Waterproof box for automobile, light-curable silicone composition and silicone gel

By using SOx-based photocurable silicone as a sealing material in the waterproof box for automobiles and combining with snap-ons, the problems of high assembly cost and insufficient heat resistance in the prior art are solved, and the re-resolution in high temperature environments are realized Assembly and long-term waterproofing.

CN113550824BActive Publication Date: 2024-11-19DENSO CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110441570.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-04-24
Filing Date
2021-04-23
Publication Date
2024-11-19
Estimated Expiration
2041-04-23

AI Technical Summary

Technical Problem

The existing automotive waterproof boxes are costly during assembly and maintenance. The sealing materials use rubber gaskets or adhesives to fasten the components, and the heat resistance is insufficient in high-temperature environments, making it difficult to achieve reassembly and long-term waterproofing performance.

Method used

Use photocured silicone with SOx group as the sealing material, and liquid-tight sealing is performed between the main body part and the cover part of the box by snap-fitting, reducing the use of fastening components, and utilizing the high adhesion and heat resistance of SOx group. Maintains waterproof performance under high temperature environments.

Benefits of technology

It reduces assembly and maintenance costs, realizes reassembly and long-term waterproofing performance in high-temperature environments, reduces the pressure requirement of sealing materials, and improves waterproofing performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113550824B_ABST
    Figure CN113550824B_ABST
Patent Text Reader

Abstract

The present invention provides a waterproof box for automobiles that can reduce the cost required for assembly work, can be reassembled, and has excellent heat resistance and waterproof performance, and a photocurable silicone composition or silicone rubber that can be used for the waterproof box. The waterproof box for automobiles comprises: a box body having a storage space for storing stored objects and an opening connected to the storage space, and a cover installed on the box body to close the opening. A material having a group selected from SO, SO 2 Base and SO 3 The sealing material is made of organic silicone with adhesiveness and at least one SOx group in the base. In addition, at least one of the box body and the cover is provided with a receiving part, and a locking convex part that is locked to the receiving part is provided at a position corresponding to the receiving part in the box body and the cover.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a waterproof box for automobiles, a light-curing organic silicon composition and organic silicon gel. Background Art

[0002] The engine room of a car is equipped with electrical components such as an engine ECU (electronic control unit), a flow path switching valve, an electronic throttle, a battery pack, a power control unit, a camera for identifying white lines, a LiDAR (light detection and ranging) sensor, etc. These electrical components have electronic components, sensors, gears and other objects to be contained and a box for containing the objects to be contained. The box has: a box body having a storage space for containing the objects to be contained and an opening connected to the storage space; a cover for closing the opening of the box body, and a sealing material interposed between the box body and the cover to make a liquid-tight seal between the two.

[0003] As sealing materials, rubber gaskets such as O-rings and washers have been used in the past. For example, Patent Document 1 describes a technique in which a sealing material made of heatable butyl rubber is applied to the sealing surface of at least one of the two housing parts.

[0004] In recent years, there has been a technique for using a so-called liquid gasket as a sealing material, in which a liquid curable composition is applied to a desired portion and cured at the portion to form a gasket.

[0005] There is also a technique in which a box body and a cover are bonded together using an adhesive to achieve a liquid-tight seal between the box body and the cover.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application No. 2001-525985 Summary of the invention

[0009] When a rubber gasket or a liquid gasket as described in Patent Document 1 is used as a sealing material, in order to achieve a liquid-tight seal between the box body and the cover, it is necessary to fasten the cover to the box body via a fastening member such as a bolt, and fully compress the gasket between the two. Therefore, the component cost of the fastening member itself and the operation cost required for the fastening operation are generated, which hinders the cost reduction of the electrical components.

[0010] In addition, when an O-ring or a gasket is used as a sealing material, these components need to be manually arranged, which may further increase the cost of the electrical component.

[0011] On the other hand, when the box body and the cover are bonded together using an adhesive, there is no need for a fastening operation of the cover and the box body, or a fastening member for fastening the two. However, in this case, after the cover is bonded to the box body, if it is necessary to remove the cover from the box body for some reason, the cured adhesive has to be destroyed. In order to avoid the above problem, a sealing material is desired, which can remove the cover from the box body and reassemble after the cover is once installed on the box body.

[0012] In addition, since the engine room is equipped with a high-heat engine, the temperature in the engine room varies widely from the outside air temperature to the high temperature during engine operation. Therefore, in addition to waterproof performance, high heat resistance is also required for such sealing materials.

[0013] The present invention has been made in view of the above problems, and an object of the present invention is to provide a waterproof box for an automobile that can reduce the cost required for assembly work, can be reassembled, and has excellent heat resistance and waterproof performance, as well as a photocurable silicone composition and silicone gel that can be used in the waterproof box for an automobile.

[0014] One embodiment of the present invention is a waterproof box (1, 102) for an automobile, having the following structure:

[0015] The box body (2) is provided with a receiving space (21) for receiving the received object and an opening (22) connected to the receiving space;

[0016] A cover (3, 302) is mounted on the box body and closes the opening;

[0017] A sealing material (4) is composed of an organic silica gel having at least one SOx group selected from SO group, SO2 group and SO3 group and having adhesiveness and is interposed between the box body and the cover;

[0018] a receiving portion (31) provided on at least one of the box body and the cover; and

[0019] The engaging protrusion (23) is arranged at a position corresponding to the receiving portion in the box body and the cover, and is locked in the receiving portion.

[0020] Another embodiment of the present invention is a photocurable silicone composition, comprising the following components (A) to (D), which are configured to form silicone gel having at least one SOx group selected from SO groups, SO2 groups, and SO3 groups:

[0021] (A) component: polyorganosiloxane having a vinyl siloxane group,

[0022] (B) component: mercapto-based crosslinking agent,

[0023] (C) component: free radical photoinitiator,

[0024] Component (D): an organic peroxide having a 10-hour half-life temperature of 150° C. or less.

[0025] Still another aspect of the present invention is an organic silica gel obtained by curing the photocurable organic silica composition of the above aspect, and having at least one SOx group selected from the group consisting of a SO group, a SO2 group, and a SO3 group.

[0026] The above-mentioned waterproof box for automobile (hereinafter, abbreviated as "waterproof box") comprises: a box body with a storage space and a cover installed on the box body. In addition, at least one of the box body and the cover is provided with a receiving portion. Moreover, a snap-fitting convex portion is provided at a position corresponding to the receiving portion in the box body and the cover, and the snap-fitting convex portion is snapped to the receiving portion. That is, the box body and the cover are snapped by so-called snap fit.

[0027] The waterproof box can mount the cover to the box body by a simple operation of pressing the engaging protrusion into the receiving portion. In addition, the waterproof box can mount the cover to the box body without using fastening components such as bolts. Therefore, according to the waterproof box, the component cost of the fastening component can be reduced, and the operation cost required for the installation of the cover and the box body can be reduced.

[0028] In addition, a sealing material composed of organic silicone having the above-mentioned SOx group and having adhesiveness is sandwiched between the box body and the cover. The organic silicone having the SOx group can adhere to the two when the cover is installed on the box body, and the gap between the sealing material and the cover and the gap between the sealing material and the box body are closed. Thus, the cover and the box body can be sealed liquid-tight. Furthermore, since the organic silicone has high heat resistance, it can maintain waterproof performance for a long time even in the engine room.

[0029] Furthermore, the waterproof box can be easily removed from the box body by fastening the box body and the cover by snap-fitting and using the specific organic silicone as a sealing material, so that after the cover is once mounted on the box body, the cover can be easily removed from the box body. Furthermore, after the cover is removed from the box body, the cover can be mounted on the box body again, so that the sealing material can be used to seal the two liquid-tightly.

[0030] In addition, the photocurable silicone composition includes the components (A) to (D) and is configured to form silicone rubber having at least one SOx group selected from the group consisting of SO, SO2, and SO3. Therefore, silicone rubber having the SOx group can be formed according to the photocurable silicone composition. Moreover, silicone rubber having the SOx group has excellent adhesion to the box body and the cover, so when used as a sealing material for a waterproof box, it can maintain waterproof performance for a long time.

[0031] As described above, according to the above-mentioned embodiment, it is possible to provide a waterproof box which can reduce the cost required for assembly work, can be reassembled, and has excellent heat resistance and waterproof performance, and a photocurable silicone composition or silicone gel which can be used for the waterproof box.

