A method for preparing a split-gate trench semiconductor power device
By using a single-layer epitaxial layer and high-energy ion implantation technology in split-block trench semiconductor power devices, a high-doping concentration N-type region is formed, which solves the difficulty of achieving low on-resistance and resistance in the high-doping epitaxial layer in the prior art. The breakdown problem improves the performance-price ratio of the device and maintains the quality and reliability of the device.
Patent Information
- Application Number
- CN202110459808.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-04-27
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-04-27
AI Technical Summary
The existing split-block trench semiconductor power devices are difficult to achieve low on-resistance and avoid premature breakdown in the highly doped epitaxial layer, and the cost of the three-layer epitaxial layer is high, which affects the cost performance.
Using a single-layer epitaxial layer and high-energy ion implantation technology, an N-type region with a high doping concentration is formed on the N-type epitaxial layer. The doping concentration of a specific region is increased through high-energy ion implantation, forming a device with a lower resistance than the resistance and a breakdown resistance.
Devices with similar performance than three-layer epitaxial layers are realized, and the cost is lower, improving the performance-price ratio of the device while maintaining the quality and reliability of the device.
Smart Images

Figure CN113611598B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of semiconductor power devices, and in particular to a method for preparing a multi-groove semiconductor power device. Background Art
[0002] Gate-controlled power devices include power MOSFET (Metal-Oxide-Semiconductor Field-Effect Transistor), IGBT (Insulated Gate Bipolar Transistor), SIT (Static Induction Transistor), MCT (MOS Controlled Thyristor), MGT (Metal-Gate Transistor), etc. The above power devices have their own characteristics and application ranges.
[0003] The gate field effect power transistor (POWER MOSFET) is a unipolar carrier type device that is easy to control. Compared with bipolar transistors, it only requires very low power to control the switch, and because of its low on-resistance and high-speed switching, it can effectively control high-frequency and large currents. At present, power MOSFET has been widely used in various electronic and communication products, and is widely used in power amplifiers, power converters, low noise amplifiers, and some personal computer power supply switches, power supply circuits, etc. At the same time, it also has many applications in industry.
[0004] When power MOSFET is used as a switching device, the losses related to the device during the application process can be divided into conduction loss and switching loss. Switching loss is mainly related to the parasitic capacitance of the device, especially to the gate. Generally, there is no tail current when turning off, and there is less switching loss, so high-frequency switching can be achieved. Conduction loss is derived from the on-resistance of the device, and the on-resistance increases significantly with the increase of the device breakdown voltage. In applications of 600V to 900V, superjunction devices can provide higher unipolar carrier current density with the help of compensation structure. In applications requiring higher voltage and current, bipolar devices generally dominate. Within 200V to 600V, the choice of general or superjunction power gate field effect transistor devices will be determined by application and cost.
[0005] In the 200V range, especially in the 100V range, trench gate field effect transistors are the most common choice, which can provide the most economical and best preferred factor (FOM). Split gate devices in trench gate power MOSFETs can provide better FOM and cost performance. There are two upper and lower polysilicon regions in the trench of the split gate device. The upper polysilicon body and the trench wall are connected to the gate oxide layer. The upper polysilicon body is equivalent to the gate of a general trench device. The oxide layer between the lower polysilicon body and the trench wall is thicker than the gate oxide layer. The general thickness can be from 300 angstroms to 1000 angstroms. To 6000 Angstroms The polysilicon region at the bottom can act as a field plate, which greatly eases the electric field distribution at the PN junction between the two trenches when the general device is reverse biased. Therefore, under the same breakdown voltage requirement, the split gate POWER MOSFET type device can use an epitaxial layer with roughly the same thickness but a higher doping concentration, so the specific resistance (Specific Ron) of the split gate type device is much lower than that of the general trench device. On the other hand, in the trench, there is a dielectric layer thicker than the gate oxide layer between the upper polysilicon body and the lower polysilicon body. The potential of the lower polysilicon body is connected to the source, which can shield the bottom capacitance effect of the upper gate, greatly reducing the parasitic capacitance gate leakage charge (Qgd) of the gate. Therefore, the switching loss of the split gate type device is better than that of the general trench device.
