Gating tube material, gating tube unit and preparation method, memory structure
By using gate materials doped with oxides, nitrides, and carbides with elements such as Te, Se, and S, the problems of complex composition, high toxicity, and slow switching speed of gate materials in the existing technology are solved, and high turn-on is achieved. current, low leakage current and fast switching speed, suitable for high-density three-dimensional information storage.
Patent Information
- Application Number
- CN202010975902.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-09-16
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-09-16
AI Technical Summary
The existing gate materials have complex composition, contain toxic substances, slow switching speed, small turn-on current, large leakage current, small gate ratio, and poor fatigue performance, which limits their application in new phase change memory devices.
Te, Se and S are used as the main elements, doped with oxides, nitrides and carbides, and the gate material is prepared through a magnetron sputtering process to achieve an instantaneous transition from a high resistance state to a low resistance state, and by optimizing the material composition Increase turn-on current, reduce leakage current, and enhance thermal stability and repeatability.
It achieves high opening current, low leakage current, fast switching speed and good repeatability of the gate material, solves the problems of simple materials, non-toxicity and insufficient performance in the existing technology, and is suitable for high-density three-dimensional information storage.
Smart Images

Figure CN113571635B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of micro-nano electronics technology, and specifically relates to a gate tube material, a gate tube unit and its preparation method, and a memory structure. Background Technology
[0002] With the gradual popularization of 5G and the booming development of emerging technologies such as VR and autonomous driving, higher demands are being placed on data storage speed and capacity. As a result, novel non-volatile storage materials, such as phase-change memory materials, have come into focus. Currently, existing data storage technologies have reached the sub-nanometer size limit. To achieve even greater unit storage capacity, it is necessary to use cross-type stacked arrays to break through the capacity limitations of dimensional storage.
[0003] A gating device with good switching performance is needed to select memory cells. A gating transistor uses an electrical signal to control the switch of the gating device. When an electrical signal is applied to the gating device cell, the material transitions from a high-resistance state to a low-resistance state, and the device is in the on state; when the electrical signal is removed, the material transitions back from a low-resistance state to a high-resistance state, and the device is in the off state. Existing gating transistors include omonic threshold switches (OTS), conductive bridge threshold switches, and metal-insulator transition switches.
[0004] However, existing gate transistors (such as OTS) have complex material compositions, evolving from binary to pentads and even hexaads. Furthermore, these complex OTS materials contain toxic substances such as aspartate (As), which is detrimental to sustainable development. Additionally, the switching speeds of these gates are in the microsecond range and above, limiting their application in novel phase-change memory devices. Moreover, there is also the issue of the turn-on current I... on Small leakage current I off Large, small gating ratio (I) on / I off Small size, poor fatigue performance, etc.
[0005] Therefore, it is necessary to provide a selection transistor material, selection transistor unit, and memory structure to solve the above-mentioned problems in the prior art. Summary of the Invention
[0006] In view of the shortcomings of the prior art described above, the purpose of this invention is to provide a selection tube material, a selection tube unit, and a memory structure to solve the problems of complex material composition, high material toxicity, low turn-on current, high leakage current, low selection ratio, and poor fatigue performance in the prior art.
[0007] To achieve the above and other related objectives, the present invention provides a channeling tube material, wherein the channeling tube material comprises at least one of Te, Se, and S:
[0008] Optionally, the chemical formula of the selection tube material is (Te x Se y S z ) 1-t M t Where M includes doped materials, and 0≤x≤100, 0≤y≤100, 0≤z≤100, 0 <t≤0.5。
[0009] Optionally, the doping material includes at least one of O, N, Ga, In, and As.
[0010] Optionally, the doped material includes at least one of oxides, nitrides, and carbides.
[0011] Optionally, the oxide includes at least one of SiOx, TiOx, TaOx, HfOx, TiOx, GeOx, SnOx, AlOx, and GaOx; and / or, the nitride includes at least one of SiNx, GeNx, AlNx, and SnNx; and / or, the carbide includes at least one of SiCx, GeCx, and AlCx.
[0012] Optionally, the gate material has nonlinear conductivity characteristics to serve as a neuron device for neural networks.
[0013] Optionally, the gate material has bidirectional threshold switch-type gate characteristics.