[0032] It should be noted that the symbols in parentheses described in the claims and the means for solving the problems indicate the correspondence relationship with the specific means described in the embodiments described later, and do not limit the technical scope of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 It is a cross-sectional view showing the main part of the waterproof box in Embodiment 1.

[0034] Figure 2 yes Figure 1 A partial enlarged view of the sealing material in FIG.

[0035] Figure 3 This is a partially enlarged cross-sectional view showing the main part of the waterproof box in the second embodiment in which the protrusion is pressed into the sealing material.

[0036] Figure 4 This is an explanatory diagram showing the tensile shear adhesive strength of test pieces II to KK in Experimental Example 2.

[0037] Figure 5 1 is an explanatory diagram showing the X-ray absorption spectra of the test pieces LL and MM in Experimental Example 3.

[0038] Figure 6 1 is an explanatory diagram showing the X-ray absorption spectra of the test pieces NN and OO in Experimental Example 4.

[0039] Explanation of symbols

[0040] 1. 102 waterproof box

[0041] 2. Box body

[0042] 21 Containment Space

[0043] 22 Opening

[0044] 23 Engagement protrusion

[0045] 3. 302 cover

[0046] 31 Receiving Department

[0047] 4 Sealing materials DETAILED DESCRIPTION

[0048] (Implementation Method 1)

[0049] Reference Figure 1-2 The embodiment of the waterproof box is described below. The waterproof box of this embodiment is a box installed in a car, specifically, a waterproof box installed in a car to store objects. Figure 1 As shown, the waterproof box 1 of this embodiment has: a box body 2 having a storage space 21 for storing the stored object and an opening 22 connected to the storage space 21, and a cover 3 installed on the box body 2 and closing the opening 22. A sealing material 4 composed of organic silica gel having at least one SOx group selected from SO groups, SO2 groups and SO3 groups and having adhesiveness is sandwiched between the box body 2 and the cover 3. In addition, a receiving portion 31 is provided on at least one of the box body 2 and the cover 3, and a locking protrusion 23 that is locked to the receiving portion 31 is provided at a position corresponding to the receiving portion 31 in the box body 2 and the cover 3.

[0050] The shape and structure of the waterproof box 1 are not particularly limited. For example, the waterproof box 1 may have one receiving space 21 surrounded by the box body 2 and the cover 3, or may have two or more receiving spaces 21. In addition, the number of openings 22 connected to the receiving space 21 may be one or two.

[0051] Although not shown in the figure, the waterproof box 1 of this embodiment is in the shape of a rectangular parallelepiped. Figure 1 As shown, the box body 2 has a bottom wall 24, a side wall 25 erected from the outer peripheral portion of the bottom wall 24, and a storage space 21 surrounded by the bottom wall 24 and the side wall 25. In addition, the waterproof box 1 has an opening 22 surrounded by the front end 251 of the side wall 25.

[0052] like Figure 2 As shown, the box body 2 of this embodiment has a sealing material holding groove 26 having a bottom surface 261 and a side surface 262 connected to the bottom surface 261 at the front end 251 of the side wall 25. The sealing material holding groove 26 is provided around the entire circumference of the front end 251 of the side wall 25. The sealing material 4 is arranged on the bottom surface 261 of the sealing material holding groove 26.

[0053] In addition, if Figure 1As shown in the figure, a plurality of engaging protrusions (also referred to as protrusions) 23 protruding outward are provided on the outer surface of the side wall portion 25. These engaging protrusions 23 are inserted into the receiving holes 311 of the receiving portion 31 described later. Thus, the engaging protrusions 23 are locked to the receiving portion 31. That is, the engaging protrusions 23 are physically fixed to the receiving portion 31 by being inserted into the receiving holes 311 of the receiving portion 31 and engaging with the receiving portion 31.

[0054] The box body 2 of this embodiment is configured so that the stored object can be stored in the storage space 21. As the stored object stored in the storage space 21, for example, components of a car, more specifically, electronic circuits, sensors, electronic devices such as motors, driving components such as gears, etc. can be cited.

[0055] The opening 22 of the box body 2 is covered by the cover 3. The cover 3 of this embodiment is in the shape of a flat plate. Figure 2 As shown in the figure, the outer peripheral portion has a sealing surface 32 in contact with the sealing material 4. In addition, a plurality of receiving portions 31 extending and protruding toward the box body 2 are provided at the edge of the cover 3. Although not shown in the figure, the receiving portion 31 of this embodiment is annular. Figure 2 As shown, the receiving portion 31 is provided with a receiving hole 311 for receiving the engaging protrusion 23. The engaging protrusion 23 is inserted into the receiving hole 311.

[0056] The box body 2 and the cover 3 may be composed of metals such as iron and aluminum, resins such as engineering plastics and super engineering plastics, or metals and resins. From the perspective of lightweighting the waterproof box 1, it is preferred that at least one of the box body 2 and the cover 3 is composed of resins, and it is more preferred that both are composed of resins. The box body 2 and the cover 3 of this embodiment are both composed of polyamide resins.

[0057] In this embodiment, the box body 2 and the cover 3 are sealed liquid-tightly by using adhesive organic silicone as the sealing material 4. Organic silicone is much softer than rubber gaskets such as O-rings, so it is possible to reduce the pressure applied to the sealing material 4 compared to conventional waterproof boxes that use rubber gaskets for sealing. Therefore, even when a resin with lower rigidity than metal is used in the box body 2 and the cover 3, the sealing material 4 can be fully compressed to ensure waterproof performance.

[0058] like Figure 1 and Figure 2 As shown, a sealing material 4 composed of organic silicone having a SOx group and having adhesiveness is sandwiched between the box body 2 and the cover 3. Figure 2 As shown in FIG. 2 , the sealing material 4 is disposed on the bottom surface 261 of the sealing material holding groove 26. Figure 2As shown by the dotted line in the figure, when the cover 3 is not installed (symbol 40), the cross-sectional shape of the box body 2 has a mountain shape, and the central part in the width direction protrudes more than the front end 251 of the side wall 25. Figure 2 As shown by the solid line in the figure, it is compressed by the sealing surface 32 of the cover 3.

[0059] Here, organic silicone refers to a gel containing a polymer of polysiloxane. Organic silicone is preferably organic silicone obtained by curing a composition containing a curable organic polysiloxane compound. It should be noted that, in order to distinguish before and after curing, the state before curing, that is, the composition in a liquid state at 25°C is referred to as an organic silicone composition, and the gel-like composition after curing is referred to as an organic silicone.

[0060] The viscosity of the silicone composition at 25°C is not particularly limited, but is preferably 200 to 600 Pa·s. In this case, the discharge property of the silicone composition can be further improved, and the flow of the silicone composition after coating can be suppressed, making it easier to maintain the shape of the silicone composition after discharge for a longer period of time. In addition, the structural viscosity ratio of the silicone composition at 25°C is preferably 2.5 to 5.5. In this case, the flow of the silicone composition after coating can be suppressed, making it easier to maintain the shape of the silicone composition after discharge for a longer period of time, and it is not easy to form corners in the silicone composition after coating.

[0061] The silicone composition is formed by reacting an organopolysiloxane compound having a functional group under the action of heat, moisture, light, etc. to form a polymer to form silicone rubber. Silicon rubber has adhesiveness, that is, the property of bonding by simply pressing the silicone rubber.

[0062] As the silicone composition, for example, a heat-curable silicone composition, a moisture-curable silicone composition, or a photocurable silicone composition can be used. The silicone composition is particularly preferably a photocurable silicone composition.

[0063] Examples of the heat-curable silicone composition include, but are not limited to, a composition comprising a polyorganosiloxane having a vinyl siloxane group and a peroxide, a polyorganosiloxane having a vinyl siloxane group, a composition comprising a hydrogen siloxane compound and a hydrosilylation metal catalyst, a composition comprising a polyorganosiloxane having an epoxy group and a thermal cationic catalyst, etc. These may be used alone or in combination of two or more.

[0064] Examples of moisture-curable silicone compositions include, but are not limited to, polyorganosiloxanes having hydrolyzable silyl groups, compositions comprising silane coupling agents and condensation catalysts, polyorganosiloxanes having isocyanate groups, compositions comprising polyol compounds and condensation catalysts, etc. These may be used alone or in combination of two or more.

