A heat storage tunnel kiln with flue gas reflow and high temperature section exhaust and roasting process
Through the regenerative tunnel kiln with flue gas reflux and high-temperature section smoke exhaust, roasting process and composite pellet technology, the problems of high energy consumption and large flue gas heat loss in the direct reduction process of iron ore tunnel kiln have been solved, and high efficiency has been achieved. The flue gas waste heat recovery and kiln car heating reduce production costs and kiln section length.
Patent Information
- Application Number
- CN202110815345.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-07-19
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2041-07-19
AI Technical Summary
The iron ore tunnel kiln direct reduction process has problems such as long reduction time, small production scale, high energy consumption, low fuel utilization efficiency and large flue gas heat loss. Especially in fuel-deficient areas, its promotion and application are limited.
It adopts a regenerative tunnel kiln and roasting process with flue gas return and high-temperature section smoke exhaust. Through composite pellet technology and spray cooling technology, it realizes the recovery of flue gas waste heat and the utilization of high-temperature air, reducing the demand for external gas fuel and shortening the reduction time. and kiln section length.
Material heating is achieved without using external gaseous fuel, which improves the thermal shock stability of the kiln car and production economy, reduces production costs, and achieves compliance with flue gas emissions standards.
Smart Images

Figure CN113624003B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of minerals and metallurgy, and in particular relates to a heat storage tunnel kiln with smoke reflow and high-temperature section smoke exhaust and a roasting process. Background Art
[0002] At present, the direct reduction process of iron ore tunnel kiln is to mix and mix the concentrate powder, coal powder and limestone powder in a certain proportion and put them into the reduction tank, then push the kiln car with the reduction tank into the tunnel kiln for roasting. After the material tank is roasted at a temperature of about 1150℃ for 35 to 40 hours and cooled in the absence of oxygen in the tunnel kiln, direct reduced iron can be obtained. Although the direct reduction process of iron ore coal-based tunnel kiln is mature in technology and simple to operate, there are problems in the direct reduction of iron ore, such as long reduction time, small production scale and high energy consumption.
[0003] In the direct reduction of iron ore tunnel kiln, in order to balance the furnace pressure distribution along the length of the tunnel kiln and reduce the positive pressure flaming and negative pressure air suction phenomenon in the kiln, the method of exhausting smoke from both ends of the tunnel kiln is generally adopted. In the preheating section of the tunnel kiln, the temperature of the coal-ore mixture gradually increases during the countercurrent heat exchange between the kiln gas and the kiln gas, and the volatile matter in the reduced coal begins to precipitate at about 350°C, resulting in a certain amount of combustible components (such as CO) in the flue gas discharged from the preheating section of the tunnel kiln. These low-content combustible gases cannot be burned at a lower temperature, but directly discharged into the atmosphere will cause environmental pollution. In the flue gas discharged from the cooling section of the tunnel kiln, the combustible component content is high, and the temperature of the flue gas is high after secondary combustion. The waste heat of the high-temperature flue gas is generally recovered by a waste heat boiler. The flue gas after cooling is then directly discharged into the atmosphere after dust removal. In the structural design of the tunnel kiln, in order to recover the waste heat of the high-temperature flue gas discharged from the preheating section and the roasting section, the tunnel kiln is generally equipped with a longer preheating section and roasting section.
[0004] At present, in the process of direct reduction of iron ore tunnel kiln, a layer of cover coal is generally covered on the surface of iron ore. After the volatile matter in the cover coal is volatilized or the carbon is gasified, it can provide part of the heat to the kiln, and most of the heat needs to be provided by external coal gas combustion. When the tunnel kiln is used in areas where gas fuel is scarce, the problem of coal gas supply is difficult to solve, which limits the promotion and application of direct reduction of iron ore tunnel kiln. However, when the tunnel kiln uses generator gas as fuel, it is generally necessary to build a gas generator. The gas generator uses coal as raw material, converts coal into generator gas through high-temperature cracking and gasification, and the generator gas is then supplied to the tunnel kiln for use. Because there is a secondary conversion of energy in the process of fuel utilization in the tunnel kiln, the utilization rate of coal resources is not high, and the energy consumption per unit of roasting ore is high.
[0005] At present, in the direct reduction process of iron ore tunnel kiln, in order to prevent secondary oxidation of the roasted ore after high-temperature reduction and to recover part of the waste heat of the high-temperature roasted ore, the normal temperature gas fuel used for heating is generally supplied from the outlet end of the cooling section. The gas fuel exchanges heat with the roasted ore during the countercurrent process of the cooling section, and the temperature can be raised to above 1000°C in the long cooling section, while the temperature of the roasted ore is reduced to below 200°C. The long cooling section of the tunnel kiln not only increases the production cost, but also makes it difficult to control the reducing atmosphere in the cooling section due to the change of furnace pressure along the length of the kiln. In addition, in the preheating section of the tunnel kiln, since the heat exchange between the flue gas and the material is mainly convective heat transfer, it takes a long preheating section to reduce the temperature of the high-temperature flue gas to below 300°C, which also increases the production cost of the tunnel kiln.
