; the thickness of the dense layer of the hydrophilic hollow fiber membrane is about 2 microns, the thickness of the transition layer is 10 microns, the transition layer has a continuous sponge pore structure, no bad bag-like closed pores are found, and the pore size of the second pores gradually increases from the center of the membrane to the surface of the membrane; there is no obvious gradient distribution of the third pores of the macroporous layer.

[0092] The average pore size of the first pores in the dense layer was 15.2 nm as measured by a liquid-liquid porosimeter. The average pore size of the third pores in the macroporous layer was 207 nm as measured by microscopic observation and counting analysis.

[0093] Through the tensile test, the average tensile breaking force of the hydrophilic hollow fiber membrane is 3.1 Newtons, and the average elongation at break is 52%. Through the contact angle test, the initial water drop contact angle of the hydrophilic hollow fiber membrane is 63 degrees, which can be reduced to 0 degrees within 15 seconds. Through the burst test, the burst pressure of the hydrophilic hollow fiber membrane is 293KPa.

[0094] After the hydrophilic hollow fiber membrane was further packaged into a membrane humidification assembly, the membrane humidification assembly was subjected to a pressure test. After the inflation pressure reached 250KPa, it was sealed and the pressure drop was 1.31KPa / minute. The membrane humidification assembly was used in the fuel cell humidifier system. Dry air at 60°C and 30% humidity was introduced into the inner cavity of the hydrophilic hollow fiber membrane; steam at 90°C and 95% humidity was introduced into the outer side. The results showed that the membrane humidification assembly had excellent humidification and heating effects on the air flowing through the inner cavity. The air temperature at the outlet of the inner cavity of the hydrophilic hollow fiber membrane was measured to be 78°C and the humidity was 75%, which met the operation requirements of the fuel cell stack.

[0095] Example 3

[0096] Based on the total weight of the casting solution, 0.5 wt % of polyurethane (Shore hardness 85A) and 10 wt % of polyphenylsulfone were added to 40 wt % of methyl pyrrolidone, and stirred at 60° C. for complete dissolution; the temperature was lowered to 40° C., and then 12 wt % of polyethersulfone was added, and stirring was continued for complete dissolution; 8 wt % of polyvinylpyrrolidone K17 and 4 wt % of polyvinylpyrrolidone K60 were added, and stirring was continued for complete dissolution; 25.5 wt % of tetraethylene glycol was added, and stirring was continued for uniform blending; vacuum degassing was then performed for 40 minutes, and the degassing was allowed to stand for 20 hours.

[0097] Prepare a 2% by mass methyl pyrrolidone aqueous solution at 40°C as an inner gel bath agent, prepare tap water at 50°C as an outer gel bath agent, adjust the liquid surface distance between the spinneret and the outer gel bath agent to 20 cm; the air humidity is 95%; extrude the inner gel bath agent and the casting solution through the spinning head at a speed of 15 m / min, enter the outer gel bath agent for phase inversion spinning, and obtain a hydrophilic hollow fiber membrane.

[0098] After cross-sectional scanning electron microscopy analysis, the membrane wall thickness of the hydrophilic hollow fiber membrane is about 95 microns; the thickness of the dense layer of the hydrophilic hollow fiber membrane is about 2.3 microns, the thickness of the transition layer is 13.9 microns, the transition layer has a continuous sponge pore structure, and no undesirable bag-like closed pores are found. The pore size of the second pores gradually increases from the center of the membrane to the surface of the membrane; there is no obvious gradient distribution of the third pores of the macroporous layer.

[0099] The average pore size of the first pores in the dense layer was 17.9 nm as measured by a liquid-liquid porosimeter. The average pore size of the third pores in the macroporous layer was 147 nm as measured by microscopic observation and counting analysis.

[0100] Through the tensile test, the average tensile breaking force of the hydrophilic hollow fiber membrane is 3.7 Newtons, and the average elongation at break is 41%. Through the contact angle test, the initial water drop contact angle of the hydrophilic hollow fiber membrane is 55 degrees, which can be reduced to 0 degrees within 15 seconds. Through the burst test, the burst pressure of the hydrophilic hollow fiber membrane is 323KPa.

[0101] After the hydrophilic hollow fiber membrane was further packaged into a membrane humidification assembly, the membrane humidification assembly was subjected to a pressure test. After the inflation pressure reached 250KPa, it was sealed and the pressure drop was 1.42KPa / minute. The membrane humidification assembly was used in the fuel cell humidifier system. Dry air at 60°C and 30% humidity was introduced into the inner cavity of the hydrophilic hollow fiber membrane; steam at 90°C and 95% humidity was introduced into the outer side. The results showed that the membrane humidification assembly had excellent humidification and heating effects on the air flowing through the inner cavity. The air temperature at the outlet of the inner cavity of the hydrophilic hollow fiber membrane was measured to be 76°C and the humidity was 74%, which met the operation requirements of the fuel cell stack.