[0065] Examples of the photocurable silicone composition include, but are not limited to, a composition comprising a polyorganosiloxane having a (meth) acrylic group and a free radical photoinitiator, a polyorganosiloxane having a vinyl siloxane group, a composition comprising a polythiol compound and a free radical photoinitiator, a composition comprising a polyorganosiloxane having an epoxy group and a photocationic catalyst, etc. These may be used alone or in combination of two or more.

[0066] In addition, the above-mentioned heat-curable silicone composition, moisture-curable silicone composition, and light-curable silicone composition may be composed of a single component or a plurality of components of two or more. From the viewpoint of forming the sealing material 4 on the spot, it is preferred to use a light-curable silicone composition that can be cured at low temperature and in a short time by a device such as an ultraviolet irradiator or an LED irradiator.

[0067] The above-mentioned organic silica gel contains one or more SOx groups selected from the group consisting of SO groups, SO2 groups and SO3 groups. These SOx groups are usually bonded to polysiloxane chains in the organic silica gel. By using the above-mentioned specific organic silica gel, the entry of moisture and the like between the box body 2 and the cover 3 can be effectively suppressed, thereby improving the waterproof performance. As the reason why the above-mentioned specific organic silica gel has such an effect, for example, the following reasons are considered. Since the SOx group has a high polarity, for example, when the box body 2 and the cover 3 have polar groups such as hydroxyl groups, amide groups and carboxyl groups, it can be hydrogen bonded with these polar groups. It is speculated that the adhesion between the organic silica gel and the box body 2 and the adhesion between the organic silica gel and the cover 3 can be improved by hydrogen bonding between such SOx groups and polar groups.

[0068] The SOx group in the organic silica gel can be formed by various methods. For example, the SOx group can be formed by oxidizing the SH group and the thioether group in the obtained organic silica gel after curing a composition containing a curable organic polysiloxane compound and a thiol-based crosslinking agent having an SH group. The method for oxidizing the SH group and the thioether group is not particularly limited. For example, the SH group and the thioether group can be oxidized by contacting the organic silica gel with an oxidizing atmosphere. In addition, it is also possible to form the SOx group by pre-adding an oxidizing agent that is configured to oxidize the SH group and the thioether group in the composition before curing, and reacting the oxidizing agent with the SH group and the thioether group during or after curing of the composition. In addition, the oxidation of the SH group and the thioether group can also be promoted by heating the curing composition and the organic silica gel. Alternatively, the organic silicone composition may contain a SOx group in advance.

[0069] The hardness of the organic silica gel can be expressed by the durometer hardness obtained by the E-type durometer specified in JIS K6253-3:2012. The hardness of the sealing material 4 when the E-type durometer is pressed with a load of 1 kg is not particularly limited, and is preferably 5 to 30, for example. At this time, when the cover 3 is mounted on the box body 2 and the sealing material 4 is compressed, the repulsive force of the sealing material 4 can be appropriately increased. As a result, the waterproof performance of the waterproof box 1 can be further improved.

[0070] The tensile shear bonding strength of the sealing material 4 is not particularly limited, and is preferably 0.10 MPa or more, more preferably 0.20 MPa or more, and further preferably 0.25 MPa or more. At this time, when the cover 3 is installed on the box body 2 and the sealing material 4 is compressed, the adhesive force of the sealing material 4 to the cover 3 and the adhesive force of the sealing material 4 to the box body 2 can be made greater, and the waterproof performance of the waterproof box 1 can be further improved.

[0071] From the viewpoint of further improving the waterproof performance of the waterproof box 1, as the sealing material 4, it is preferred to use an organic silicone gel obtained by curing a photocurable silicone composition containing the following components (A) to (C), and it is more preferred to use an organic silicone gel obtained by curing a photocurable silicone composition containing the following components (A) to (D).

[0072] (A) Component: Polyorganosiloxane having vinyl siloxane groups

[0073] Component (B): mercapto-based crosslinking agent

[0074] (C) Component: Free Radical Photoinitiator

[0075] Component (D): an oxidizing agent capable of oxidizing SH groups and thioether groups

[0076] The photocurable silicone composition containing the above-mentioned components (A) to (D) is constituted in such a way that a polymerization reaction of polyorganosiloxane is induced by irradiation with energy rays such as visible light and ultraviolet rays. In addition, by pre-adding the above-mentioned oxidizing agent (component (D)) to the photocurable silicone composition, the SH groups and thioether groups present in the cured silicone rubber can react with the above-mentioned oxidizing agent, so that the SH groups and thioether groups in the silicone rubber can be easily oxidized. Therefore, according to the above-mentioned photocurable silicone composition, silicone rubber having the above-mentioned SOx groups can be formed.

[0077] The molecular structure of the polyorganosiloxane having a vinylsiloxane group (component (A)) is preferably linear, but may have a branched structure. Examples of the polyorganosiloxane include dimethylsiloxane terminated with dimethylvinylsiloxy groups at the molecular chain ends, dimethylsiloxane / diphenylsiloxane copolymer terminated with dimethylvinylsiloxy groups at the molecular chain ends, dimethylsiloxane / methylvinylsiloxane / diphenylsiloxane copolymer terminated with dimethylvinylsiloxane groups at the molecular chain ends, dimethylsiloxane in which one molecular chain end is terminated with dimethylvinylsiloxy groups and the other molecular chain end is terminated with trimethylsiloxy groups, dimethylsiloxane in which one molecular chain end is terminated with dimethylvinylsiloxy groups and the other molecular chain end is terminated with trimethylsiloxy groups, methylvinylsiloxane / diphenylsiloxane, dimethylsiloxane / methylvinylsiloxane copolymer terminated with trimethylsiloxy groups at both molecular chain ends, and dimethylsiloxane / methylvinylsiloxane / diphenylsiloxane copolymer terminated with trimethylsiloxy groups at both molecular chain ends. These may be used alone or in combination of two or more. The functional group equivalent weight (ie, vinyl group equivalent weight) of the polyorganosiloxane having a vinylsiloxane group is not particularly limited, but is preferably 100 g / eq to 50,000 g / eq, for example.

[0078] As the mercapto-based crosslinking agent (component (B)), for example, a polythiol compound having a plurality of SH groups in one molecule can be used. Examples of the polythiol compound include trimethylolpropane tris(3-mercaptopropionate), pentaerythritol tetrakis(3-mercaptopropionate), trimethylolpropane tris(3-mercaptobutyrate), trimethylolethane tris(3-mercaptobutyrate), trimethylolethane tris(3-mercaptobutyrate), ethylene glycol bis(3-mercaptoglycolate), butanediol bis(3-mercaptoglycolate), trimethylolpropane tris(3-mercaptoglycolate), pentaerythritol tetrakis(3-mercaptoglycolate), tris-[(3-mercaptopropionyloxy)-ethyl]-isocyanurate, pentaerythritol tetrakis(3-mercaptopropionate), tetraethylene glycol bis(3-mercaptopropionate), dipentaerythritol hexa(3-mercaptopropionate), pentaerythritol tetrakis(3-mercaptobutyrate), 1,4-bis(3-mercaptobutyryloxy)butane, polyorganosiloxane having a mercapto group, and polysulfide polymer having a mercapto group. These may be used alone or in combination of two or more. By using a cured product of a silicone composition containing a mercapto-based crosslinking agent as the sealing material 4, the adhesive force of the sealing material 4 to the lid 3 and the adhesive force of the sealing material 4 to the box body 2 can be made greater, and the waterproof performance of the waterproof box 1 can be further improved. The mercapto-based crosslinking agent is preferably a polythiol compound having two or more mercapto groups (mercapt-, thio-) in one molecule.

[0079] The photocurable silicone composition may contain one compound selected from the compounds having a mercapto group as the component (B), or may contain two or more compounds. In addition, the functional group equivalent of the component (B) (i.e., the equivalent of the mercapto group) is preferably 100 g / eq to 50,000 g / eq.