[0006] At present, when direct reduction of iron ore is carried out in a tunnel kiln, generally more than 80% of the flue gas is discharged from the kiln entrance. The amount of flue gas discharged from the kiln entrance is large, and its exhaust temperature is also high. The high exhaust temperature takes away a lot of heat, causing the coal volatile matter volatilization or carbon gasification on the kiln car cover to produce gas that cannot meet the needs of tunnel kiln material heating and reduction.
[0007] Among the regenerative heat technologies commonly used in metallurgical enterprises, the regenerative heat technology integrates the functions of air-gas preheating and flue gas cooling and emission, which can maximize the recovery of the flue gas sensible heat of the furnace, reduce energy consumption, and improve the heating quality of materials. High-temperature air-gas heat exchange technology based on the regenerative heat exchange principle is a heat exchange technology that has been widely promoted and applied in recent years. It has the advantages of high flue gas waste heat recovery efficiency, high air preheating temperature, and low pollution emissions. At present, regenerative heat exchange technology is widely used in thermal equipment such as steel rolling heating furnaces and chamber furnaces, but there is no application of regenerative combustion technology in tunnel kilns for direct reduction of iron ore.
[0008] In summary, the main problems of direct reduction of iron ore in tunnel kilns are: (1) gas fuel is required for heating of tunnel kilns; (2) the exhaust temperature of tunnel kilns is relatively high, resulting in large heat losses caused by flue gas; (3) the reduction time of iron ore is relatively long and the energy consumption is relatively high; and (4) tunnel kilns are equipped with relatively long preheating and heating sections. Summary of the invention
[0009] The present invention provides a heat storage tunnel kiln with smoke reflow and high-temperature smoke exhaust and a roasting process, aiming to solve the above technical problems.
[0010] To this end, the present invention adopts the following technical solutions:
[0011] A regenerative tunnel kiln with flue gas recirculation and high-temperature smoke exhaust and a roasting process, the regenerative tunnel kiln comprising a tunnel kiln body, a kiln car, a flue gas recirculation system, a regenerative heat exchange system, a dry dust removal system, a wet dust removal system and a spray cooling zone system, the tunnel kiln body comprising a preheating section, a roasting section, an air cooling section and a water cooling section from front to back;
[0012] The flue gas recirculation system is arranged between the preheating section and the air cooling section, and is used to introduce the air of the preheating section into the air cooling section; the regenerative heat exchange system is arranged on the roasting section, the dry dust removal system is arranged on the regenerative heat exchange system, and the wet dust removal system is arranged on the water cooling section;
[0013] The roasting process comprises the following steps:
[0014] 1) After the particle size classification, the 0-30 mm iron ore is divided into three particle size ranges: 0-5 mm fine particles, 5-15 mm medium particles, and 15-30 mm coarse particles. The iron ore in each particle size range is mixed with the reducing coal to form 20-25 mm composite pellets;
[0015] 2) Place a layer of bituminous coal with a particle size of 5 to 30 mm at the bottom of the kiln car material basin, place 3 to 5 layers of composite pellets on the bituminous coal layer, place a layer of coke with a particle size of 5 to 30 mm on the composite pellet layer, and place a layer of covering agent with a particle size of 5 to 10 mm, mainly made of siliceous materials, on the top;
[0016] 3) The kiln car loaded with materials enters from the kiln entrance of the tunnel kiln body. When the kiln car passes through the preheating section, the materials are preheated to about 400°C by a part of the flue gas extracted from the preheating section. The coal begins to gasify and the iron ore begins to be reduced;
[0017] 4) After the kiln car enters the roasting section, the material is gradually heated to 1000-1100℃ by the high-temperature flue gas in the kiln, and the reduction rate of the iron ore is accelerated; when the kiln car enters the end of the roasting section, the reduction of the iron ore on the upper layer of the kiln car is basically completed; the high-temperature flue gas discharged from the roasting section passes through the regenerative heat exchanger and the temperature drops to about 200℃, the low-temperature flue gas is discharged through the dust collector and the smoke exhauster, and the normal temperature air is preheated and sent to the roasting section for use;
[0018] 5) When the kiln car enters the air cooling section, the material and the kiln car are cooled by the 200°C reflux gas introduced from the outlet of the flue gas reflux system of the air cooling section, which can reduce the surface temperature of the roasting material layer from about 1100°C to about 400°C within 60 to 90 minutes;
[0019] 6) After air cooling, the medium-temperature material enters the water cooling section again. The medium-temperature material is cooled by the atomized water sprayed from the top of the kiln. The atomized water absorbs heat and vaporizes into steam, which is drawn out from the top of the water cooling section. The temperature of the medium-temperature material drops to below 200°C and is discharged from the kiln outlet.