[0014] Optionally, the selector material can achieve an instantaneous transition from a high-resistance state to a low-resistance state when the voltage is applied to a preset value, and spontaneously return to a high-resistance state instantaneously when the electrical signal is removed.
[0015] Optionally, the instantaneous transition time of the selector tube material from a high-resistivity state to a low-resistivity state is between 100 ps and 1 μs, and the instantaneous transition time from a low-resistivity state to a high-resistivity state is between 500 ps and 5 μs.
[0016] Optionally, when the gate material is in a high-resistivity state, the gate material includes an amorphous or crystalline state; when the gate material is in a low-resistivity state, the gate material includes an amorphous, crystalline, or molten state.
[0017] In addition, the present invention also provides a gate tube unit, the gate tube unit comprising:
[0018] The channel material layer includes the channel material as described in any of the above embodiments;
[0019] The first electrode is located on the upper surface of the selector tube material layer;
[0020] The second electrode is located on the lower surface of the selection tube material layer;
[0021] Alternatively, the gate unit may include:
[0022] The channel material layer includes the channel material as described in any of the above embodiments;
[0023] The first electrode and the second electrode are located on the upper or lower surface of the selection tube material layer, forming a transverse structure.
[0024] Optionally, the shape of the second electrode includes T-type, μ-type, partially or fully defined type.
[0025] Optionally, the thickness of the channel material layer is between 2nm and 100nm.
[0026] Optionally, the turn-on current of the selector unit is greater than or equal to 10. -4 A, the leakage current of the selected transistor unit is less than or equal to 10. -5 A, the number of cycles of the selector unit is greater than or equal to 10. 3 Second-rate.
[0027] As an example, the on / off current ratio of the selected transistor unit is between 1 and 8 orders of magnitude.
[0028] The present invention also provides a method for fabricating a gate tube unit, comprising the steps of: providing a substrate, and fabricating a first electrode, a second electrode and a gate tube material layer on the substrate, wherein the gate tube material layer is fabricated based on a magnetron sputtering process.
[0029] In addition, the present invention also provides a memory structure, the memory structure comprising:
[0030] The selection tube unit as described in any of the above schemes;
[0031] A storage material layer is located on the lower surface of the second electrode;
[0032] The third electrode is located on the lower surface of the storage material layer.
[0033] Optionally, the storage material layer includes any one of a phase change storage material layer, a resistive switching storage material layer, a magnetic storage material layer, and a ferroelectric storage material layer.
[0034] Optionally, the storage device structure includes a plurality of parallel-spaced first electrodes and a plurality of parallel-spaced third electrodes, wherein the first electrodes extend along a first direction, the third electrodes extend along a second direction, and the first direction and the second direction form an angle less than 0° and greater than or equal to 90°; the gate material layer, the second electrodes, and the storage material layer together constitute a gated storage unit, and the storage device structure includes a plurality of such gated storage units, wherein the gated storage units are located in the overlapping area of the first electrodes and the third electrodes.
[0035] Optionally, the gate material layer, the second electrode, and the storage material layer each comprise at least N layers, stacked in the vertical direction to form an N-layer structure, resulting in a memory structure with a storage density of 4F. 2 / N, to achieve massive storage, where F is the semiconductor process feature size and N is an integer greater than or equal to 2.
[0036] As described above, the gate material, gate unit, and memory structure of the present invention utilize Te, Se, and S elements or compounds composed of any of these elements as the gate material. Performance can be improved by incorporating elements such as O, N, Ga, In, and As, as well as oxides, nitrides, and carbides. The threshold voltage, turn-on current, and fatigue characteristics of the gate unit made from this material can be adjusted and optimized. This improves the thermal stability of the gate unit, reduces leakage current, and enhances repeatability. When used in gate units, it offers advantages such as high turn-on current, simple materials, fast switching speed, good repeatability, and low toxicity, contributing to the realization of high-density three-dimensional information storage. Attached Figure Description
[0037] Figure 1 The image shown is a cross-sectional view of an example of a selector tube unit provided in an embodiment of the present invention.
[0038] Figure 2 The diagram shown is a cross-sectional view of an example memory structure provided in an embodiment of the present invention.
[0039] Figure 3 The diagram shown is a partial top view of the memory structure provided in an embodiment of the present invention.