[0080] The content of the above-mentioned (B) component in the photocurable silicone composition is not particularly limited, and is preferably 0.1 to 10 parts by mass relative to 100 parts by mass of the above-mentioned (A) component. By making the content of the above-mentioned (B) component 0.1 parts by mass or more, the photocurability can be further improved. In addition, by making the content of the above-mentioned (B) component 10 parts by mass or less, the storage stability can be further improved. From the viewpoint of making the adhesion of the sealing material 4 to the cover 3 and the adhesion of the sealing material 4 to the box body 2 greater, the content of the above-mentioned (B) component is more preferably 0.50 to 5.0 parts by mass relative to 100 parts by mass of the above-mentioned (A) component.

[0081] The radical photoinitiator (component (C)) is not particularly limited as long as it is a compound that can promote the reaction of a vinylsiloxane group and a mercapto group by light irradiation. Examples of the radical photoinitiator include 1-hydroxy-cyclohexyl phenyl ketone, 2,2-dimethoxy-2-acetophenone, xanthone, fluorenone, benzaldehyde, fluorene, anthraquinone, triphenylamine, carbazole, 3-methylacetophenone, 4-chlorobenzophenone, 4,4'-dimethoxybenzophenone, 4,4'-diaminobenzophenone, Michler's ketone, benzoin propyl ether, benzoin ethyl ether, benzyl dimethyl ketal, 1-(4-isopropylphenyl)-2-hydroxybenzophenone ... The free radical photoinitiator may be used alone or in combination of two or more. In addition, the free radical photoinitiator may be a compound having an absorption peak wavelength in the ultraviolet region and / or the visible light region.

[0082] The content of the above-mentioned (C) component in the photocurable silicone composition is not particularly limited, and is preferably 0.1 to 5.0 parts by mass relative to 100 parts by mass of the above-mentioned (A) component. The photocurability can be manifested by making the content of the above-mentioned (C) component 0.1 parts by mass or more. In addition, the storage stability can be further improved by making the content of the above-mentioned (C) component 5.0 parts by mass or less.

[0083] As the oxidizing agent (component (D)) contained in the photocurable silicone composition, a compound that can oxidize the SH group and the thioether group can be used. More specifically, a peroxide, preferably an organic peroxide, can be used as the oxidizing agent. The 10-hour half-life temperature of the organic peroxide as the oxidizing agent is not particularly limited, and for example, it is preferably below 150°C, and more preferably 60°C to 110°C. It should be noted that the half-life is an indicator of the decomposition rate of the organic peroxide at a certain temperature, and refers to the time required for the original organic peroxide to decompose and its active oxygen content to become 1 / 2. In addition, the aforementioned 10-hour half-life temperature refers to the temperature at which the half-life is 10 hours when the organic peroxide is decomposed at a certain temperature.

[0084] The organic peroxide as the component (D) is preferably a peroxyester, and more preferably has a molecular structure represented by the following general formula (1) or the following general formula (2).

[0085] R 1 -O-O-CO-R 2 ···General formula (1)

[0086] R 3 -O-O-CO-O-R 4 ···General formula (2)

[0087] (R 5 (-CO-O-O) n -R 6 ···General formula (3)

[0088] It should be noted that R in the above general formula (1), the above general formula (2) and the above general formula (3) 1 ~R 6 Each is independently a substituted or unsubstituted aromatic group, a hydrocarbon group selected from an aliphatic hydrocarbon group and an unsaturated hydrocarbon group. In addition, n is a natural number greater than 1.

[0089] Here, as the aromatic group, for example, monocyclic aromatic groups such as substituted or unsubstituted phenyl, fused polycyclic aromatic groups such as substituted or unsubstituted naphthyl, non-fused polycyclic aromatic groups such as biphenyl, etc. can be mentioned. The aromatic group may have one or more substituents, and as the substituent, for example, an aliphatic hydrocarbon group described later can be mentioned. In addition, the aromatic group can be bonded to the adjacent oxygen atom in formula (1), (2), and (3) via a substituent. The number of carbon atoms in the aromatic group is not particularly limited, and is, for example, 6 to 40, preferably 6 to 20.

[0090] As the aliphatic hydrocarbon group, for example, a straight-chain alkyl group, a branched-chain alkyl group, a cycloalkyl group, etc. can be cited. As the straight-chain alkyl group, for example, a methyl group, an ethyl group, a n-propyl group, a n-butyl group, a n-pentyl group, a n-hexyl group, a n-heptyl group, a n-octyl group, a n-nonyl group, a n-decyl group, a n-undecyl group, and a n-dodecyl group can be cited. In addition, as the branched-chain alkyl group, for example, an isopropyl group, a tert-butyl group, an isobutyl group can be cited. As the cycloalkyl group, for example, a cyclopentyl group, a cyclohexyl group, a cycloheptyl group, a cyclooctyl group, etc. can be cited. It should be noted that the cycloalkyl group can be substituted by a straight-chain alkyl group and / or a branched-chain alkyl group. The number of carbon atoms in the aliphatic hydrocarbon group is not particularly limited, and is, for example, 1 to 40, preferably 1 to 20, and more preferably 1 to 10.

[0091] Examples of the unsaturated hydrocarbon group include vinyl, n-propenyl, n-butenyl, n-pentenyl, n-hexenyl, n-heptenyl, n-octenyl, n-nonenyl, n-decenyl, n-undecenyl, and n-dodecenyl. The number of carbon atoms in the unsaturated hydrocarbon group is not particularly limited, and is, for example, 1 to 40, preferably 1 to 20, and more preferably 1 to 10.

[0092] It should be noted that the above hydrocarbon group may be bonded to the adjacent oxygen atom in formula (1), (2) or (3) at any position. In addition, when the hydrocarbon group is polyvalent, it may replace any hydrogen atom of the hydrocarbon group and bond to the adjacent oxygen atom in formula (1), (2) or (3).

[0093] As the organic peroxide that can be used as (D) component in commercially available organic peroxide, for example, the following goods can be cited. PERHEXYL PV, PERBUTYL PV, PERHEXA 25O, PEROCTA O, PERHEXYLO, PERBUTYL O, PERBUTYL L, PERBUTYL 355, PERHEXYL I, PERBUTYL I, PERBUTYL E, PERHEXA25Z, PERHEXYL Z, PERBUTYL ZT, PERBUTYL Z, PERCUMYL ND, PEROCTA ND, PERHEXYL ND, PERBUTYL ND, PERBUTYL A, PERCURE O, etc. manufactured by NOF Corporation. These organic peroxides can be used alone or in combination with more than two kinds. In addition, above-mentioned (D) component is not limited to the aforementioned goods. It should be noted that "PERHEXYL", "PERBUTYL", "PERHEXA", "PEROCTA", "PERCUMYL" are registered trademarks of NOF Corporation.

[0094] The content of the above-mentioned (D) component in the photocurable silicone composition is not particularly limited, and is preferably 0.1 to 5.0 parts by mass relative to 100 parts by mass of the above-mentioned (A) component. By making the content of the above-mentioned (D) component 0.1 parts by mass or more, the above-mentioned SOx group can be more reliably formed in the organic silica gel formed by curing the photocurable silicone composition. As a result, the adhesion between the sealing material 4 and the box body 2 and the adhesion between the sealing material 4 and the cover 3 can be further improved. In addition, by making the content of the above-mentioned (D) component 5.0 parts by mass or less, the storage stability can be further improved.

[0095] The silicone composition may further contain a filler as component (E). As the filler, for example, inorganic fillers such as calcium carbonate powder, silica powder, fumed silica powder, talc powder, aluminum hydroxide powder, glass beads, and organic fillers such as polystyrene powder, polyurethane powder, acrylic powder, silicone rubber powder, and silicone resin powder can be used, but it is not limited to these. From the viewpoint of controlling the fluidity of the composition, the specific surface area of ​​the filler measured by the BET method is not particularly limited, for example, preferably 105m 2 / g~135m 2 / g. From the same point of view, the particle size of the filler is not particularly limited, for example, preferably 1nm to 100μm. It should be noted that when the particle size of the filler is at the nm level, the particle size of the filler is a value calculated based on an electron microscope image. In addition, when the particle size of the filler is at the μm level, the particle size of the filler refers to the value of the 50% average particle size (so-called d50) of the particle size distribution obtained using a laser particle size analyzer. In addition, the filler is preferably composed of silicon dioxide.