[0006] J. Baliga applied for the first patent related to the split gate device in 1999, and related patents were subsequently filed. Existing split gate devices are all made of epitaxial layers with relatively high doping concentrations, so the specific resistance (Specific Ron) of split gate devices is much lower than that of general trench devices. There are two disadvantages to using epitaxial layers with relatively high doping concentrations: (1) It is difficult to implement the inversion region on the surface (such as the surface P-type base region of an N-channel gate field-controlled transistor) on an epitaxial layer with relatively high doping concentration; (2) The concentration of the epitaxial layer at the bottom of the trench is relatively high, which will cause premature breakdown. If an epitaxial layer with relatively low concentration is used, the on-resistance will increase.
[0007] In order to solve the above shortcomings, the prior art adopts a two-layer epitaxial layer method, that is, the epitaxial layer near the bottom of the trench is relatively light, and the doping from the surface to the bottom of the trench is relatively dense (such as Figure 1As shown). In this way, the N-type region above the bottom of the trench has a relatively high concentration, which can reduce the on-resistance without causing premature breakdown of the device. However, the disadvantage of using two epitaxial layers is that the surface inversion region (such as the surface P-type base region of the N-channel gate field-controlled transistor) is difficult to implement on the N-type region with a higher doping concentration. In order to obtain a more optimized device, there are also three epitaxial layers used to make devices. Among the three epitaxial layers, the concentration of the bottom layer near the bottom of the trench is relatively light, the doping concentration from the bottom of the trench to about 1um from the surface is relatively high, and the concentration of the top layer about 1um is relatively light. There are reports claiming that devices made with three layers of epitaxy with different doping concentrations have better performance, but the cost of three layers of epitaxy is higher, which makes the cost performance of the device worse. Different epitaxial layer device structures, the number of epitaxial layers, thickness and resistivity are as follows Fig.28 shown. Summary of the invention
[0008] In order to solve the deficiencies of the prior art, the object of the present invention is to provide a method for preparing a split-gate trench semiconductor power device, which uses a single-layer epitaxial layer and ion implantation to increase the performance of the device without affecting the quality and reliability of the split-gate trench power device.
[0009] To achieve the above object, the present invention provides a method for preparing a split-gate trench semiconductor power device, comprising the following steps:
[0010] Forming a groove on the N-type epitaxial layer by etching;
[0011] After forming a dielectric layer on the sidewalls and bottom wall of the trench, a conductive material is filled in to form a first trench;
[0012] After etching away the conductive material on the upper portion of at least one of the first-type trenches, a dielectric layer is formed on the bottom wall and side walls of the upper portion and then filled with conductive material to form a second-type trench;
[0013] forming a P-type base region, an N-type region and an N+-type source region on the N-type epitaxial layer;
[0014] A source region metal pad layer, a gate connection and a terminal region field plate are formed on the N-type epitaxial layer.
[0015] Furthermore, the step of forming a P-type base region, an N-type region and an N+ type source region on the N-type epitaxial layer further includes:
[0016] Injecting P-type dopants into the source region of the N-type epitaxial layer to form a P-type base region;
[0017] Using high energy ions to implant N-type dopants into the source region of the N-type epitaxial layer to form an N-type region;
[0018] N-type dopants are injected into the N-type epitaxial layer through an N+ mask, and diffused into the P-type base region to form an N+ type source region.
[0019] Furthermore, the energy of the high-energy ions is 400 KeV to 5 MeV, and the dose is 4e12 / cm 3 to 2e13 / cm 3 .
[0020] Furthermore, the N-type region is located below the P-type base region and between the trenches.
[0021] Furthermore, the step of using high-energy ions to implant N-type dopants into the source region of the N-type epitaxial layer to form the N-type region also includes implanting the N-type dopant more than once using high-energy ions with different energies and different doses.
[0022] Furthermore, the step of using high-energy ions to implant N-type dopants into the source region of the N-type epitaxial layer to form the N-type region is performed under the same mask as the P-type base region, so that the concentration of the N-type region is higher than that of the N-type epitaxial layer.