[0040] Figure 4 The voltage-current curve of the selector unit in Embodiment 1 of the present invention is shown.
[0041] Figure 5 The image shows the pulse test curve of the selector unit in Embodiment 1 of the present invention.
[0042] Figure 6 The voltage-current curve of the selector unit in Embodiment 2 of the present invention is shown.
[0043] Component designation explanation
[0044] 10. Selective Pipe Material Layer
[0045] 11 First Electrode
[0046] 12 Second Electrode
[0047] 13 Storage Material Layer
[0048] 14 Third Electrode Detailed Implementation
[0049] The following specific examples illustrate the implementation of the present invention. Those skilled in the art can easily understand other advantages and effects of the present invention from the content disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and various details in this specification can also be modified or changed based on different viewpoints and applications without departing from the spirit of the present invention.
[0050] In the detailed description of embodiments of the present invention, for ease of explanation, the cross-sectional views illustrating the device structure may be partially enlarged and not to scale. Furthermore, the schematic diagrams are merely examples and should not limit the scope of protection of the present invention. In actual fabrication, the three-dimensional spatial dimensions of length, width, and depth should be included.
[0051] For ease of description, spatial relation terms such as "below," "below," "less than," "below," "above," and "upper" may be used herein to describe the relationship between one element or feature shown in the accompanying drawings and other elements or features. It will be understood that these spatial relation terms are intended to include directions other than those depicted in the drawings for devices in use or operation. Furthermore, when a layer is referred to as being "between" two layers, it can be the only layer between the two layers, or there may be one or more layers in between. Additionally, the term "between" as used in this invention includes both endpoint values.
[0052] In the context of this application, the structure described above the first feature may include embodiments in which the first and second features are formed in direct contact, or embodiments in which additional features are formed between the first and second features, such that the first and second features may not be in direct contact.
[0053] It should be noted that the illustrations provided in this embodiment only schematically illustrate the basic concept of the present invention. Therefore, only the components related to the present invention are shown in the illustrations, rather than being drawn according to the number, shape, and size of the components in actual implementation. The type, quantity, and ratio of each component in actual implementation can be arbitrarily changed, and the component layout type may also be more complex.
[0054] The present invention provides a strobing tube material, which includes at least one of Te, Se, and S. The strobing tube material is composed of at least one element of Te (tellurium), Se (selenium), and S (sulfur). That is, the strobing tube material can be Te, Se, and S单质, or a mixture of any two of them, or a mixture of the three elements. When this material is used in the strobing tube unit, it has the advantages of large on-current, small leakage current, good thermal stability, simple material, non-toxicity, and fast switching speed.
[0055] In one example, the chemical general formula of the strobing tube material is Te a Se b S c , where 0 ≤ a ≤ 1, 0 ≤ b ≤ 1, 0 ≤ c ≤ 1, and a + b + c = 1. a, b, and c are the atomic percentages of the elements. In a preferred example, such as pure Te, it has the advantages of simple material, large on-current, long device life, good performance consistency, and can work normally in a high-temperature environment from room temperature to 400 °C. In a preferred example, adding Se to Te will further increase the bandgap width, reduce the device leakage conductance, and increase the device switching ratio. At the same time, since the melting point of Se is only about 250 °C, the energy required for melting is reduced, thus reducing the operating power consumption. For example, the specific design can be Te80Se20, Te50Se50, Te20Se80.
[0056] As an example, the chemical general formula of the strobing tube material is (Te x Se y S z ) 1-t M t , where M includes a doping material, and 0 ≤ x ≤ 100, 0 ≤ y ≤ 100, 0 ≤ z ≤ 100, 0 < t ≤ 0.5. t is the atomic percentage of the doping material in the strobing tube material. For example, t can be 0.05, 0.1, 0.15, 0.2, 0.25, 0.3, 0.4, etc.
[0057] In one example, the doping material includes at least one of O, N, Ga, In, and As; that is, the doping material can be any one of O, N, Ga, In, and As, or a combination of at least two of the above elements. The doping content does not exceed 50 at.%, for example, it can be 20 at.%, 30 at.%, 40 at.%, etc. After doping, the device performance of the material will be improved, including improved thermal stability, increased on-state current, reduced leakage current, increased on / off ratio, and extended device lifetime. In this example, doping the above elements into the gate material can adjust and optimize the threshold voltage, on-state current, and fatigue characteristics of the gate unit made of the gate material, resulting in increased on-state current, increased gate ratio, and better cycle performance.