[0096] Pigments, colorants, plasticizers, flame retardants, antioxidants, polymerization inhibitors, defoamers, coupling agents, leveling agents, rheology control agents, etc. can be further added to the silicone composition within a range that does not impair its properties. By adding these other components, a composition and a cured product thereof having excellent resin strength, adhesive strength, workability, storage stability, etc. can be obtained.

[0097] The photocurable silicone composition is preferably constructed in a manner that can be cured by irradiation with energy rays such as ultraviolet rays and visible light. In this case, the energy consumption in the manufacturing process of the waterproof box 1 can be further reduced, and the operating cost during manufacturing can be further reduced. As an irradiation device for irradiating energy rays, for example, a SPOT-type irradiation device having an energy ray source constructed in a manner that can locally irradiate energy rays to the object to be processed and constructed in a manner that the energy ray source can be moved, a conveyor-type irradiation device having an energy ray source constructed in a manner that can irradiate energy rays and a conveyor belt constructed in a manner that allows the object to be processed to move relative to the energy ray source, etc. can be used. In addition, as an energy ray source, for example, an LED (i.e., light emitting diode) lamp, a high-pressure mercury lamp, etc. can be used. From the viewpoint of further reducing energy consumption in the manufacturing process, as an energy ray source, it is preferred to use an LED lamp that consumes less power.

[0098] The sealing material 4 of the present embodiment is arranged on the bottom surface 261 of the sealing material holding groove 26, and is compressed by the bottom surface 261 and the sealing surface 32 of the cover 3. In addition, a gap is formed between the side surface 262 of the sealing material holding groove 26 and the sealing material 4. By arranging the sealing material 4 in this way, it is possible to ensure a gap for the sealing material 4 to deform when the cover 3 is installed on the box body 2. As a result, it is possible to avoid excessive increase in the repulsive force of the sealing material 4 when the sealing material 4 is compressed. As a result, it is possible to avoid excessive increase in the load applied to the receiving portion 31 and the engaging protrusion 23, and it is possible to maintain the state in which the engaging protrusion 23 is engaged with the receiving portion 31 for a longer period of time.

[0099] In addition, in the present embodiment, the sealing material 4 is compressed so that the height Hf of the compressed state between the box body 2 and the cover 3 is 40 to 80% of the height Hi of the uncompressed state. By making the compression amount of the sealing material 4 within the above-mentioned specific range, the repulsive force of the sealing material 4 can be appropriately increased when the cover 3 is attached to the box body 2 and the sealing material 4 is compressed. As a result, the waterproof performance of the waterproof box 1 can be further improved.

[0100] The waterproof box 1 of this embodiment can be manufactured, for example, by the following manufacturing method, which comprises the following steps: a coating step of coating the silicone composition on the desired positions of the box body and the cover; a curing step of curing the silicone composition to form the sealing material; and an installation step of installing the cover to the box body so that the sealing material is interposed therebetween and the engaging protrusion is stopped at the receiving portion.

[0101] In the coating step, for example, a coating device including a coating nozzle configured to discharge the silicone composition may be used, and the silicone composition may be discharged from the coating nozzle while the coating nozzle is moved along the portion where the sealing material is to be disposed.

[0102] In addition, in the curing step, it is sufficient to adopt an appropriate curing method corresponding to the curing system of the silicone composition. For example, when the silicone composition is a heat-curing silicone composition, the silicone composition can be cured to form a sealing material by heating the silicone composition after the silicone composition is applied to the box body and / or the cover.

[0103] When the silicone composition is a photocurable silicone composition, the coating step and the curing step may be performed as separate steps or may be performed continuously. In the former case, for example, the following method may be adopted: after the coating of the photocurable silicone composition is completed in the coating step, the entire photocurable silicone composition is irradiated with energy rays to form the sealing material 4.

[0104] In the latter case, the following method can be adopted: in the above-mentioned coating process, while coating the photocurable silicone composition on the desired part, the photocurable silicone composition coated on the desired part is locally irradiated with energy rays. In this case, the coating process and the curing process can be carried out in parallel, so the number of processes can be reduced and productivity can be further improved. In addition, in this case, the energy ray source can be miniaturized, so the equipment cost can be further reduced, and the energy required for manufacturing the waterproof box 1 can be further reduced.

[0105] More specifically, the above method can be implemented, for example, by using a coating device having a coating nozzle configured to coat the photocurable silicone composition and an energy ray source configured to irradiate energy rays, and moving the coating nozzle and the energy ray source in a manner such that the energy ray source follows the discharge nozzle.

[0106] Next, the effects of the waterproof box 1 of this embodiment will be described. The box body 2 and the cover 3 in the waterproof box 1 of this embodiment are locked by a so-called snap fit in which the locking protrusion 23 is locked in the receiving portion 31. Therefore, the cover 3 can be mounted on the box body 2 by a simple operation of pressing the locking protrusion 23 into the receiving portion 31. As a result, the cost required for the assembly operation of the waterproof box 1 can be reduced.

[0107] The box body 2 and the cover 3 are sealed by a sealing material 4 made of organic silicone having a SOx group and having adhesiveness. Thus, the cover 3 and the box body 2 can be sealed liquid-tightly and waterproof performance can be maintained for a long time.

[0108] Furthermore, the waterproof box 1 can be fastened by snapping the box body 2 and the cover 3 together, and can easily remove the cover 3 from the box body 2 after the cover 3 is once mounted on the box body 2 by using the organic silicone having the above-mentioned specific SOx group as the sealing material 4. In addition, by removing the cover 3 from the box body 2 and then installing the cover 3 on the box body 2 again, the sealing material 4 can be used to seal the two liquid-tightly.

[0109] As described above, the waterproof box 1 of this embodiment can reduce the cost of assembly work, can be reassembled, and has excellent heat resistance and waterproof performance. In addition, the waterproof box 1 of this embodiment can be placed in the engine room of a car for use.

[0110] (Implementation Method 2)

[0111] like Figure 3 As shown, the waterproof box 102 of this embodiment has a protrusion 33 protruding from the outer peripheral portion of the cover 302 and pressed into the sealing material 4. It should be noted that among the symbols used in the second embodiment and thereafter, the same symbols as those used in the above embodiment represent the same components as those in the above embodiment unless otherwise specified.

[0112] The waterproof box 102 of the present embodiment has a box body 2, a cover 302, and a sealing material 4 between the box body 2 and the cover 302. A protrusion 33 protruding toward the bottom surface 261 of the sealing material retaining groove 26 is provided at a position opposite to the sealing material retaining groove 26 in the box body 2 and the cover 302, and the protrusion 33 is preferably pressed into the sealing material 4. The protrusion 33 only needs to be arranged at a position opposite to the sealing material retaining groove 26. For example, the sealing material retaining groove 26 of the present embodiment is arranged at the front end 251 of the side wall portion 25 in the box body 2. Therefore, the protrusion 33 of the present embodiment is provided at a position opposite to the sealing material retaining groove 26 in the cover 302, that is, the sealing surface 32.

[0113] When the protrusion 33 is pressed into the sealing material 4 as in the present embodiment, the height of the portion compressed by the protrusion 33 is the height Hf of the sealing material 4 in the state of being compressed between the box body 2 and the cover 302. That is, in the present embodiment, the distance from the bottom surface 261 of the sealing material holding groove 26 to the protrusion 33 is the height Hf of the sealing material 4 in the compressed state. Other aspects are the same as those of the first embodiment.

[0114] By providing the protrusion 33 as in the present embodiment, the compression amount of the sealing material 4 can be made larger than that in the case where the protrusion 33 is not provided, and the repulsive force of the sealing material 4 can be appropriately increased. In addition, by pressing the protrusion 33 into the sealing material 4, the contact area between the protrusion 33 and the sealing material 4 can be made larger, and the formation of a gap between the protrusion 33 and the sealing material 4 can be more effectively suppressed. As a result of these, the waterproof performance of the waterproof box 102 can be further improved. In addition, the waterproof box 102 of the present embodiment can achieve the same effect as that of the first embodiment.

[0115] [Example]

[0116] (Experimental Example 1)

[0117] This example is an example of evaluating the adhesiveness of silicone gels obtained by curing various silicone compositions. In this example, first, photocurable silicone compositions (compositions A to H) having the compositions shown in Table 1 were prepared.