[0020] 7) In the water-cooling section of the tunnel kiln, the cooling water is pressurized and filtered by a water pump and then atomized to cool the high-temperature materials. The vaporized water is then passed through a vibrating screen for dust removal and water vapor recovery, air cooler for cooling, sludge sedimentation and treatment, and sewage treatment before being recycled into the system.
[0021] The roasting principle of the present invention is as follows:
[0022] The composite pellets are composed of a core, a skin and a shirt. The core is a 20-25mm iron ore carbon-containing pellet, which is produced by mixing iron materials (iron concentrate, blast furnace gas ash, converter OG mud, etc.), limestone, bituminous coal powder and cement in a certain proportion, and then using a disc or cylinder ball making method; the material mixed with iron materials (iron concentrate, converter OG mud, etc.) and bentonite in a certain proportion is wrapped on the outside of the core by a ball making disc or cylinder to form a skin, and the particle size is controlled at 25-31mm; then a certain amount of bituminous coal powder is wrapped outside the skin by a ball making disc or cylinder to form a shirt, and the overall particle size of the composite pellets is controlled at 27-33mm. When the composite pellets are heated and reduced in the tunnel kiln, the skin limits the expansion of the core, so that the composite pellets have sufficient strength after the reduction is completed. The bituminous coal powder in the core and skin of the composite pellets plays a dual role as a reducing agent and a fuel. During the reduction process of the composite pellets, the core is easy to reduce, the skin is only 5-10mm thick and there is coal powder on both the inside and outside. The internal diffusion resistance of reduction is small and it is also easy to be reduced.
[0023] The composite pellets are produced in the tunnel kiln using layered material distribution and hydrocarbon combined reduction technology: (1) a layer of bituminous coal with a particle size of 5 to 30 mm (the amount is about 20% of the weight of the composite pellets) is laid at the bottom of the kiln car material basin, 3 to 5 layers of composite pellets are laid on the bituminous coal layer, a layer of coke with a particle size of 5 to 30 mm (the amount is about 20% of the weight of the composite pellets) is laid on the composite pellet layer, and a layer of covering agent with a particle size of 5 to 10 mm mainly composed of siliceous materials (the amount is about 5% of the weight of the composite pellets) is laid on the top. (2) During the roasting process of the materials in the tunnel kiln, the bituminous coal at the bottom will undergo a coal distillation process. A part of the H2 in the gaseous distillation products released by the heat will reduce the iron oxides in the upper composite pellets, and the remaining H2 and CH4, tar, benzene, naphthalene and other gaseous distillation products will be discharged from the material layer into the tunnel kiln as heating fuel, and the solid distillation product - coke will be laid on the top of the composite pellet layer in the subsequent layered distribution of the kiln car material basin. (3) The bituminous coal powder (ball coat) wrapped on the outermost side of the composite pellet and the bituminous coal powder mixed in the core of the pellet also need to undergo a coal dry distillation process during the heating process. A portion of the H2 in the gaseous dry distillation product will reduce the iron oxides in the composite pellet, and the remaining H2 and CH4, tar, benzene, naphthalene and other gaseous dry distillation products will be discharged from the material layer into the tunnel kiln as heating fuel, and the solid dry distillation product - coke will be gasified by CO2 or H2O in the material layer in the middle and late stages of the composite pellet reduction to generate gaseous reducing agents CO and H2, and reduce the iron oxides in the composite pellet. In the early stage of the composite pellet reduction, when the composite pellet temperature is below 800℃, H2 reduction is the main method; in the middle and late stages of the composite pellet reduction, when the composite pellet temperature is above 800℃, CO reduction is the main method. (4) Most of the coke spread on the top of the composite pellet layer is consumed by the CO2 or H2O in the metallurgical gas produced by the metallurgical reduction reaction of the composite pellet layer and generates new CO and H2, which are discharged from the material layer into the tunnel kiln together with the high-temperature metallurgical gas produced by the reduction reaction and used as heating fuel. (5) The covering agent spread on the top of the material layer has the following functions: First, during the roasting process, it protects the coke spread on the top of the composite pellet from being gasified by the CO2 or H2O in the high-temperature flue gas generated by the combustion in the kiln, thereby improving the heat transfer level to the material layer; second, in the later stage of roasting, as the overall material temperature increases, the covering agent naturally generates a glassy soft melt, which plays an oxygen-isolating role and prevents the metallized pellets from being oxidized during the cooling process.