[0058] As an example, the doping material includes at least one of oxides, nitrides, and carbides. The doping material can be any one of oxides, nitrides, and carbides, or a combination of any two or three of them. After doping, it has the effects of improving thermal stability, increasing on-state current, reducing leakage current, increasing the on / off ratio, and extending device lifespan.
[0059] As an example, the oxide includes at least one of SiOx, TiOx, TaOx, HfOx, TiOx, GeOx, SnOx, AlOx, and GaOx.
[0060] As an example, the nitride includes at least one of SiNx, GeNx, AlNx, and SnNx.
[0061] As an example, the carbide includes at least one of SiCx, GeCx, and AlCx.
[0062] Wherein, "and / or" indicates that the three doping materials can be selected simultaneously, or any one of them can be selected, or any two of them can be selected. For example, the design of the present invention can be Te80(SiO2)20, Te50(SiO2)50, Se80(SiN)20, Se50(SiN)50, S80(SiC)20, and S50(SiC)50.
[0063] As an example, the selector material obtained by the present invention can achieve an instantaneous transition from a high-resistance state (off state) to a low-resistance state (on state) when a voltage is applied to a preset value (threshold voltage), and spontaneously return to the high-resistance state (off state) instantaneously when the electrical signal is removed.
[0064] In a further example, the instantaneous transition time of the gate material from a high-resistivity state to a low-resistivity state is between 100 ps and 1 μs, and the instantaneous transition time from a low-resistivity state to a high-resistivity state is between 500 ps and 5 μs. The instantaneous transition time of the gate material varies depending on the chemical formula of the constituent elements of this invention. The instantaneous transition time from a high-resistivity state to a low-resistivity state in this invention can be 100 ps, 1 ns, 10 ns, or 1 μs, and the instantaneous transition time from a low-resistivity state to a high-resistivity state can be 500 ps, 5 ns, 50 ns, or 50 μs.
[0065] As an example, in the material design of this invention, when the gate material is in a high-resistivity state, the gate material includes an amorphous or crystalline state. The high-resistivity state in the amorphous state utilizes the electron transport mechanism, resulting in fast switching speeds. The high-resistivity state in the crystalline state can avoid material crystallization caused by high-temperature downstream processes, thus preventing device failure. When the gate material is in a low-resistivity state, the gate material includes an amorphous, crystalline, or molten state. The different states of the material can be controlled and adjusted by the material growth temperature and thickness.
[0066] As an example, the gate material has nonlinear conductivity characteristics and can be used as a neuron device or a neural synapse device to realize functions such as converting external analog signals into pulse signals for use in neural networks.
[0067] As an example, the selector material exhibits bidirectional threshold switch-type gating characteristics. It can be used as a bidirectional threshold switch (OTS). The basic principle of an OTS selector is to use an electrical signal to control the switching of the gating device. When the applied electrical signal is higher than the threshold voltage, the material transitions from a high-resistance state to a low-resistance state, at which point the device is in the on state; when the electrical signal is removed, the material transitions back from a low-resistance state to a high-resistance state, and the device is in the off state. Based on the above material design, this invention can obtain an OTS. The OTS material possesses bidirectional gating characteristics, which can meet the MA / cm requirements of phase-change memory. 2 The on-state current density is crucial for achieving high-density three-dimensional integration of memory. However, existing OTS materials have complex compositions, including toxic substances such as aspartate (As), which hinders sustainable development. Other types of gates currently cannot meet the MA / cm² requirements for driving phase-change memories. 2 The current density of these gates is limited. Furthermore, the switching speed of these gates is in the microsecond range and above, which restricts their application in novel phase-change memory devices. The gate material of this invention solves the above-mentioned problems of OTS, possessing advantages such as large turn-on current, low leakage current, good thermal stability, simple material, non-toxicity, and fast switching speed.
[0068] As an example, the on / off current ratio (i.e., the gate ratio) of the gate material can include 1 to 8 orders of magnitude, for example, it can be 2, 3, or 6 orders of magnitude.