[0118] In addition, specifically, the compounds shown in Table 1 are as follows.

[0119] (A)Ingredients

[0120] Compound A: polydimethylsiloxane having a vinyl siloxane group at the end (viscosity at 25°C: 30,000 mm 2 / s, functional group equivalent: 26000g / eq)

[0121] (B) Ingredients

[0122] Compound B: Polythiol compound (viscosity at 25°C: 200 mm 2 / s, functional group equivalent: 1900g / eq)

[0123] (C) Ingredients

[0124] Compound C: Free radical photoinitiator (absorption peak wavelength: 244nm and 330nm)

[0125] (D) Ingredients

[0126] Compound D1: organic peroxide ("PERBUTYL I" manufactured by NOF Corporation, 10-hour half-life temperature: 98.7°C)

[0127] Compound D2: organic peroxide ("PERCURE O" manufactured by NOF Corporation, 10-hour half-life temperature: 72.1°C)

[0128] Compound D3: organic peroxide ("PERBUTYL I" manufactured by NOF Corporation, 10-hour half-life temperature: 104.3°C)

[0129] (D') Component

[0130] Compound D'1: organic peroxide ("PERCUMYL H-80" manufactured by NOF Corporation, 10-hour half-life temperature: 157.9°C)

[0131] Compound D'2: Oleic acid (reagent)

[0132] Compound D'3: Heptanoic acid (reagent)

[0133] In addition, (D') component is a comparative component with respect to (D) component.

[0134] (E) Ingredients

[0135] Filler E: Diluted hydrophobic fumed silica powder (specific surface area: 120 m 2 / g, particle size: 20nm)

[0136] Specifically, the preparation method of compositions A to H is as follows. First, components (A) to (D) and other components shown in Table 1 are weighed in a manner to obtain the mass ratio shown in Table 1, and are put into a stirring tank. Next, components (A) to (D) and other components in the stirring tank are mixed for 30 minutes while being vacuum degassed. After the mixing and vacuum degassed, component (E) is weighed in a manner to obtain the mass ratio shown in Table 1. After the weighed component (E) is put into the stirring tank, components (A) to (E) and other components in the stirring tank are mixed for 60 minutes while being vacuum degassed. In this way, compositions A to H can be obtained.

[0137] [Table 1]

[0138]

[0139] Using the obtained compositions A to H, the viscosity, structural viscosity ratio and adhesive strength were measured by the following methods.

[0140] [Determination of viscosity and structural viscosity ratio]

[0141] The viscosity and structural viscosity ratio were determined using a cone-plate type rotational viscometer (E-type viscometer) adjusted to 25°C using a circulating thermostatic bath. Take 0.5cc of composition A to H and discharge it into the center of the sample cup. The sample cup is mounted on the body of the viscometer, and the composition A to H is sandwiched between the cone plate of 3°×R12 and the sample cup. In this state, the cone plate is rotated at a rotation speed of 1.0 rpm for 5 minutes. The viscosity at the moment of 5 minutes from the start of rotation is recorded in the "Viscosity" column of Table 2 as the viscosity of composition A to H.

[0142] In addition, the viscosity of compositions A to H was measured in the same manner as described above except that the rotation speed of the cone plate was changed to 0.5 rpm or 2.5 rpm. The value obtained by dividing the viscosity of the composition at a rotation speed of 0.5 rpm obtained in this way by the viscosity of the composition at a rotation speed of 2.5 rpm was recorded in the "Structural Viscosity Ratio" column of Table 2 as the structural viscosity ratio of compositions A to H.

[0143] [Measurement of Adhesive Strength]

[0144] In order to evaluate the adhesive force of the organic silicone obtained by curing the compositions A to H, the tensile shear bonding strength was measured according to JIS K6850:1999. The preparation method of the test pieces AA to HH (see Table 2) used in the measurement of the tensile shear bonding strength is as follows. First, prepare two sheets of coating materials made of PA66 (i.e., nylon 66) with a length of 80 mm, a width of 25 mm, and a thickness of 4 mm. Two 1.5 mm thick spacers are overlapped and attached to one of the two coating materials to form a 10 mm × 15 mm coating area surrounded by the spacers. After injecting any one of the compositions A to H into the coating area, rolling is performed to make the composition smooth and flat, so that the coating thickness of the compositions A to H is 3 mm. Thereafter, an ultraviolet irradiator equipped with an LED lamp is used to irradiate the composition with ultraviolet rays to cure the composition, thereby forming an organic silicone on the coating material. It should be noted that the central wavelength of the ultraviolet rays irradiated by the LED lamp is 365 nm. The cumulative amount of ultraviolet light irradiated on the composition was 1500 mJ / cm 2 .

[0145] After peeling off one piece of the separator from the covering material formed with the organic silica gel, the other covering material is attached to the organic silica gel. Next, the two covering materials are fixed and compressed with a clamp to make the thickness of the organic silica gel 50% of the initial thickness. After keeping the test pieces AA to HH (see Table 2) thus obtained at a temperature of 100°C in a hot air drying furnace for 300 hours, the test pieces AA to HH are taken out from the hot air drying furnace. After the test pieces are cooled to room temperature, the clamps are removed.

[0146] Using the heated test pieces AA to HH, a tensile test was performed in accordance with JIS K6850:1999. It should be noted that the crosshead speed of the tensile tester was 5 mm / min. The maximum strength in the tensile test is shown in the "Tensile Shear Adhesion Strength" column of Table 2. In addition, the state of the fracture surface was evaluated by visually observing the organic silicone after the tensile test. In the "Fracture State" column of Table 2, when the entire bonding surface is a cohesive fracture, it is recorded as "A", and when the bonding surface includes a cross-sectional fracture, it is recorded as "B".

[0147] [Table 2]

[0148]

[0149] As shown in Table 2, the silicone rubber formed by curing compositions A to D has a higher tensile shear bonding strength than the silicone rubber formed by curing compositions E to H. In addition, the entire bonding surface of the silicone rubber formed by curing compositions A to D underwent cohesive fracture, whereas a portion of the bonding surface of the silicone rubber formed by curing compositions E to H underwent cross-sectional fracture. Based on these results, it can be understood that when a photocurable silicone composition is cured using ultraviolet rays with lower energy using an LED lamp as a light source, the photocurable silicone composition containing component (D) can improve the adhesion of the silicone rubber compared to a photocurable silicone composition not containing component (D).

[0150] Although not shown in the table, the tensile shear adhesive strength of the silicone rubber obtained by curing composition A at 100°C for 24 hours was 0.28 MPa. From this result, it can be understood that the tensile shear adhesive strength can be increased by increasing the heating time.

[0151] Furthermore, after the compositions A and D were stored at 25°C for one month, the viscosity of the composition A became 473 Pa·s, and the viscosity of the composition D became 549 Pa·s. Comparison of these viscosity values ​​with the initial viscosity values ​​shown in Table 1 shows that the viscosity of the compositions A and D changed little during storage and had sufficient storage stability.

[0152] (Experimental Example 2)

[0153] In this example, the adhesiveness of the organic silicone rubber was evaluated when the coating material was PBT (ie, polybutylene terephthalate). The method for preparing the test piece in this example is as follows.

[0154] <Test piece II>

[0155] The method for preparing the test piece II was the same as the method for preparing the test piece AA in Experimental Example 1, except that the material of the coating material was changed to PBT.

[0156] <Test piece JJ>

[0157] The method for preparing test piece JJ was the same as the method for preparing test piece II, except that composition E was used instead of composition A as the photocurable silicone composition and composition E was cured using an ultraviolet irradiator equipped with a high-pressure mercury lamp. It should be noted that the cumulative light intensity of ultraviolet rays irradiated by the high-pressure mercury lamp in the method for preparing test piece JJ was 4500 mJ / cm 2 .

[0158] <Test piece KK>

[0159] The method for preparing the test piece KK was the same as the method for preparing the test piece EE in Experimental Example 1, except that the material of the coating material was changed to PBT.

[0160] The tensile test was carried out using the test pieces II to KK obtained above under the same conditions as those in Experimental Example 1, and the tensile shear adhesive strength of each test piece was measured.