[0023] Furthermore, the step of using high-energy ions to implant N-type dopants into the source region of the N-type epitaxial layer to form the N-type region also includes:
[0024] Before forming the trench, high energy ions are used to implant N-type dopants into the source region of the N-type epitaxial layer to form an N-type region; or
[0025] When forming the P-type base region, high-energy ions are used to implant N-type dopants into the source region of the N-type epitaxial layer to form an N-type region; or
[0026] When forming an N+ type source region, high energy ions are used to implant N type dopants into the source region of the N type epitaxial layer to form an N type region; or
[0027] Ions with different energies and doses are implanted in different steps and then synthesized into the final N-type region.
[0028] To achieve the above-mentioned object, the present invention provides a split gate trench semiconductor power device, comprising a trench, a split gate gate, a P-type base region, an N-type region, an N+ type source region, a terminal region, a source region metal pad layer, and a gate metal pad layer, wherein:
[0029] The trench, the split gate, the P-type base region, the N-type region, the N+-type source region, the terminal region, the source region metal pad layer, and the gate metal pad layer are made of an epitaxial layer;
[0030] The N-type region is formed by high-energy ion implantation, and its concentration is higher than that of the epitaxial layer.
[0031] Furthermore, the grooves include a first type of groove and a second type of groove, wherein:
[0032] The first type of trench has a dielectric layer on its sidewalls and bottom wall, and a conductive material in the middle, and the formed conductor is connected to the source region metal pad layer;
[0033] The second groove has an upper groove portion and a lower groove portion;
[0034] The side walls and bottom walls of the lower trench portion are dielectric layers, with conductive material in the middle, and the conductor formed is connected to the source metal pad layer; the side walls and bottom walls of the upper trench portion are dielectric layers, with conductive material in the middle, and the conductor formed is connected to the gate metal pad layer and is used as the gate of the device.
[0035] Furthermore, the N-type region is located at the bottom of the P-type base region and between the trenches;
[0036] The N+ type source region is located on the upper part of the P type base region.
[0037] The method for preparing a split gate trench semiconductor power device of the present invention combines a process flow with a new board layout design, overcomes the shortcomings of the prior art, and enables a split gate trench device to be made with only a single epitaxial layer plus ion implantation to produce a device that is equal to or better than a device made with three epitaxial layers. The present invention uses only a single epitaxial layer with a relatively light doping concentration, and then uses high-energy ion implantation to convert the required area into an N-type area with a higher doping concentration. The doping concentration of the area where the high-energy N-type ions are not implanted or the area outside the diffusion length of the implantation point is not affected, such as Fig.24 terminal area.
[0038] Fig. 27 is a schematic diagram of the doping concentration of the N-type region according to the present invention, as shown in Fig. 27 As shown in the figure, the solid line is the doping concentration distribution of the area in the active region that has been injected with high-energy ions after high-temperature diffusion; the dotted line is the distribution of the doping concentration of the three epitaxial layers before high-temperature diffusion, which is roughly the same as that of the high-energy ion implantation after high-temperature diffusion. Because there is no high-energy N-type ion implantation in the terminal region, the doping concentration of the terminal region is basically the doping concentration of the original N-type epitaxial layer. Therefore, when the device is under the same reverse bias, the electric field in the terminal region is relatively less concentrated. The design of the terminal part is relatively simple and only occupies a small space to meet the requirements of the device electrical performance specifications (such as Fig.24 ). The simple and effective terminal design makes the device save more chip area and can be applied to units with different geometric designs, thus improving the performance-price ratio of semiconductor devices. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] The accompanying drawings are used to provide a further understanding of the present invention and are used together with the embodiments of the present invention to explain the present invention, but do not constitute a limitation of the present invention:
[0040] Figure 1 A flow chart of a method for preparing a split-gate trench semiconductor power device according to the present invention;