[0069] In addition, such as Figure 1 As shown, the present invention also provides a gate tube unit, the gate tube unit comprising: a gate tube material layer 10, a first electrode 11, and a second electrode 12. Wherein:
[0070] The gate material layer 10 includes the gate material as described in any of the above embodiments, that is, the gate material layer 10 is a material layer made of the gate material as described in any of the above embodiments; for the specific composition of the gate material layer 10, please refer to the specific description of the gate material above, which will not be repeated here.
[0071] The first electrode 11 is located on the upper surface of the gate tube material layer 10; the second electrode 12 is located on the lower surface of the gate tube material layer 10. Alternatively, both the first electrode 11 and the second electrode 12 may be located on the upper surface of the gate tube material layer 10 or both may be located on the lower surface of the gate tube material layer 10, forming a transverse structure.
[0072] As an example, the shape of the second electrode includes T-type, μ-type, partially or fully defined type.
[0073] As an example, the gate material layer 10 can be formed by, but is not limited to, magnetron sputtering. For elemental materials such as Te, Se, and S, single-target sputtering is used; for mixtures of at least two elements, co-sputtering with alloy targets or elemental targets can be used; doping can be achieved by alloy targets or co-sputtering with compound targets.
[0074] As an example, the thickness of the gate material layer 10 can be set according to actual needs. Preferably, the thickness of the gate material layer 10 can be 2nm-100nm. More preferably, in this embodiment, the thickness of the gate material layer 10 is 5nm-20nm, for example, 10nm or 15nm.
[0075] As an example, the first electrode 11 can be formed on the upper surface of the gate material layer 10 using any one of the following methods: sputtering, evaporation, chemical vapor deposition (CVD), plasma-enhanced chemical vapor deposition (PECVD), low-pressure chemical vapor deposition (LPCVD), metal compound vapor deposition (MOCVD), molecular beam epitaxy (MBE), atomic vapor deposition (AVD), or atomic layer deposition (ALD).
[0076] As an example, the second electrode 12 can be formed on the lower surface of the gate tube material layer 10 using any one of the following methods: sputtering, evaporation, chemical vapor deposition (CVD), plasma-enhanced chemical vapor deposition (PECVD), low-pressure chemical vapor deposition (LPCVD), metal compound vapor deposition (MOCVD), molecular beam epitaxy (MBE), atomic vapor deposition (AVD), or atomic layer deposition (ALD).
[0077] As an example, the material of the first electrode 11 may include, but is not limited to, at least one of Ti (titanium), TiN (titanium nitride), Ag (silver), Au (gold), Cu (copper), Al (aluminum), and W (tungsten). The material of the second electrode 12 may include, but is not limited to, at least one of Ti, TiN, Ag, Au, Cu, Al, and W.
[0078] As an example, a transition layer (not shown) may be provided between the first electrode 11 and the gate material layer 10. In this case, the transition layer is located on the upper surface of the gate material layer 10, and the first electrode 11 is located on the upper surface of the transition layer. The material of the transition layer may include, but is not limited to, TiN (titanium nitride), and the transition layer is used to increase the adhesion between the first electrode 11 and the gate material layer 10. The thickness of the transition layer can be set according to actual needs; for example, the thickness of the transition layer may be, but is not limited to, 2 nm, 8 nm, or 10 nm. Of course, if the transition layer is not provided between the first electrode 11 and the gate material layer 10, the first electrode 11 can be directly formed on the upper surface of the gate material layer 10.
[0079] As an example, a transition layer (not shown) may also be provided between the second electrode 12 and the gate material layer 10. In this case, the transition layer is located on the lower surface of the gate material layer 10, and the second electrode 12 is located on the lower surface of the transition layer. The material of the transition layer may include, but is not limited to, TiN (titanium nitride), and the transition layer is used to increase the adhesion between the second electrode 12 and the gate material layer 10. The thickness of the transition layer can be set according to actual needs; for example, the thickness of the transition layer may be, but is not limited to, 2 nm, 8 nm, or 10 nm. Of course, if no transition layer is provided between the second electrode 12 and the gate material layer 10, the second electrode 12 can be directly formed on the lower surface of the gate material layer 10.