[0161] The tensile shear bond strengths of test pieces II to KK are shown in Figure 4 It should be noted that Figure 4 The vertical axis is the tensile shear bonding strength (MPa). In the test pieces II and JJ, the entire bonding surface was cohesively fractured inside the silicone rubber by the tensile test. On the other hand, in the test piece KK, a portion of the bonding surface was fractured in the cross section between the silicone rubber and the covering material by the tensile test.

[0162] like Figure 4 As shown, the tensile shear bonding strength of the silicone rubber in the test pieces II and JJ is higher than the tensile shear bonding strength of the silicone rubber in the test piece KK. In addition, the test piece II in which the oxidation of the SH group and the thioether group in the silicone rubber is promoted by the oxidant shows a higher tensile shear bonding strength than the test piece KK.

[0163] (Experimental Example 3)

[0164] This example is an example of conducting a detailed investigation of the chemical state of S atoms in organic silica gel by X-ray absorption fine structure analysis using radiation light. In this example, first, a test piece LL simulating the test piece AA in Experimental Example 1 and a test piece MM simulating the test piece AA before heating were prepared. The specific method of preparing the test pieces LL and MM is as follows.

[0165] <Test piece LL>

[0166] Composition A is applied on a substrate made of PBT. The coating thickness of composition A is 10 μm. Next, composition A applied on the substrate is irradiated with ultraviolet light using an LED lamp as a light source under the same conditions as test piece AA, thereby curing composition A to form an organic silica gel. The cured organic silica gel is heated together with the substrate at a temperature of 100° C. for 300 hours. Thereafter, the organic silica gel is separated from the substrate. The organic silica gel obtained by heating the organic silica gel obtained above, that is, the cured product of composition A, is used as test piece LL.

[0167] <Test piece MM>

[0168] The method for preparing the test piece MM was the same as the method for preparing the test piece LL, except that the silicone rubber was not heated after the composition A was cured to prepare the silicone rubber.

[0169] The chemical state of the S atoms in the organic silica gel in the test pieces LL and MM obtained above was analyzed by hard X-ray XAFS (X-ray absorption edge fine structure method). Specifically, the test pieces LL and MM were irradiated with X-rays obtained by splitting the radiation light, and the absorption spectrum near the X-ray absorption edge of the S atoms was obtained. Then, based on the obtained absorption spectrum, the X-ray absorption fine structure of the S atoms in the organic silica gel was analyzed. Figure 5 ] The X-ray absorption spectra of the test pieces LL and MM are shown in FIG. Figure 5 The vertical axis is the standardized absorption intensity, and the horizontal axis is the energy of the incident light (eV).

[0170] in addition, Figure 5 The positions of absorption peaks of S atoms derived from SH groups, S atoms derived from SO groups, S atoms derived from SO2 groups, and S atoms derived from SO3 groups are shown in . These peak positions are determined based on the absorption spectrum near the X-ray absorption edge of the aforementioned reference sample having each functional group.

[0171] The X-ray absorption spectrum was obtained at the Aichi Synchrotron Optical Center Aichi SR Beamline BL6N1. The detection method was the fluorescence yield method, and the K-terminus of the S atom was measured. The beam diameter of the incident X-ray was 2.00 mm × 1.00 mm.

[0172] like Figure 5 As shown, in the X-ray absorption spectra of the test pieces LL and MM, an absorption peak with a vertex appears near 2475 eV, and an absorption peak with a vertex appears near 2481 eV. In addition, the absorption peak with a vertex near 2481 eV has a shoulder near 2479 eV. Based on these results, it can be understood that the organic silica gel obtained by curing the photocurable organic silicone composition containing the above-mentioned components (A) to (D) as in the test pieces AA to DD and the test pieces LL to MM has SH groups, SO2 groups and SO3 groups.

[0173] (Experimental Example 4)

[0174] This example is an example of detailed investigation of the chemical state of S atoms in the organic silica gel in the test pieces JJ and KK of Experimental Example 2 by X-ray absorption fine structure analysis using radiated light. In this example, first, a test piece NN simulating the test piece JJ in Experimental Example 2 and a test piece OO simulating the test piece KK were prepared. The specific method of preparing the test pieces NN and OO is as follows.

[0175] <Test piece NN>

[0176] Composition E was applied to a substrate made of PBT. The coating thickness of composition E was 10 μm. Next, composition E applied to the substrate was irradiated with ultraviolet light using a high-pressure mercury lamp as a light source under the same conditions as test piece JJ, thereby curing composition E to form organic silica gel. The organic silica gel was kept at a temperature of 100° C. for 300 hours in the atmosphere together with the substrate. Thus, test piece NN simulating test piece JJ was obtained.

[0177] <Test piece OO>

[0178] The method for preparing the test piece OO is the same as the method for preparing the test piece NN, except that an LED lamp is used as the light source of ultraviolet light instead of the high-pressure mercury lamp.

[0179] The chemical state of the S atoms in the organic silica gel in the test pieces NN and OO obtained above was analyzed by hard X-ray XAFS (X-ray absorption edge fine structure method). The method and conditions for obtaining the X-ray absorption spectrum in this example are the same as those in Experimental Example 3, except that the organic silica gel on the substrate is irradiated with X-rays.

[0180] Figure 6 ] The X-ray absorption spectra of S atoms in the test pieces NN and OO are shown in FIG. Figure 6 The vertical axis is the standardized absorption intensity, and the horizontal axis is the energy of the incident light (eV). Figure 6 The positions of absorption peaks of S atoms derived from SH groups, S atoms derived from SO groups, S atoms derived from SO2 groups, and S atoms derived from SO3 groups are shown in . These peak positions are determined based on the absorption spectrum near the X-ray absorption edge of the aforementioned reference sample having each functional group.

[0181] like Figure 6 As shown, in the X-ray absorption spectrum of the test piece NN, an absorption peak with a vertex appears near 2475 eV, and a larger absorption peak with a vertex appears near 2481 eV. In addition, the larger peak with a vertex near 2481 eV has a shoulder near 2479 eV. Figure 6 From the X-ray absorption spectrum shown in , it can be understood that the organic silica gel of the test piece NN, that is, the organic silica gel obtained by heating the composition E by high-pressure mercury lamp curing, has SH groups, SO2 groups, and SO3 groups.

[0182] In addition, the absorption peak of the S atom from the SH group in the test piece NN is shifted to the high energy side by about 200 meV compared with the absorption peak of the reference sample. In addition, the absorption peak of the S atom from the SO3 group is shifted to the low energy side by about 200 meV compared with the absorption peak of the reference sample. It can be inferred that the shift of these absorption peaks is caused by the hydrogen bonding of the SH group and SO3 group in the organic silica gel in the test piece NN with the polar group of the coating material. Therefore, it is believed that the test piece JJ exhibits high shear bonding strength through hydrogen bonding of the SO3 group in the organic silica gel with the polar group of the coating material.

[0183] On the other hand, in the X-ray absorption spectrum of the test piece OO, no peaks indicating the presence of SH groups and SOx groups appeared.

[0184] Based on the above results, it can be understood that even if the photocurable silicone composition does not contain the above-mentioned component (D), SOx groups can be formed in the silicone by heating the obtained silicone after curing the silicone composition using high-energy energy rays such as ultraviolet rays irradiated by a high-pressure mercury lamp.

[0185] (Reference example)

[0186] This example is an example of evaluating the waterproof performance using a test body simulating the above-mentioned waterproof box. In this example, first, a waterproof box 102 having the same method as that of Embodiment 2 is prepared. It should be noted that the material of the box body 2 and the cover 3 is PA66. The width of the sealing material holding groove 26 provided in the box body 2 is 4.0 mm and the depth is 2.2 mm. In addition, a protrusion 33 with a height of 1.5 mm is formed on the cover 302.

[0187] The sealing material 4 made of organic silicone obtained by curing the composition E is arranged in the sealing material retaining groove 26 .

[0188] The silicone composition was applied with a width of 3.0 mm and a height of 1.7 ± 0.2 mm. The silicone composition was then irradiated with a cumulative light intensity of 4500 mJ / cm 2 The light of 400° is applied to cure the organic silicon composition to form the sealing material 4. The coating width and coating height Hi of the sealing material 4 are the same as the coating width and coating height of the organic silicon composition.