[0024] Fuel supply technology for direct reduction of composite pelletizing tunnel kiln (i.e., self-heating balance): (1) Layered distribution During the heating process of the materials in the kiln car material basin, a large amount of metallurgical gas is produced due to coal distillation, limestone decomposition, and a series of metallurgical reduction reactions centered on carbon gasification, and is discharged from the material layer into the tunnel kiln. This metallurgical gas has a high calorific value (combustible gas components such as CO, H2, and CH4 account for more than 90% of the volume) and a high temperature (average of about 1000°C). As long as an appropriate amount of air is added to the tunnel kiln to assist combustion, the heat released by the combustion of the self-produced metallurgical gas is sufficient to meet the heat demand of the tunnel kiln itself, and self-heating balance can be achieved without the need for external gas fuel. (2) Since the tunnel kiln adopts a thermal system of exhausting smoke at the feeding end and circulating it, and exhausting smoke in the roasting section, the exhaust volume at the feeding end accounts for about 15-20% of the total smoke volume. This part of the smoke has been used to dry and preheat the materials in the tunnel kiln, and the temperature when it is discharged from the tunnel kiln is about 200°C; the roasting section discharges all the smoke in the kiln to the outside, and the exhaust temperature of the smoke is about 1100°C. The heat taken away by this part of the smoke accounts for about 50-60% of the total heat balance of the tunnel kiln. (3) When high-temperature heat storage technology is used to recover the waste heat of high-temperature smoke, high-temperature smoke at about 1100°C is used to replace high-temperature air above 1000°C, and the high-temperature air is reused in the roasting and reduction section of the tunnel kiln as combustion air, which can improve the economic efficiency of the tunnel kiln operation.
[0025] Rapid cooling technology for high-temperature roasted ore (i.e., spray cooling): (1) Composite pellets are roasted at high temperature in a tunnel kiln to become metallized pellets, which have smaller particle size than the composite pellets before roasting, denser structure (without the characteristics of sponge iron), and higher strength (above 1000N). The present invention cools the metallized pellets in the kiln car material basin to about 400°C before leaving the kiln, thereby preventing them from being oxidized by contact with air. (2) The present invention provides a spray device in the water-cooling section of the tunnel kiln, so that the atomized water is vaporized before it contacts the surface of the kiln car and the material basin after being sprayed in from the kiln top, thereby protecting the kiln car and the material basin from damage due to rapid cooling.
[0026] The roasting process of composite pellets in the tunnel kiln: After the composite pellets, the covering coal and the covering agent are placed on the kiln car, the kiln car enters from the tunnel kiln entrance. When the kiln car passes through the preheating section, the material is preheated to about 400°C by the 15-20% flue gas extracted from the entrance end, and the reduced coal begins to decompose and the iron ore begins to be reduced. When the kiln car enters the roasting section, the material is gradually heated to about 1000°C by the high-temperature flue gas in the kiln, and the reduction rate of the iron ore is accelerated. When the kiln car enters the end of the roasting section, the reduction of the composite pellets on the kiln car is basically completed. When the kiln car enters the air cooling section, the roasting material is cooled by the reflux gas of about 200°C introduced from the outlet of the air cooling section, which can reduce the surface temperature of the roasting material layer from about 1000°C to about 400°C within 60-90 minutes. After the initial cooling, the medium-temperature material enters the water cooling section again, where it is cooled by the atomized water sprayed from the top of the kiln. The atomized water absorbs heat and vaporizes into steam, which is drawn out from the top of the water cooling section. The temperature of the medium-temperature material drops below 200°C and is discharged from the kiln outlet.
[0027] In the present invention, after the kiln car loaded with materials enters the preheating section, the temperature of the cover coal on the surface of the kiln car increases under the heating of the countercurrent flue gas. When the temperature of the cover coal increases to above 350°C, the volatile matter, tar, naphthalene, etc. in the coal begin to be released and enter the kiln gas, making the countercurrent flue gas present a certain reduction property. When the countercurrent flue gas flows to the kiln inlet end and its temperature drops to 200-250°C, the countercurrent flue gas is extracted by the exhaust ports at the upper and lower parts of the kiln car and used as reflux gas. As the kiln car advances in the preheating section, the volatile matter released from the cover coal gradually increases. When the temperature of the composite pellets on the upper layer of the kiln car increases to above 300°C, the limonite in the iron ore begins to remove crystal water; when the temperature increases to above 400°C, the siderite in the composite pellets begins to decompose and the hematite begins to reduce. When the gas released during the reduction of iron ore passes through the cover coal, the CO2 and water vapor in the gas react with the cover coal to form a carbon gasification reaction, and the combustible gas released by the reaction enters the kiln chamber space and is used as fuel. When the kiln car enters the roasting section, the volatile matter released by coal decomposition, the combustible gas released by the carbon gasification reaction, and the gas released by the reduction of the composite pellets are mixed with the high-temperature air supplied by the roasting section to burn and produce high-temperature flue gas. Part of the heat of the high-temperature flue gas is used to heat and reduce the material, and part of the heat enters the preheating section with the countercurrent flue gas flow to preheat the kiln car and the material, and most of the heat of the high-temperature flue gas is taken away by the flue gas extracted from the roasting section. When the kiln car enters the end of the roasting section, the reduction of the upper composite pellets is basically completed, and most of the reduction of the middle and lower composite pellets is completed. When the kiln car enters the air cooling section, the roasting material and the return flue gas supplied from the end of the air cooling section are countercurrently exchanged. When the return gas temperature rises to about 1000℃, the surface temperature of the kiln car material also drops from about 1000℃ to below 400℃. After the high-temperature return flue gas flows to the roasting section, it mixes with the high-temperature combustion-supporting air supplied, which can cause the combustible components in it to burn. During the cooling process of the kiln car material in the air cooling section, the temperature of the upper iron ore drops faster, while the temperature of the middle and lower iron ore drops slower, which can make the middle and lower iron ore further reduced during the slow cooling process, thereby improving the direct reduction quality of the iron ore. When the kiln car material enters the water cooling section, the atomized water sprayed from the top of the water cooling section exchanges heat with the high-temperature kiln gas during the falling process. The atomized water absorbs heat and vaporizes into water vapor, which is discharged from the end of the water cooling section. After the temperature of the high-temperature kiln gas drops, it exchanges heat with the roasting material again, which can reduce the temperature of the roasting material. When the temperature of the roasted material drops below 200°C, it is discharged from the discharging end.