[0041] Figure 2 A schematic diagram of exposing a surface oxide layer according to an embodiment of the present invention;
[0042] Figure 3 It is a schematic diagram of an embodiment of the present invention after the epitaxial layer is exposed through a trench mask step;
[0043] Figure 4 It is a schematic diagram of an embodiment of the present invention after a groove is formed by etching;
[0044] Figure 5 A schematic diagram of a groove formed in an embodiment of the present invention;
[0045] Figure 6 A schematic diagram of forming an oxide layer in a trench according to an embodiment of the present invention;
[0046] Figure 7 A schematic diagram of depositing highly doped polysilicon in a trench according to an embodiment of the present invention;
[0047] Figure 8 It is a schematic diagram of a polysilicon layer after plane processing according to an embodiment of the present invention;
[0048] Fig. 9 A schematic diagram of a surface of a portion of a groove covered by a photolithography coating according to an embodiment of the present invention;
[0049] Fig.10 A schematic diagram of filling a dielectric layer in a trench according to an embodiment of the present invention;
[0050] Fig.11 A schematic diagram of a surface of a portion of a groove covered by a photolithography coating according to an embodiment of the present invention;
[0051] Fig.12 A schematic diagram of leaving a dielectric layer on a trench field plate according to an embodiment of the present invention;
[0052] Fig.13 A schematic diagram of forming a gate oxide layer in a trench according to an embodiment of the present invention;
[0053] Fig.14 is a schematic diagram of filling highly doped polysilicon in a trench according to an embodiment of the present invention;
[0054] Fig.15 It is a schematic diagram of a polysilicon layer after plane processing according to an embodiment of the present invention;
[0055] Fig.16A schematic diagram of ions implanted into a device to form a P-type base region by using a mask plate according to an embodiment of the present invention;
[0056] Fig.17 A schematic diagram of an embodiment of the present invention in which high-energy ions with a relatively high concentration in an N-type region of a device are injected through a mask;
[0057] Fig.18 It is a schematic diagram of an embodiment of the present invention after high temperature diffusion treatment;
[0058] Fig.19 It is a schematic diagram of an embodiment of the present invention after passing through the N+ source region step;
[0059] Fig. 20 A schematic diagram of forming an interlayer dielectric on a surface of an embodiment of the present invention;
[0060] Fig.21 A schematic diagram of injecting a P-type high dopant into a contact hole trench according to an embodiment of the present invention;
[0061] Fig. 22 It is a schematic diagram of an embodiment of the present invention after a metal etching step;
[0062] Fig.23 A schematic cross-sectional view of an active region structure of a split gate field effect transistor power device according to the present invention;
[0063] Fig.24 It is a schematic diagram of forming an N-type region by ion implantation under a P-type base region and between trenches according to the present invention;
[0064] Fig.25 is a schematic cross-sectional view of an embodiment of the present invention after all front-end process steps are completed;
[0065] Fig.26 is a cross-sectional schematic diagram of a P-type guard ring at the terminal according to the present invention;
[0066] Fig. 27 is a schematic diagram of the doping concentration of the N-type region according to the present invention;
[0067] Fig.28 Schematic diagram of epitaxial layer thickness and resistivity of different epitaxial layer device structures in the prior art. DETAILED DESCRIPTION
[0068] The preferred embodiments of the present invention are described below in conjunction with the accompanying drawings. It should be understood that the preferred embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0069] The split-gate trench semiconductor power device of the present invention has a variety of implementable methods, the key point being to use a high-energy ion implantation method to implant N-type ions below the surface P-type base region and between the trenches, so that the N-type doping concentration in this region is higher than that of the original N-type doped epitaxial layer, generally one to five times higher, thereby eliminating the need for a denser N-type epitaxial layer while optimizing device performance and making the process simple and effective, thereby improving the cost-effectiveness of the device.
[0070] Example 1
[0071] Figure 1 The flowchart of the method for preparing the split gate trench semiconductor power device according to the present invention is as follows. Figure 1 , the preparation method of the split-gate trench semiconductor power device of the present invention is described in detail.
[0072] First, in step 101 , a trench is formed on an N-type epitaxial layer by etching.