[0080] As an example, the turn-on current I of the selected transistor unit on ≥10 -4 A, the leakage current I of the selected transistor unit off ≤10 -5A, the number of cycles of the selector unit is greater than or equal to 10. 3 Next; preferably, in this embodiment, the turn-on current I of the selection tube unit on ≥10 -3 A, the leakage current I of the selected transistor unit off ≤10 -10 A, the number of cycles for the selector unit can be greater than or equal to 10. 7 Second-rate.
[0081] As an example, the on / off current ratio of the selector material is between 1 and 8 orders of magnitude, for example, it can be 2, 3, or 6 orders of magnitude. In addition, the selectability ratio of the selector unit can be greater than or equal to 6.
[0082] In addition, such as Figure 2-3 As shown, the present invention also provides a storage device structure, the storage device structure comprising: a selection tube unit as described in any of the above examples, a storage material layer 13, and a third electrode 14; wherein, the specific structure of the selection tube unit is described in the above examples and will not be repeated here; the storage material layer 13 is located on the lower surface of the second electrode 12; the third electrode 14 is located on the lower surface of the storage material layer 14. In this case, the first electrode 11 serves as the upper electrode, the second electrode 12 serves as the middle electrode, and the third electrode 14 serves as the lower electrode.
[0083] As an example, the thickness of the second electrode 12 can be set according to actual needs. Preferably, in this embodiment, the thickness of the second electrode 12 can include 5nm-100nm, for example, 10nm, 15nm, or 25nm.
[0084] As an example, the storage material layer 13 includes any one of a phase change storage material layer, a resistive switching storage material layer, a magnetic storage material layer, and a ferroelectric storage material layer.
[0085] As an example, the storage device structure may include a plurality of parallel-spaced first electrodes 11 and a plurality of parallel-spaced third electrodes 14, wherein the first electrodes 11 extend along a first direction and the third electrodes 14 extend along a second direction, the first direction and the second direction having an angle less than 0° and greater than or equal to 90°, for example, 45°, 60°, etc.; the gate material layer 10, the second electrode 12 and the storage material layer 13 together constitute a gated storage unit, the storage device structure includes a plurality of such gated storage units, the gated storage units are located between the first electrodes 11 and the third electrodes 14, and are located in the overlapping area of the first electrodes 11 and the third electrodes 14. It should be noted that the gating storage unit being located in the overlapping area of the first electrode 11 and the third electrode 14 means that the orthographic projection of the gating storage unit on the plane where the third electrode 14 is located is within the orthographic projection of the first electrode 11 on the plane where the third electrode 14 is located, and the orthographic projection of the gating storage unit on the plane where the first electrode 11 is located is within the orthographic projection of the third electrode 14 on the plane where the first electrode 11 is located.
[0086] As an example, the selected tube material can be three-dimensionally integrated with novel memory types such as phase-change memory, ferroelectric memory, magnetic memory, and resistive switching memory, and can be used in cross-type or vertical memory arrays with an array density of 4F. 2 (F represents the semiconductor process feature size).
[0087] In another example, the gate material layer, the second electrode, and the storage material layer each comprise at least N layers, stacked vertically to form an N-layer structure, resulting in a memory structure with a storage density of 4F. 2 / N, to achieve massive storage, where F is the semiconductor process feature size and N is an integer greater than or equal to 2.
[0088] Existing data storage technologies have reached the sub-nanometer size limit. To achieve massive storage capacity per unit, a cross-type stacked array must be used to overcome the capacity limitations of dimensional storage. However, this array structure suffers from leakage crosstalk during read and write operations, thus requiring the addition of a gate transistor to the storage cell, such as the device fabricated based on the gate transistor material of this invention. These gate transistors exhibit nonlinear conductivity characteristics, generating a large on-state current (I0) when the applied voltage reaches a threshold. ON The gate transistor is used to operate the memory cell; at half the threshold voltage, the gate transistor is in the off state, limiting the leakage current (I0) in the corresponding memory cell to be more than an order of magnitude smaller than the read / write current. OFF )pass.
[0089] To further illustrate the beneficial effects of the present invention, the following embodiments are also provided.