[0028] The present invention extracts 250°C reflux flue gas from the preheating section, pressurizes it through a smoke extractor, and then transports it to the outlet of the air cooling section for use as cooling gas for roasting materials. The amount of reflux flue gas extracted is 15-20% of the total flue gas volume of the system. The main functions of extracting reflux flue gas from the preheating section of the tunnel kiln and supplying it to the cooling section are: (1) When the tunnel kiln car passes through the preheating section, the reflux flue gas is used to preheat the materials and the kiln car, which improves the thermal shock stability of the kiln car refractory materials and recovers part of the flue gas waste heat, thereby reducing the energy consumption of the tunnel kiln; (2) In order to pressurize the reflux gas with a heat-resistant blower, according to the fact that the operating temperature of the heat-resistant blower should be below 300°C, by controlling the amount of flue gas extracted from the preheating section of the tunnel kiln to be 15-20% of the total flue gas volume of the system as reflux flue gas, the reflux flue gas temperature can be maintained at about 250°C.
[0029] The length of the preheating section and air cooling section of the tunnel kiln is determined as follows: According to the fact that during the direct reduction process of the composite pelletizing tunnel kiln, the pellets heat up faster in the preheating section in the temperature range of 0 to 600°C and heat up slower in the temperature range of 600 to 1000°C, while the pellets cool down faster in the cooling section in the temperature range of 400 to 1000°C and cool down slower in the temperature range of 0 to 400°C, and considering the thermal shock stability of the refractory materials of the kiln car, the present invention sets a preheating section and air cooling section of reasonable length for the tunnel kiln.
[0030] In order to achieve standard emission of smoke generated by the tunnel kiln, the present invention supplies a certain amount of excess air into the roasting section of the tunnel kiln, and can adjust the kiln temperature of the roasting section to 1150-1250°C by adjusting the amount of excess air while the combustible components in the kiln gas are completely burned. The high-temperature smoke after heat exchange is discharged from the middle and rear part of the roasting section. The high-temperature smoke of about 1250°C discharged from the tunnel kiln enters the regenerative heat exchanger to exchange heat with the normal-temperature air blown in from the blower, so that the smoke temperature can be reduced from about 1250°C to below 200°C. The cooled smoke is then dedusted by the dry dust collector, extracted by the smoke exhauster and discharged into the atmosphere through the chimney. In the regenerative heat exchanger, after the air temperature rises to about 1000°C, it is respectively supplied to the heating space at the upper and lower parts of the kiln car by the high-temperature air duct along the length direction of the roasting section. The high-temperature air is used as combustion-supporting air after heating the kiln car on both sides.
[0031] In the air-cooling section of the tunnel kiln, the high-temperature materials after reduction and the kiln car exchange heat with the return flue gas introduced from the outlet of the air-cooling section in a countercurrent manner, which can increase the temperature of the return flue gas from about 200°C to about 1100°C. The high-temperature return gas then flows into the roasting section and mixes with the high-temperature air supplied from the roasting section before burning. The high-temperature flue gas generated by the combustion exchanges heat with the materials and is discharged from the exhaust port of the roasting section. In the air-cooling section, when the upper surface temperature of the materials drops below 400°C, the kiln car is pushed out of the air-cooling section.
[0032] In the water cooling section of the tunnel kiln, spray cooling is used to cool the surface temperature of the material from about 400°C to below 200°C within 60 to 90 minutes. The spray cooling system pressurizes and filters the cooling water through a water pump and then atomizes it through an atomizing device. The atomized water with smaller particles can be cooled without contacting the material during the falling process. The present invention sets a plurality of atomizing nozzles along the length direction at the top of the tunnel kiln, which prolongs the spray cooling time of the high-temperature material. After the roasted ore is atomized and cooled, the temperature of the entire material is 150 to 200°C, and the material is in a dry state.