[0189] Thereafter, the cover 302 was attached to the box body 2 by locking the engagement convex portion 23 to the receiving portion 31 while pressing the protrusion 33 into the sealing material 4. Thus, the test body R1 was prepared. The height Hf of the sealing material 4 in the test body R1 with the protrusion 33 pressed in was 0.4±0.2 mm.

[0190] In this example, for comparison with the test body R1, a test body R2 having the same structure as the conventional waterproof box 102 was prepared. Although not shown in the figure, the test body R2 has an O-ring as a sealing material 4 interposed between the box body 2 and the cover 302, and has a structure in which the box body 2 and the cover 302 are fastened by bolts as fastening members.

[0191] In this example, for comparison with the test body R1, the test body R3 was prepared in which the sealing material 4 in the test body R1 was replaced with an O-ring. However, the repulsive force from the O-ring is much higher than that of the sealing material 4 made of organic silicone. Therefore, during the process of pressing the cover 302 into the box body 2, the cover 302 was deformed at a time when the compression rate of the O-ring was about 50%, and the cover 302 and the box body 2 could not be sealed liquid-tightly.

[0192] The test bodies R1 and R2 having the above structures were pressurized in such a way that the internal pressure of the containing space reached 10 kPa. Furthermore, the test bodies were kept at a temperature of 130°C and subjected to a high temperature placement test. In addition, a cold and hot cycle test was performed separately from the high temperature placement test as follows: a cycle of repeatedly keeping the test body at a temperature of -30°C for 30 minutes and then at a temperature of 100°C for 30 minutes was repeated.

[0193] In the high temperature storage test, all test bodies maintained the internal pressure before the start of the test when the holding time reached 187.5 hours. In addition, in the thermal cycle test, all test bodies maintained the internal pressure before the start of the test when the number of cycles reached 600.

[0194] Based on these results, it can be understood that the test body R1 has a waterproof performance equal to or better than that of the conventional waterproof box 102 using an O-ring. In addition, by using organic silicone having a SOx group such as the test pieces AA to DD in Experimental Example 1 and the test pieces II to JJ in Experimental Example 2 as the sealing material 4 in the test body R1, it can be expected that the sealing material 4 will be more strongly bonded to the box body 2 and the cover 302, and the waterproof performance of the waterproof box 102 will be further improved.

[0195] The present invention is not limited to the above-mentioned embodiments, and can be used in various embodiments without departing from the gist thereof. For example, in Embodiments 1 and 2, examples are shown in which the engaging protrusion 23 is provided on the box body 2 and the receiving portion 31 is provided on the cover 3, 302, respectively. The receiving portion can be provided on the box body 2, and the engaging protrusion can be provided on the cover 3, 302. In addition, the engaging protrusion can be provided on the box body 2 and the cover 3, 302, respectively, and the receiving portion can be provided in a manner corresponding to these engaging protrusions.

[0196] The structure of the engaging protrusion 23 and the receiving portion 31 is not limited to the method of the first and second embodiments, and a structure that can realize so-called snap fit can be adopted. For example, the engaging protrusion can be locked to the receiving portion by pressing a pin as the engaging protrusion into a hole as the receiving portion.

[0197] The sealing material holding groove 26 may be provided in the box body 2. That is, the sealing material 4 may be directly arranged at the front end 251 of the side wall 25, and the sealing surface of the cover 3 may compress the sealing material 4.

[0198] Alternatively, the cover portion 3 may be provided with a sealing material holding groove, and the sealing material 4 may be arranged in the sealing material holding groove.

[0199] The sealing material 4 in the waterproof box 1, 102 may be composed of one kind of organic silicone. In this case, for example, a single organic silicone composition may be applied to the portion of the box body 2 and the cover 3, 302 where the sealing material 4 is to be provided, and then the organic silicone composition may be cured to form the sealing material 4 composed of a single kind of organic silicone.

[0200] In addition, the sealing material 4 may contain two or more kinds of silicone. In this case, for example, the sealing material 4 composed of two or more kinds of silicone can be formed by coating the parts of the box body 2 and the cover 3, 302 where the sealing material 4 is to be set with silicone compositions of different compositions, respectively, and then curing these silicone compositions. In the sealing material 4 containing two or more kinds of silicone, the combination of silicone is not particularly limited. For example, the sealing material 4 may contain two or more silicones selected from silicone having an SO group and having adhesiveness, silicone having an SO2 group and having adhesiveness, silicone having an SO3 group and having adhesiveness, silicone having an SO and SO2 group and having adhesiveness, silicone having an SO and SO3 group and having adhesiveness, silicone having an SO2 group and an SO3 group and having adhesiveness, silicone having an SO2 group and an SO3 group and having adhesiveness and an SO group, silicone having an SO2 group and an SO3 group and having adhesiveness.

[0201] In addition, although the examples of using the photocurable silicone composition and the silicone rubber for the sealing material of the waterproof box are shown in Embodiments 1 and 2, the use of the photocurable silicone composition and the silicone rubber is not limited to the sealing material of the waterproof box.

Claims

1. A waterproof box for automobile, having the following structure: The box body has a receiving space for receiving the received object and an opening connected to the receiving space; A cover portion, mounted on the box body portion and closing the opening; A sealing material, which is composed of an organic silica gel having at least one SOx group selected from SO group, SO2 group and SO3 group and having adhesiveness and is interposed between the box body and the cover; A receiving portion, provided on at least one of the box body and the cover; as well as The engaging convex part is provided at a position corresponding to the receiving part in the box main body part and the cover part, and is locked in the receiving part. The organic silica gel is a cured product of a photocurable organic silicone composition, wherein the photocurable organic silicone composition comprises a mercapto-based crosslinking agent having an SH group and an oxidizing agent capable of oxidizing the SH group and the thioether group. The oxidant is an organic peroxide having a 10-hour half-life temperature of 150° C. or less.

2. The automotive waterproof box according to claim 1, wherein: At least one of the case body and the cover is made of resin.

3. The automotive waterproof box according to claim 1, wherein: Either the box body or the cover is provided with a sealing material holding groove having a bottom surface and a side surface connected to the bottom surface, and the sealing material is arranged on the bottom surface with a gap between the sealing material and the side surface.

4. The automotive waterproof box according to claim 3, wherein: A protrusion that protrudes toward the bottom surface is provided at a position of the box body and the cover that faces the sealing material holding groove, and the protrusion is pressed into the sealing material.

5. The automotive waterproof box according to claim 1, wherein: The sealing material is compressed between the box body and the cover so that a height Hf of the compressed state reaches 40 to 80% of a height Hi of the uncompressed state.

6. The automotive waterproof box according to claim 1, which is used in an engine room of an automobile.

7. A photocurable silicone composition comprising the following components A to D, which are configured to form a silicone gel having at least one SOx group selected from the group consisting of a SO group, a SO2 group and a SO3 group, Component A: polyorganosiloxane having a vinyl siloxane group, Component B: mercapto crosslinking agent, Component C: free radical photoinitiator, Component D: an organic peroxide having a 10-hour half-life temperature of 150°C or less.

8. The photocurable silicone composition according to claim 7, wherein: The component B is contained in an amount of 0.1 to 10 parts by mass, the component C is contained in an amount of 0.1 to 5.0 parts by mass, and the component D is contained in an amount of 0.1 to 5.0 parts by mass, based on 100 parts by mass of the component A.

9. The photocurable silicone composition according to claim 7, wherein: The component D is an organic peroxide having a peroxyester structure.

10. The photocurable silicone composition according to claim 9, wherein: The D component has a molecular structure represented by the following general formula (1) or the following general formula (2), R 1 -O-O-C-O-R 2 ···Tokyo (1), R 3 -O-O-CO-O-R 4 ...Tokyo (2), Wherein, R in the general formula (1) and the general formula (2) 1 ~R 4 Each is independently a substituted or unsubstituted aromatic group, a hydrocarbon group selected from an aliphatic hydrocarbon group and an unsaturated hydrocarbon group.

11. The photocurable silicone composition according to claim 7, wherein: The 10-hour half-life temperature of the D component is 60 to 110°C.

12. The photocurable silicone composition according to claim 7, wherein: Furthermore, a filler is contained as the E component.

13. An organic silica gel obtained by curing the photocurable organic silica composition according to any one of claims 7 to 12, the organic silica gel having at least one SOx group selected from the group consisting of a SO group, a SO2 group and a SO3 group.