[0073] In the embodiment of the present invention, an N-type epitaxial layer (N Epi Layer) is placed on top of an N+ type substrate (N+ Substrate), and an oxide layer (an oxide hard mask with a thickness of 0.3um to 1.5um) is formed on the upper surface of the N-type epitaxial layer by deposition or thermal growth, and then a photolithography coating is deposited on the oxide layer, and then a pattern is formed by a trench mask to expose some parts of the oxide layer, such as Figure 2 As shown;
[0074] After dry etching the oxide layer exposed by the pattern formed by the trench mask, the N-type epitaxial layer is exposed; then the photoresist coating is removed, such as Figure 3 As shown;
[0075] At least two trenches (with a depth of 1.0 um to 3.0 um and a width of 0.2 um to 1.0 um) are formed by etching, and the formed trenches extend to the N-type epitaxial layer, such as Figure 4 As shown;
[0076] After the trench is formed, the trench is subjected to sacrificial oxidation (for 10 minutes to 100 minutes at a temperature of 1000° C. to 1200° C.) to eliminate the silicon layer damaged by the plasma during the trenching process; after all the oxide layers are removed, the trench is as follows: Figure 5 shown.
[0077] In step 102, an oxide layer is formed on the sidewalls and bottom wall of the trench and filled with a conductive material (polysilicon).
[0078] In the embodiment of the present invention, an oxide layer (with a thickness of 0.03 um to 0.6 um) is formed on the exposed sidewalls and bottom of the trench and the upper surface of the N-type epitaxial layer by thermal growth. Figure 6 As shown;
[0079] N-type highly doped polysilicon is deposited in the trench to fill the trench and cover the top surface of the N-type epitaxial layer, such as Figure 7 As shown, the polysilicon doping concentration is R S =5Ω / □ to 100Ω / □ (Ω / □ is the unit of square resistance);
[0080] The polysilicon layer (poly layer) on the surface of the N-type epitaxial layer is subjected to planar etching or chemical mechanical polishing to etch away the polysilicon on the surface of the N-type epitaxial layer. Figure 8 shown.
[0081] In step 103, the polysilicon in the upper portion of at least one trench is etched away, a dielectric layer is formed on the bottom wall of the upper portion of the at least one trench, and a new dielectric layer is formed on the sidewall of the upper portion of the at least one trench and filled with conductive material (polysilicon).
[0082] In the embodiment of the present invention, after a photoresist coating is deposited on the surface of the N-type epitaxial layer, a pattern is formed by a mask to cover a portion of the surface of the groove; the polysilicon in the groove is etched away, and the polysilicon in the uncovered groove between about 0.8um and 1.5um from the upper surface of the polysilicon is etched away, such as Fig. 9 As shown;
[0083] After removing the photoresist coating, a dielectric layer (silicon dioxide or silicon nitride, etc.) is deposited in the trench to fill the trench and cover the top surface of the N-type epitaxial layer, such as Fig.10 As shown;
[0084] The dielectric layer on the surface of the N-type epitaxial layer is subjected to planar etching or chemical mechanical polishing to etch away the dielectric layer on the surface of the N-type epitaxial layer; after a layer of photoresist is deposited on the surface of the N-type epitaxial layer, a pattern is formed through a mask to cover a portion of the surface of the groove, such as Fig.11 As shown;
[0085] The dielectric layer in the trench without the protection of the photolithography layer is etched to remove the dielectric layer about 0.02um to 0.3um from the upper surface of the polysilicon in the trench, that is, only the dielectric layer about 0.02um to 0.3um from the upper surface of the polysilicon in the trench is retained. Fig.12 As shown;
[0086] By thermal growth, a thin gate oxide layer (thickness of 0.01um to 0.04um) is formed on the exposed sidewalls of the trench and the upper surface of the N-type epitaxial layer. Fig.13 As shown;
[0087] N-type highly doped polysilicon is deposited in the trench to fill the trench and cover the top surface of the N-type epitaxial layer, such as Fig.14 As shown, the polysilicon doping concentration is RS=5Ω / □ to 100Ω / □ (Ω / □ is the unit of square resistance);
[0088] The polysilicon layer on the surface of the N-type epitaxial layer is subjected to planar etching or chemical mechanical polishing, such as Fig.15 shown.
[0089] In step 104, a P-type base region, an N-type region with a higher concentration below the P-type base region, and an N+ type source region on the P-type base region are formed on the N-type epitaxial layer.