[0102] Example 4

[0103] Based on the total weight of the casting solution, 2 wt % of polyurethane (Shore hardness 75A) was added to a mixed solution of 20 wt % of dimethyl sulfoxide and 20 wt % of dimethylacetamide, and stirred at 55° C. for complete dissolution; the temperature was lowered to 30° C., and then 21 wt % of polyether sulfone was added, and stirring was continued for complete dissolution; 8 wt % of polyvinyl pyrrolidone K23 was added, and stirring was continued for complete dissolution; 20 wt % of diethylene glycol and 9 wt % of tetraethylene glycol were added, and stirring was continued for uniform blending; vacuum degassing was then performed for 60 minutes, and the degassing was allowed to stand for 15 hours.

[0104] Prepare deionized water at 20°C as an inner gel bath, prepare tap water at 30°C as an outer gel bath, adjust the liquid surface distance between the spinneret and the outer gel bath to 12 cm; the air humidity is 90%; extrude the inner gel bath and the casting solution through the spinning head at a speed of 10 m / min, enter the outer gel bath for phase inversion spinning, and obtain a hydrophilic hollow fiber membrane.

[0105] After cross-sectional scanning electron microscopy analysis, the membrane wall thickness of the hydrophilic hollow fiber membrane is about 90 microns; the thickness of the dense layer of the hydrophilic hollow fiber membrane is about 3 microns, the thickness of the transition layer is 12 microns, the transition layer has a continuous sponge pore structure, and no undesirable bag-like closed pores are found. The pore size of the second pores gradually increases from the center of the membrane to the surface of the membrane; there is no obvious gradient distribution of the third pores of the macroporous layer.

[0106] The average pore size of the first pores in the dense layer was 12.1 nm as measured by a liquid-liquid porosimeter. The average pore size of the third pores in the macroporous layer was 131 nm as measured by microscopic observation and counting analysis.

[0107] Through the tensile test, the average tensile breaking force of the hydrophilic hollow fiber membrane is 4.2 Newtons, and the average elongation at break is 55%. Through the contact angle test, the initial water drop contact angle of the hydrophilic hollow fiber membrane is 60 degrees, which can be reduced to 0 degrees within 13 seconds. Through the burst test, the burst pressure of the hydrophilic hollow fiber membrane is 300KPa.

[0108] After the hydrophilic hollow fiber membrane was further packaged into a membrane humidification assembly, the membrane humidification assembly was subjected to a pressure test. After the inflation pressure reached 250KPa, it was sealed and the pressure drop was 1.02KPa / minute. The membrane humidification assembly was used in the fuel cell humidifier system. Dry air at 60°C and 30% humidity was introduced into the inner cavity of the hydrophilic hollow fiber membrane; steam at 90°C and 95% humidity was introduced into the outer cavity. The results showed that the membrane humidification assembly had excellent humidification and heating effects on the air flowing through the inner cavity. The air temperature at the outlet of the inner cavity of the hydrophilic hollow fiber membrane was measured to be 72°C and the humidity was 71%, which met the operation requirements of the fuel cell stack.

[0109] Example 5

[0110] Based on the total weight of the casting solution, 1.5 wt% of polyurethane (Shore hardness 70A) was added to 30 wt% of dimethylacetamide, and stirred at 60°C for complete dissolution; the temperature was lowered to 45°C, and then 20 wt% of polyphenylsulfone was added, and stirring was continued for complete dissolution; 9 wt% of polyvinylpyrrolidone K30 was added, and stirring was continued for complete dissolution; 39.5 wt% of triethylene glycol was added, and stirring was continued for uniform blending; vacuum degassing was then performed for 40 minutes, and the degassing was allowed to stand for 18 hours.

[0111] Prepare a 3% by mass dimethylacetamide aqueous solution at 40°C as an inner gel bath agent, prepare tap water at 40°C as an outer gel bath agent, adjust the liquid surface distance between the spinneret and the outer gel bath agent to 16 cm; the air humidity is 80%; extrude the inner gel bath agent and the casting solution through the spinning head at a speed of 8 m / min, enter the outer gel bath agent for phase inversion spinning, and obtain a hydrophilic hollow fiber membrane.