[0033] The present invention aims at the dusty and humid gas generated after the atomized water cools the material in the water cooling section of the tunnel kiln. In order to remove the dust in the gas and recover the steam, the dusty and humid gas is subjected to the vibrating screen to remove the dust and recover most of the water, and the purified gas is pressurized by the smoke extractor and discharged into the atmosphere through the chimney. The dusty sewage discharged from the bottom of the vibrating screen is cooled to about 30°C by the air cooling tower and then discharged into the sewage sedimentation tank for sedimentation. After removing most of the dust and mud from the sewage, it is passed into the sewage treatment tank for sewage treatment. The treated sewage is pressurized and filtered by the water pump and then returned to the vibrating screen for utilization.
[0034] In order to make the combustible gas generated by the gasification of the cover coal in the tunnel kiln burn in a dispersed state, the present invention arranges 5 to 8 hot air supply channels along the length direction on both sides of the roasting section of the tunnel kiln, and each hot air supply channel is provided with a flow control valve. The flow control valve controls the flow rate of preheated air supplied into different hot air supply channels, so that the combustible gas generated by the gasification of the cover coal in the tunnel kiln can be burned at different positions in the tunnel kiln, thereby realizing the adjustment of the temperature distribution of the roasting section of the tunnel kiln along the length direction of the kiln.
[0035] The present invention has the following beneficial effects compared with the prior art:
[0036] 1. The high-temperature flue gas discharged from the roasting section is subjected to waste heat recovery by a heat storage heat exchanger, so that the tunnel kiln can heat materials using coal as fuel without using external gas fuel;
[0037] 2. By extracting part of the high-temperature flue gas from the tunnel kiln preheating section to preheat the kiln car and materials, and returning the extracted reflux gas to the air cooling section as cooling gas for the high-temperature materials and the kiln car, the thermal shock stability of the kiln car can be improved while recovering the waste heat of the flue gas;
[0038] 3. By supplying excess air into the roasting section, the combustible components in the kiln gas can be completely burned while adjusting the temperature distribution of the roasting section to achieve standard emission of flue gas;
[0039] 4. The use of composite pelletizing technology and high-temperature roasted material spray cooling process shortens the direct reduction time of iron ore and the length of the tunnel kiln preheating and cooling sections, thereby reducing the production cost of direct reduction of iron ore. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 It is a structural schematic diagram of the heat storage tunnel kiln of the present invention;
[0041] In the figure: In the figure: 1-kiln car, 2-air inlet pipe, 3-exhaust pipe, 4-air guide pipe, 5-first smoke exhaust fan, 6-high-temperature air inlet pipe, 7-heat storage heat exchanger, 8-blower, 9-high-temperature air outlet pipe, 10-dust collector, 11-second smoke exhaust fan, 12-first chimney, 13-water reservoir, 14-first water pump, 15-first filter, 16-nozzle, 17-dust condenser, 18-air cooling tower, 19-sewage sedimentation tank, 20-third smoke exhaust fan, 21-second chimney, 22-second filter, 23-sewage treatment tank, 24-second water pump. DETAILED DESCRIPTION
[0042] The present invention will be further described below in conjunction with the accompanying drawings:
[0043] like Figure 1 As shown, a regenerative tunnel kiln with flue gas recirculation and high temperature section exhaust comprises a tunnel kiln body, a kiln car 1, a flue gas recirculation system, a regenerative heat exchange system, a dry dust removal system, a wet dust removal system and a spray cooling zone system. The tunnel kiln body comprises a preheating section, a roasting section, an air cooling section and a water cooling section from front to back. The flue gas recirculation system is arranged between the preheating section and the air cooling section, the regenerative heat exchange system is arranged on the roasting section, the dry dust removal system is arranged on the regenerative heat exchange system, and the wet dust removal system is arranged on the water cooling section.
[0044] The smoke return system is arranged between the preheating section and the air cooling section, and is used to guide the air in the preheating section into the air cooling section. It includes an air inlet pipe 2 arranged in the preheating section and an exhaust pipe 3 arranged in the air cooling section. The upper ends of the air inlet pipe 2 and the exhaust pipe 3 are both extended out of the tunnel kiln body. An air guide pipe 4 is connected between the air inlet pipe 2 and the exhaust pipe 3, and a first smoke exhaust fan 5 is arranged on the air guide pipe 4.
[0045] The regenerative heat exchange system is arranged on the roasting section, including a plurality of high-temperature air inlet pipes 6 arranged in the roasting section, the high-temperature air inlet pipes 6 extend out of the tunnel kiln body, and are connected to the inlet of the regenerative heat exchanger 7. The outlet of the regenerative heat exchanger 7 is connected with a high-temperature air outlet pipe 9, the head end of which extends into the roasting section of the tunnel kiln, and the regenerative heat exchanger 7 is also connected with a blower 8. The dry dust removal system includes a dust collector 10, a second smoke exhauster 11 and a first chimney 12 connected in sequence, and the inlet of the dust collector 10 is connected to the regenerative heat exchanger 7 through a pipeline. The upper end of the air inlet pipe 2 is connected to the tail end of the second smoke exhauster 11 through a pipeline.
[0046] The spray cooling zone system comprises a water reservoir 13, a first water pump 14, a first filter 15 and a plurality of nozzles 16 which are connected in sequence. The nozzles 16 are arranged on the top of the inner wall of the water cooling section.