[0090] In the embodiment of the present invention, after a photoresist coating is deposited on the surface of the N-type epitaxial layer, the thickness of the photoresist coating is 0.5um to 3.0um, and then a pattern is formed through a P-type region mask to expose the source region where the P-type base region needs to be injected; then a P-type dopant (boron, with a dose of 8e12 / cm 3 to 2e14 / cm 3 , energy is 100KeV to 300KeV), forming a P-type base region, such as Fig.16 As shown;
[0091] Then, high-energy ions are used to implant N-type dopants (phosphorus, with a dose of 4e12 / cm 3 to 2e13 / cm 3 , energy is 500KeV to 3MeV), forming an N-type region with a higher concentration below the P-type base region on the N-type epitaxial layer, such as Fig.17 As shown;
[0092] Through a high temperature diffusion treatment (temperature of 950°C to 1200°C, time of 10 minutes to 1000 minutes), the P-type base region is diffused into the N-type epitaxial layer (depth of 0.5um to 2.0um) and the high-energy injected N-type dopant is diffused to about 1.0um from the surface and to the depth of the trench bottom, such as Fig.18 As shown;
[0093] N-type dopants (phosphorus or arsenic, with a dose of 1e15 / cm2) are implanted into the N-type epitaxial layer through the N+ mask step. 3 to 2e16 / cm 3 ); then through a secondary high temperature diffusion treatment (temperature of 950°C to 1200°C, time of 10 minutes to 100 minutes), the N-type region is diffused into the P-type base region to form an N+ type source region, such as Fig.19 As shown;
[0094] The depth of the N+ type source region is 0.2um to 0.5um, and the depth of the P type base region is 0.5um to 1.5um.
[0095] In the embodiment of the present invention, high-energy ions are used to implant N-type dopants into the source region of the N-type epitaxial layer to form an N-type region with a higher concentration below the P-type base region on the N-type epitaxial layer. The implantation may be performed more than once and with more than one energy and dosage, and performed under the same mask coating as the P-type base region. In this way, there must be an N-type region with a higher concentration below the P-type base region and between the trenches. If a mask dedicated to this step is used to implement ion implantation, there may not necessarily be an N-type region with a higher concentration than the N-type epitaxial layer below the P-type base region. The N-type region with a higher concentration than the N-type epitaxial layer is formed by high-energy ion implantation before trenching, or by high-energy ion implantation when forming the P-type base region or when forming the n+ highly doped source region, or by implantation of ions with corresponding high energy and dosage in different steps of the entire process flow, and then finally synthesized into an N-type region with a relatively high concentration below the P-type base region.
[0096] In step 105, a source metal pad layer, a gate connection and a terminal field plate are formed on the N-type epitaxial layer.
[0097] In the embodiment of the present invention, an undoped silicon dioxide layer (with a thickness of 0.1 um to 0.5 um) is first deposited on the surface of the N-type epitaxial layer, and then borophosphorus glass (with a thickness of 0.1 um to 0.8 um) is deposited to form an interlayer dielectric. Fig. 20 As shown;
[0098] A photoresist coating is deposited on the surface of the interlayer dielectric, and a contact hole mask is used to expose part of the interlayer dielectric. The exposed part of the interlayer dielectric is then dry-etched to form multiple contact hole mask openings in the interlayer dielectric, and then the photoresist coating is removed; the surface of the silicon wafer containing dopants is etched to make the contact hole groove (depth of 0.4um to 1.5um, width of 0.12um to 1.6um) pass through the N-type source region and enter the P-type base region, and then the contact hole groove is injected with P-type high dopant (concentration of 10E14 / cm3 to 5×10E15 / cm3) to reduce the contact resistance between the P-type base region and the metal plug, effectively increasing the safe use area of the device, such as Fig.21 As shown;
[0099] After depositing a layer of titanium or titanium nitride on the sidewalls, bottom and upper surface of the interlayer dielectric of the contact hole trench, the contact hole trench is filled with tungsten to form a metal plug; after depositing a layer of aluminum-copper alloy (thickness of 0.8um to 10um) on the top of the device, metal etching is performed through a metal mask to form a source metal pad layer, a gate connection and a terminal field plate, such as Fig. 22 shown.
[0100] Example 2
[0101] The embodiment of the present invention further provides a split-gate trench semiconductor power device, comprising:
[0102] At least two types of grooves: a first type of groove and a second type of groove.
[0103] The sidewalls and bottom wall of the first trench are dielectric layers, the middle of the first trench is conductive material, the conductor formed by the first trench is connected to the source metal at the top, and there is a P-type base region between the two first trenches.