[0112] After cross-sectional scanning electron microscopy analysis, the membrane wall thickness of the hydrophilic hollow fiber membrane is about 92 microns; the thickness of the dense layer of the hydrophilic hollow fiber membrane is about 1.8 microns, the thickness of the transition layer is 14 microns, the transition layer has a continuous sponge pore structure, no bad bag-like closed pores are found, and the pore size of the second pores gradually increases from the center of the membrane to the surface of the membrane; there is no obvious gradient distribution of the third pores of the macroporous layer.

[0113] The average pore size of the first pores in the dense layer was 19.4 nm as measured by a liquid-liquid porosimeter. The average pore size of the third pores in the macroporous layer was 239 nm as measured by microscopic observation and counting analysis.

[0114] Through the tensile test, the average tensile breaking force of the hydrophilic hollow fiber membrane is 3.6 Newtons, and the average elongation at break is 43%. Through the contact angle test, the initial water drop contact angle of the hydrophilic hollow fiber membrane is 65 degrees, which can be reduced to 0 degrees within 11 seconds. Through the burst test, the burst pressure of the hydrophilic hollow fiber membrane is 299KPa.

[0115] After the hydrophilic hollow fiber membrane was further packaged into a membrane humidification assembly, the membrane humidification assembly was subjected to a pressure test. After the inflation pressure reached 250KPa, it was sealed and the pressure drop was 1.57KPa / minute. The membrane humidification assembly was used in the fuel cell humidifier system. Dry air at 60°C and 30% humidity was introduced into the inner cavity of the hydrophilic hollow fiber membrane; steam at 90°C and 95% humidity was introduced into the outer side. The results showed that the membrane humidification assembly had excellent humidification and heating effects on the air flowing through the inner cavity. The air temperature at the outlet of the inner cavity of the hydrophilic hollow fiber membrane was measured to be 79°C and the humidity was 78%, which met the operation requirements of the fuel cell stack.

[0116] Example 6

[0117] Based on the total weight of the casting solution, 3 wt% of polyurethane (Shore hardness 70A) was added to 40 wt% of methyl pyrrolidone, and stirred at 50°C for complete dissolution; the temperature was lowered to 30°C, and then 18 wt% of polyether sulfone was added, and stirring was continued for complete dissolution; 4 wt% of polyvinyl pyrrolidone K60 and 10 wt% of polyvinyl pyrrolidone K23 were added, and stirring was continued for complete dissolution; 25 wt% of triethylene glycol was added, and stirring was continued for uniform blending; vacuum degassing was then carried out for 60 minutes, and the degassing was allowed to stand for 15 hours.

[0118] Prepare deionized water at 20°C as an inner gel bath, prepare tap water at 20°C as an outer gel bath, adjust the liquid surface distance between the spinneret and the outer gel bath to 14 cm; the air humidity is 85%; extrude the inner gel bath and the casting solution through the spinning head at a speed of 10 m / min, enter the outer gel bath for phase inversion spinning, and obtain a hydrophilic hollow fiber membrane.

[0119] After cross-sectional scanning electron microscopy analysis, the membrane wall thickness of the hydrophilic hollow fiber membrane is about 100 microns; the thickness of the dense layer of the hydrophilic hollow fiber membrane is about 2.6 microns, the thickness of the transition layer is 10.5 microns, the transition layer has a continuous sponge pore structure, and no undesirable bag-like closed pores are found. The pore size of the second pores gradually increases from the center of the membrane to the surface of the membrane; there is no obvious gradient distribution of the third pores of the macroporous layer.

[0120] The average pore size of the first pores in the dense layer was 13.3 nm as measured by a liquid-liquid porosimeter. The average pore size of the third pores in the macroporous layer was 159 nm as measured by microscopic observation and counting analysis.

[0121] Through the tensile test, the average tensile breaking force of the hydrophilic hollow fiber membrane is 3.7 Newtons, and the average elongation at break is 65%. Through the contact angle test, the initial water drop contact angle of the hydrophilic hollow fiber membrane is 53 degrees, which can be reduced to 0 degrees within 7 seconds. Through the burst test, the burst pressure of the hydrophilic hollow fiber membrane is 307KPa.

[0122] After the hydrophilic hollow fiber membrane was further packaged into a membrane humidification assembly, the membrane humidification assembly was subjected to a pressure test. After the inflation pressure reached 250KPa, it was sealed and the pressure drop was 1.32KPa / minute. The membrane humidification assembly was used in the fuel cell humidifier system. Dry air at 60°C and 30% humidity was introduced into the inner cavity of the hydrophilic hollow fiber membrane; steam at 90°C and 95% humidity was introduced into the outer cavity. The results showed that the membrane humidification assembly had excellent humidification and heating effects on the air flowing through the inner cavity. The air temperature at the outlet of the inner cavity of the hydrophilic hollow fiber membrane was measured to be 69°C and the humidity was 70%, which met the operation requirements of the fuel cell stack.