[0047] The wet dust removal system includes a high-temperature moisture recovery pipe, the lower end of which extends into the water cooling section and the upper end is connected to the dust condenser 17. The bottom of the dust condenser 17 is connected to the air cooling tower 18, and the bottom of the air cooling tower 18 is connected to the sewage sedimentation tank 19; the side of the dust condenser 17 is connected to the third smoke exhaust fan 20 through a pipeline, and the tail end of the third smoke exhaust fan 20 is connected to the second chimney 21; the top of the dust condenser 17 is connected to the filter through a pipeline, and the bottom of the second filter 22 is connected to the sewage treatment tank 23 through the second water pump 24. The overflow of the sewage sedimentation tank 19 is connected to the sewage treatment tank 23. A sludge discharge pipe is provided at the bottom of the sewage sedimentation tank 19, and a sewage discharge pipe is connected to the bottom of the sewage sedimentation tank 19.
[0048] 1) After particle size classification, 0-30 mm iron ore is divided into three particle size ranges: 0-5 mm fine particles, 5-15 mm medium particles, and 15-30 mm coarse particles. The iron ore in each particle size range is mixed with reducing coal to form 20-25 mm composite pellets.
[0049] 2) Place a layer of bituminous coal with a particle size of 5-30 mm at the bottom of the kiln car material basin, place 3-5 layers of composite pellets on the bituminous coal layer, place a layer of coke with a particle size of 5-30 mm on the composite pellet layer, and place a layer of covering agent mainly made of siliceous material with a particle size of 5-10 mm on the top.
[0050] 3) The kiln car loaded with materials enters from the kiln entrance of the tunnel kiln body. When the kiln car passes through the preheating section, the materials are preheated to about 400°C by a part of the flue gas extracted from the preheating section. The coal begins to gasify and the iron ore begins to be reduced.
[0051] 4) After the kiln car enters the roasting section, the material is gradually heated to 1000-1100℃ by the high-temperature flue gas in the kiln, and the reduction rate of the iron ore is accelerated; when the kiln car enters the end of the roasting section, the reduction of the iron ore on the upper layer of the kiln car is basically completed; the high-temperature flue gas discharged from the roasting section passes through the regenerative heat exchanger and the temperature drops to about 200℃, and the low-temperature flue gas is discharged through the dust collector and the smoke exhaust fan, and is sent to the roasting section for utilization after being preheated with normal temperature air.
[0052] 5) When the kiln car enters the air cooling section, the materials and the kiln car are cooled by the reflux gas at about 200°C introduced from the outlet of the flue gas reflux system of the air cooling section, which can reduce the surface temperature of the material layer from about 1100°C to about 400°C within 60 to 90 minutes.
[0053] 6) After air cooling, the medium-temperature material enters the water cooling section again. The medium-temperature material is cooled by the atomized water sprayed from the top of the kiln. The atomized water absorbs heat and vaporizes into steam, which is extracted from the top of the water cooling section. The temperature of the medium-temperature material drops below 200°C and is discharged from the kiln outlet.
[0054] 7) In the water-cooling section of the tunnel kiln, the cooling water is pressurized and filtered by a water pump and then atomized to cool the high-temperature materials. The vaporized water is then passed through a vibrating screen for dust removal and water vapor recovery, air cooler for cooling, sludge sedimentation and treatment, and sewage treatment before being recycled into the system.
[0055] It should be noted that the above are only some embodiments of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and substitutions can be made without departing from the technical principles of the present invention. These improvements and substitutions should also be regarded as the scope of protection of the present invention.