[0104] The second type of groove has a two-part structure: an upper groove and a lower groove.
[0105] The side walls and bottom walls of the lower trench are dielectric layers, the middle of the lower trench is conductive material, and the conductor formed by the lower trench is connected to the source metal (for example, connected to the source metal by connecting the conductor of the first trench) as a field plate; the side walls and bottom walls of the upper trench are dielectric layers, the middle of the upper trench is conductive material, and the conductor formed by the upper trench is connected to the gate metal (for example, gate connection, wire bonding metal pad) and used as the gate of the device.
[0106] There is a P-type base region between the two second trenches and an N-type region with a higher concentration formed under the P-type base region by a high-energy ion implantation method.
[0107] The split gate trench semiconductor power device also has at least a split gate, a P-type base region, a high-concentration N-type region formed under the P-type base region by a high-energy ion implantation method, an N+ type source region, a terminal region, a source region metal pad layer and a gate metal pad layer.
[0108] In the embodiment of the present invention, the depth of the two grooves is about 1.0um to 3.0um, the width is about 0.2um to 1.0um, and the surface plate structure can be strip, rectangular, square or hexagonal.
[0109] In the embodiments of the present invention, the high energy ion implantation step can be implemented before trenching, or can be implemented together when forming a P-type base region or an N+ type source region, or can be implanted separately with ions of corresponding high energy and dosage in different steps of the entire process flow, and then finally synthesize an N-type region with a relatively high concentration under the P-type base region. In the following embodiments, the N-type region with a relatively high concentration under the P-type base region is ion implanted using the same mask coating as the P-type base region.
[0110] Fig.23 FIG. 1 is a schematic cross-sectional view of the active region structure of a split gate field effect transistor power device according to the present invention. Fig.23As shown, the split gate field effect transistor power device of the present invention includes a split gate, a P-type base region, an N-type region with a higher doping concentration than the N-type epitaxial layer under the P-type base region and between the trenches, an N+ type source region and a source region metal pad layer. The difference from the prior art is that the N-type region with a higher doping concentration than the original epitaxial layer under the P-type base region and between the two trenches is formed by ion implantation.
[0111] Fig.24 FIG. 1 is a schematic diagram of forming an N-type region by ion implantation under a P-type base region and between trenches according to the present invention, as shown in FIG. Fig.24 As shown in the figure, the N-type region with a higher doping concentration than the original epitaxial layer under the P-type base region and between the trenches is completed by more than one implantation and more than one ion implantation method with energy and dose. The implanted ions are phosphorus with a dose of 4e12 / cm 3 to 2e13 / cm 3 , energy ranges from 500KeV to 5MeV.
[0112] In the embodiment of the present invention, an N-type region with a doping concentration higher than that of the original epitaxial layer under the P-type base region and between the trenches can be formed by ion implantation under the same mask coating as the P-type base region, so that there must be an N-type region with a higher concentration under the P-type base region and between the trenches.
[0113] In the embodiment of the present invention, the N-type region with a doping concentration higher than that of the original epitaxial layer under the P-type base region and between the trenches is ion implanted using its own dedicated mask. Thus, there may not be an N-type region with a higher doping concentration under the P-type base region and between the trenches under the P-type base region. Fig.25 and 26 shown.
[0114] In the embodiment of the present invention, an N-type region with a doping concentration higher than that of the original epitaxial layer under the P-type base region and between the trenches can be formed by high-energy ion implantation before digging the trenches, or by high-energy ion implantation when forming the P-type base region or when forming the n+ highly doped source region. It can also be formed by implanting ions with corresponding high energy and dosage separately in different steps of the entire process flow, and then finally synthesizing an N-type region with relatively high concentration under the P-type base region.
[0115] The method for preparing the split-gate trench semiconductor power device of the present invention can increase the performance-price ratio of the device without affecting the quality and reliability of the trench power device.