[0090] Example 1:
[0091] In this embodiment 1, the gate material layer 10 in the gate unit is a 20nm thick Te layer obtained by magnetron sputtering (directly sputtering with a Te target) (i.e., the gate material layer is elemental Te at this time), the second electrode 12 is an electrode with a diameter of 200nm (i.e., the device is a columnar electrode with a diameter of 200nm), and the first electrode 11 is a TiN electrode. In this example, the voltage-current curve obtained after repeated testing of the gate unit by the probe station is as follows. Figure 4 As shown (where, Figure 4 Taking the example of obtaining twenty voltage-current curves through twenty repeated tests, the data is derived from... Figure 4 It can be seen that when a voltage less than 3V is applied to the selector unit, the selector unit is in the off state, and the current through the selector unit is very small, less than 10V. -7 A; When the voltage applied to the selector unit exceeds the threshold voltage (3V~3.7V), the selector unit is instantaneously turned on, and the current through the selector unit increases sharply to 10. -3 A; When the voltage applied to the selector unit is removed, the selector unit is instantly turned off, and the current through the selector unit decreases sharply, becoming a high-resistance state. Figure 4 It can be seen that the voltage-current curves obtained from repeated tests of the selected transistor unit have consistent performance each time, which indicates that the selector unit has very good repeatability.
[0092] In addition, in this example, the gating unit obtains a curve such as the one shown after testing the pulse response using a probe station. Figure 5 As shown. By Figure 5 It can be seen that when the voltage applied to the selector unit is less than 3V, the selector unit is in the off state, and the current through the selector unit is very small; when the voltage applied to the selector unit is increased further and exceeds the threshold voltage, the selector unit is turned on instantaneously, and the current through the selector unit increases sharply. The time required to turn on the selector unit is about 40ns; when the voltage applied to the selector unit decreases to 1.5V, the selector unit is turned off instantaneously again, and the current through the selector unit decreases sharply, becoming a high-resistance state. The time required to turn off the selector unit is about 100ns, indicating that the switching speed of the selector unit is very fast.
[0093] Example 2:
[0094] In this embodiment 2, the gate material layer 10 in the gate unit is a 20nm thick Te layer obtained by magnetron sputtering (directly sputtering with a Te target) (i.e., the gate material layer 10 is elemental Te). The second electrode 12 is an electrode with a diameter of 150nm (i.e., the device is a 150nm diameter columnar electrode). Different electrode sizes result in the same current; smaller sizes result in higher current density. The first electrode 11 is a TiN electrode. The voltage-current curves obtained after repeated testing of the gate unit using a probe station in this example are shown below. Figure 6 As shown (where, Figure 6 Taking the example of obtaining four voltage-current curves through four repeated tests, the data is derived from... Figure 6 It can be seen that when a voltage less than 2V is applied to the selector unit, the selector unit is in the off state, and the current through the selector unit is very small, less than 10V. -7 A; When the voltage applied to the selector unit exceeds the threshold voltage (2V~2.8V), the selector unit is instantaneously turned on, and the current through the selector unit increases sharply to 10. -3 A; When the voltage applied to the selector unit is removed, the selector unit is instantly turned off, and the current through the selector unit decreases sharply, entering a high-resistance state. Because the device size decreases while the on-state current remains almost constant, the current density increases sharply as the device size shrinks. Therefore, this selector material has greater advantages after device miniaturization. Figure 6 It can be seen that the voltage-current curves obtained from repeated tests of the selected transistor unit have consistent performance each time, which indicates that the selector unit has very good repeatability.
[0095] In summary, the selector material, selector unit, preparation method, and memory structure of this invention utilize elemental Te, Se, and S, or compounds composed of any of these elements. Performance can be improved by incorporating elements such as O, N, Ga, In, and As, as well as dielectric materials such as oxides, nitrides, and carbides. The threshold voltage, turn-on current, and fatigue characteristics of the selector unit fabricated from this material can be adjusted and optimized. This improves the thermal stability, reduces leakage current, and enhances the repeatability of the selector unit. When used in selector units, it offers advantages such as high turn-on current, simple materials, fast switching speed, good repeatability, and low toxicity, contributing to high-density three-dimensional information storage. Therefore, this invention effectively overcomes the various shortcomings of existing technologies and possesses high industrial applicability.
[0096] The above embodiments are merely illustrative of the principles and effects of the present invention and are not intended to limit the invention. Any person skilled in the art can modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by those skilled in the art without departing from the spirit and technical concept disclosed in the present invention should still be covered by the claims of the present invention.