[0123] The water vapor permeation rate of the hydrophilic hollow fiber membranes of Examples 1-6 and Comparative Example 1 was tested under the following test conditions: 10 hydrophilic hollow fiber membranes with an effective length of 25 cm were used and packaged into a small test assembly with both ends open. Dry air at 60°C and 30% humidity was circulated from the inner cavity of the membrane; steam at 90°C and 95% humidity was circulated on the outside of the membrane; the time-average water vapor permeation amount was measured, and the water vapor permeation rate per unit area, per unit time, and per unit water vapor partial pressure difference between the inside and outside of the membrane was calculated. The detailed results are shown in Table 1.

[0124] Table 1

[0125]

[0126] The technical features of the above embodiments may be combined arbitrarily. To make the description concise, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0127] The above embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for those of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A hydrophilic hollow fiber membrane, It is characterized in that It comprises a dense layer, a transition layer and a macroporous layer which are arranged in sequence from the center of the membrane to the surface of the membrane, the dense layer contains first pores, the transition layer contains second pores, the macroporous layer contains third pores, the average pore size of the second pores is larger than the average pore size of the first pores and smaller than the average pore size of the third pores, the pore size of the second pores gradually increases from the center of the membrane to the surface of the membrane, the thickness of the dense layer is 2μm-3μm, the thickness of the transition layer is 4 times-8 times the thickness of the dense layer, the transition layer is a continuous sponge pore structure, the membrane wall thickness of the hydrophilic hollow fiber membrane is 90μm-110μm; the material of the hydrophilic hollow fiber membrane comprises a membrane-making polymer, a hydrophilic polymer and a reinforcing polymer, the initial contact angle of the hollow fiber membrane with a water droplet is less than or equal to 65 degrees, and the contact angle drops to 0 degrees within 20 seconds.

2. The hydrophilic hollow fiber membrane according to claim 1, It is characterized in that The average pore size of the first pores is less than or equal to 20 nm; And / or, the average pore diameter of the third pores is greater than or equal to 100 nm.

3. The hydrophilic hollow fiber membrane according to claim 1 or 2, It is characterized in that The membrane-forming polymer includes at least one of polyethersulfone or polyphenylsulfone, the hydrophilic polymer includes polyvinylpyrrolidone, and the reinforcing polymer includes polyurethane resin.

4. A method for preparing a hydrophilic hollow fiber membrane according to any one of claims 1 to 3, It is characterized in that The steps include: Providing a casting solution, the casting solution comprising a film-forming polymer, a hydrophilic polymer, a first hydrophilic organic solvent, a structure regulator and a reinforcing polymer, wherein the mass fraction of the film-forming polymer in the casting solution is 17%-22%, the mass fraction of the hydrophilic polymer in the casting solution is 6%-14%, the structure regulator comprises oligoethylene glycol, the mass fraction of the structure regulator in the casting solution is 25%-40%, and the mass fraction of the reinforcing polymer in the casting solution is 0.5%-3%; The casting solution and the inner gel bath are extruded through a spinneret and enter the outer gel bath for phase inversion spinning to obtain a hydrophilic hollow fiber membrane.

5. The method for preparing a hydrophilic hollow fiber membrane according to claim 4, It is characterized in that The mass fraction of the first hydrophilic organic solvent in the casting solution is 30%-40%.

6. The method for preparing a hydrophilic hollow fiber membrane according to claim 4, It is characterized in that In the step of extruding the casting liquid and the inner gel bath through a spinneret and entering the outer gel bath for phase inversion spinning, the distance between the spinneret and the liquid surface of the outer gel bath is 8 cm-25 cm, the spinning speed of the phase inversion spinning is 5 m / min-15 m / min, and the humidity of the air between the spinneret and the liquid surface of the outer gel bath is 60%-100%.

7. The method for preparing a hydrophilic hollow fiber membrane according to claim 4, It is characterized in that The inner gel bath agent comprises a second hydrophilic organic solvent and water, and the mass fraction of the second hydrophilic organic solvent in the inner gel bath agent is less than or equal to 5%.

8. Use of the hydrophilic hollow fiber membrane according to any one of claims 1 to 3 in a membrane humidification component.