[0116] Finally, it should be noted that the present invention can be used to manufacture various trench semiconductor power devices (for example, trench insulated gate bipolar transistors (Trench IGBTs), trench diodes or trench Schottky diodes). The present invention can be used to prepare 12V to 1200V trench semiconductor power devices. The embodiments of the present invention are described with reference to N-type channel devices. The present invention can also be used for P-type channel devices. Although the present invention is described in detail with reference to the embodiments, for those skilled in the art, they can still modify the technical solutions recorded in the aforementioned embodiments, or make equivalent substitutions for some of the technical features therein. However, any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a split-gate trench semiconductor power device, The following steps are involved: Forming a groove on the N-type epitaxial layer by etching; After forming a dielectric layer on the sidewalls and bottom wall of the trench, a conductive material is filled in to form a first trench; After etching away the conductive material on the upper portion of at least one of the first-type trenches, a dielectric layer is formed on the bottom wall and side walls of the upper portion and then filled with conductive material to form a second-type trench; Forming a P-type base region, an N-type region and an N+-type source region on the N-type epitaxial layer, wherein the N-type region is located below the P-type base region and between the trenches; The step of forming an N-type region on the N-type epitaxial layer includes: before forming the trench, using high-energy ions to implant N-type dopants into the source region of the N-type epitaxial layer to form the N-type region; or when forming the P-type base region, using high-energy ions to implant N-type dopants into the source region of the N-type epitaxial layer to form the N-type region; or when forming the N+ type source region, using high-energy ions to implant N-type dopants into the source region of the N-type epitaxial layer to form the N-type region; or using ions of different energies and doses to implant them separately in different steps, and then synthesizing them into the final N-type region; the step of forming the N-type region is performed under the same mask as the P-type base region, so that the concentration of the N-type region is higher than that of the N-type epitaxial layer; wherein, when forming the N-type region, the N-type dopant doped by high-energy implantation is diffused to a depth of 1.0 μm from the surface and to the bottom of the first trench by high-temperature diffusion treatment; A source region metal pad layer, a gate connection and a terminal region field plate are formed on the N-type epitaxial layer.
2. The method for preparing a split-gate trench semiconductor power device according to claim 1, It is characterized in that The step of forming a P-type base region, an N-type region and an N+ type source region on the N-type epitaxial layer further includes: Injecting P-type dopants into the source region of the N-type epitaxial layer to form a P-type base region; N-type dopants are injected into the N-type epitaxial layer through an N+ mask, and diffused into the P-type base region to form an N+ type source region.
3. The method for preparing a split-gate trench semiconductor power device according to claim 2, It is characterized in that The energy of the high-energy ions is 400 KeV to 5 MeV, and the dose is 4e12 / cm 3 to 2e13 / cm 3 .
4. A split-gate trench semiconductor power device, manufactured by the manufacturing method according to any one of claims 1 to 3, comprising a trench, a split-gate gate, a P-type base region, an N-type region, an N+-type source region, a terminal region, a source region metal pad layer, and a gate metal pad layer, It is characterized in that The trench, the split gate, the P-type base region, the N-type region, the N+-type source region, the terminal region, the source region metal pad layer, and the gate metal pad layer are made of a single epitaxial layer.
5. The split-gate trench semiconductor power device according to claim 4, It is characterized in that The groove, It includes a first groove and a second groove, wherein: The first type of trench has a dielectric layer on its sidewalls and bottom wall, and a conductive material in the middle, and the formed conductor is connected to the source region metal pad layer; The second groove has an upper groove portion and a lower groove portion; The side walls and bottom walls of the lower trench portion are dielectric layers, with conductive material in the middle, and the conductor formed is connected to the source metal pad layer; the side walls and bottom walls of the upper trench portion are dielectric layers, with conductive material in the middle, and the conductor formed is connected to the gate metal pad layer and is used as the gate of the device.
6. The split-gate trench semiconductor power device according to claim 4, It is characterized in that The N+ type source region is located on the upper part of the P type base region.
Citation Information
Patent Citations
Method of preparing groove semiconductor power device
CN103632964A
Double split trench gate charge storage type insulated gate bipolar transistor (IGBT) and manufacturing method thereof
CN105789291A
Epitaxial layer structure of metal-oxide channel semiconductor field effect transistor
CN107546257A
Multi-groove semiconductor power device and preparation method thereof
CN108417637A
Shielding gate power device and manufacturing method thereof
CN109979987A