Claims
1. A gate tube material, characterized in that: The chemical formula of the gate tube material is (Te x Se y S z ) 1-t M t , wherein 0≤x≤100, 0≤y≤100, 0≤z≤100, x+y+z=100, 0≤t≤0.5, M is at least one of O and N, or M is at least one of oxide, nitride and carbide.
2. The gate tube material according to claim 1, characterized in that: The oxide includes at least one of SiOx, TiOx, TaOx, HfOx, TiOx, GeOx, SnOx, AlOx, and GaOx; and / or the nitride includes at least one of SiNx, GeNx, AlNx, and SnNx; and / or the carbide includes at least one of SiCx, GeCx, and AlCx.
3. The gate tube material according to claim 1, characterized in that: The gate tube material has nonlinear conductivity characteristics so as to be used as a neuron device in a neural network; and / or, the gate tube material has bidirectional threshold switch type gating characteristics.
4. The gate tube material according to any one of claims 1 to 3, characterized in that: The gate tube material can realize instantaneous transition from a high-resistance state to a low-resistance state when a voltage is applied to a preset value, and can instantaneously return to a high-resistance state when the electrical signal is removed.
5. The gate tube material according to claim 4, characterized in that: The instantaneous transition time of the gate tube material from the high resistance state to the low resistance state is between 100 ps-1 μs, and the instantaneous transition time from the low resistance state to the high resistance state is between 500 ps-5 μs.
6. The gate tube material according to claim 4, characterized in that: When the gate tube material is in a high resistance state, the gate tube material includes an amorphous state or a crystalline state; when the gate tube material is in a low resistance state, the gate tube material includes an amorphous state, a crystalline state or a molten state.
7. A gate tube unit, characterized in that: The gate tube unit includes: A gate tube material layer, a first electrode and a second electrode, wherein the gate tube material layer includes the gate tube material according to any one of claims 1 to 6, the first electrode and the second electrode are respectively located on the upper and lower surfaces of the gate tube material layer, or the first electrode and the second electrode are located on the same surface of the gate tube material layer.
8. The gate tube unit according to claim 7, characterized in that: The thickness of the gate tube material layer is between 2nm and 100nm; the shape of the second electrode includes T-type, μ-type, partially or fully defined type.
9. The gate tube unit according to any one of claims 7 to 8, characterized in that: The opening current of the gate tube unit is greater than or equal to 10 -4 A, the leakage current of the gate tube unit is less than or equal to 10 -5 A, the number of cycles of the gate tube unit is greater than or equal to 10 3 times; the on / off current ratio of the gate tube unit is between 1-8 orders of magnitude.
10. A method for preparing a gate tube unit according to any one of claims 7 to 9, characterized in that: The preparation method includes the steps of: providing a substrate, and preparing the first electrode, the second electrode and the gate tube material layer on the substrate, wherein the gate tube material layer is prepared based on a magnetron sputtering process.
11. A memory structure, characterized in that: The memory structure includes: The gate tube unit according to any one of claims 7 to 9; a storage material layer, located on the lower surface of the second electrode; The third electrode is located on the lower surface of the storage material layer.
12. The memory structure according to claim 11, wherein: The storage material layer includes any one of a phase change storage material layer, a resistive storage material layer, a magnetic storage material layer and a ferroelectric storage material layer.
13. The memory structure according to any one of claims 11 to 12, characterized in that: The storage device structure includes a plurality of first electrodes arranged in parallel and spaced apart and a plurality of third electrodes arranged in parallel and spaced apart, wherein the first electrodes extend along a first direction, the third electrodes extend along a second direction, the first direction and the second direction have an angle, and the angle is less than 0° and greater than or equal to 90°; the gate tube material layer, the second electrode and the storage material layer together constitute a gated storage unit, and the storage device structure includes a plurality of the gated storage units, and the gated storage units are located in the overlapping area of the first electrode and the third electrode.
14. The memory structure according to claim 13, wherein: The gate material layer, the second electrode and the storage material layer each include at least N layers, which are stacked in a vertical direction to form an N-layer structure. The storage density of the memory structure obtained is 4F. 2 / N to achieve mass storage, where F is the semiconductor process feature size and N is an integer greater than or equal to 2.
Citation Information
Patent Citations
Phase-varying storage layer, its making method and phase-varying storage unit
CN1996633A
Switch device, storage apparatus, and memory system
US20190252609A1