Claims
1. A roasting process of a heat storage tunnel kiln with flue gas recirculation and high temperature section exhaust, Features: The regenerative tunnel kiln includes a tunnel kiln body, a kiln car, a flue gas recirculation system, a regenerative heat exchange system, a dry dust removal system, a wet dust removal system and a spray cooling zone system. The tunnel kiln body includes a preheating section, a roasting section, an air cooling section and a water cooling section from front to back; The flue gas recirculation system is arranged between the preheating section and the air cooling section, and is used to introduce the air of the preheating section into the air cooling section; the regenerative heat exchange system is arranged on the roasting section, the dry dust removal system is arranged on the regenerative heat exchange system, and the wet dust removal system is arranged on the water cooling section; The roasting process comprises the following steps: 1) After the particle size classification, the 0-30 mm iron ore is divided into three particle size ranges: 0-5 mm fine particles, 5-15 mm medium particles, and 15-30 mm coarse particles. The iron ore in each particle size range is mixed with the reducing coal to form 20-25 mm composite pellets; 2) Place a layer of bituminous coal with a particle size of 5 to 30 mm at the bottom of the kiln car material basin, place 3 to 5 layers of composite pellets on the bituminous coal layer, place a layer of coke with a particle size of 5 to 30 mm on the composite pellet layer, and place a layer of covering agent with a particle size of 5 to 10 mm, mainly made of siliceous materials, on the top; 3) The kiln car loaded with materials enters from the kiln entrance of the tunnel kiln body. When the kiln car passes through the preheating section, the materials are preheated to 400°C by a part of the flue gas extracted from the preheating section. The coal begins to gasify and the iron ore begins to be reduced. 4) After the kiln car enters the roasting section, the material is gradually heated to 1000-1100℃ by the high-temperature flue gas in the kiln, and the reduction rate of the iron ore is accelerated; when the kiln car enters the end of the roasting section, the reduction of the iron ore on the upper layer of the kiln car is basically completed; the high-temperature flue gas discharged from the roasting section is cooled to 200℃ after passing through the regenerative heat exchanger, and the low-temperature flue gas is discharged through the dust collector and the smoke exhauster, and the normal temperature air is preheated and sent to the roasting section for utilization; 5) When the kiln car enters the air cooling section, the material and the kiln car are cooled by the 200°C reflux gas introduced from the outlet of the flue gas reflux system of the air cooling section, so that the surface temperature of the roasting material layer is reduced from 1100°C to 400°C within 60 to 90 minutes; 6) After air cooling, the medium-temperature material enters the water cooling section again. The medium-temperature material is cooled by the atomized water sprayed from the top of the kiln. The atomized water absorbs heat and vaporizes into steam, which is drawn out from the top of the water cooling section. The temperature of the medium-temperature material drops to below 200°C and is discharged from the kiln outlet. 7) In the water-cooling section of the tunnel kiln, the cooling water is pressurized and filtered by a water pump and then atomized to cool the high-temperature materials. The vaporized water is then passed through a vibrating screen for dust removal and water vapor recovery, air cooler for cooling, sludge sedimentation and treatment, and sewage treatment before being recycled into the system.
2. The roasting process of the heat storage tunnel kiln with flue gas recirculation and high temperature section exhaust according to claim 1, It is characterized in that The smoke reflow system includes an air inlet duct arranged in the preheating section and an exhaust duct arranged in the air cooling section. The upper ends of the air inlet duct and the exhaust duct extend out of the tunnel kiln. An air guide duct is connected between the air inlet duct and the exhaust duct, and a first smoke exhaust fan is arranged on the air guide duct.
3. The roasting process of the heat storage tunnel kiln with flue gas reflow and high temperature section exhaust according to claim 2, It is characterized in that The regenerative heat exchange system includes a plurality of high-temperature air inlet pipes arranged in the roasting section, the high-temperature air inlet pipes extend out of the tunnel kiln, the high-temperature air inlet pipes are connected to the inlet of the regenerative heat exchanger, the outlet of the regenerative heat exchanger is connected to a high-temperature air outlet pipe, and the head end of the high-temperature air outlet pipe extends into the roasting section of the tunnel kiln; the regenerative heat exchanger is also connected to a blower.
4. The roasting process of the heat storage tunnel kiln with flue gas recirculation and high temperature section exhaust according to claim 3, It is characterized in that The dry dust removal system comprises a dust collector, a second smoke exhaust fan and a first chimney which are connected in sequence, and the inlet of the dust collector is connected to the heat storage heat exchanger through a pipeline.
5. The roasting process of the heat storage tunnel kiln with flue gas recirculation and high temperature section exhaust according to claim 4, It is characterized in that The upper end of the air inlet pipe is connected to the rear end of the second smoke extractor through a pipeline.
6. The roasting process of the heat storage tunnel kiln with flue gas recirculation and high temperature section exhaust according to claim 1, It is characterized in that The spray cooling zone system comprises a water reservoir, a first water pump, a first filter and a plurality of nozzles which are connected in sequence, and the nozzles are arranged on the top of the inner wall of the water cooling section.
7. The roasting process of the heat storage tunnel kiln with flue gas recirculation and high temperature section exhaust according to claim 6, It is characterized in that The wet dust removal system includes a high-temperature moisture recovery pipe, the lower end of which extends into the water cooling section and the upper end of which is connected to a dust condenser; the bottom of the dust condenser is connected to an air cooling tower, and the bottom of the air cooling tower is connected to a sewage sedimentation tank; the side of the dust condenser is connected to a third smoke exhaust fan through a pipe, and the tail end of the third smoke exhaust fan is connected to a second chimney; the top of the dust condenser is connected to a filter through a pipe, and the bottom of the second filter is connected to a sewage treatment tank through a second water pump.
Citation Information
Patent Citations
Hierarchical material distribution reduction method for sponge iron tunnel kiln and tunnel kiln applying same
CN103937921A
Novel heat accumulating type tunnel kiln for magnetizing roasting or direct reduction of iron ore
CN106369996A
Iron ore magnetizing roasting tunnel kiln and iron ore magnetizing roasting method
CN106854684A
Heat accumulating type tunnel kiln with smoke backflow and high-temperature section smoke exhaust functions
CN216049087U
Downstream type tunnel kiln for coal-based direct reduced iron and production process therefor
WO2014169442A1