A method and device for low temperature etching

Through low-temperature etching technology and the use of halogen gases, the charge accumulation problem in semiconductor devices is solved, the etching depth and morphological quality are improved, and high-efficiency etching of high-deep aspect ratio media is achieved.

CN113643973BActive Publication Date: 2024-11-08ADVANCED MICRO FAB EQUIP INC CHINA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010345284.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-04-27
Publication Date
2024-11-08
Estimated Expiration
2040-04-27

AI Technical Summary

Technical Problem

In the manufacturing process of semiconductor devices, especially in the deep hole or trench etching process of 3D NAND structures, charge accumulation leads to slowing down the etching rate and distorted and deformation of characteristic morphology, which is difficult to effectively solve in the prior art.

Method used

Using low-temperature etching technology, the halogen group and its compound gases generate conductivity at extremely low temperatures, combining reactants with the negative charge of the etched solid surface to reduce charge accumulation, and cooling the substrate to below- 20°C to improve etching efficiency.

Benefits of technology

It significantly improves the maximum etching depth and the morphological quality of the structure, reduces the characteristic deformation caused by charge accumulation, is suitable for etching of high-deep aspect ratio media, and improves the structural accuracy and stability after etching.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113643973B_ABST
    Figure CN113643973B_ABST
Patent Text Reader

Abstract

The present invention discloses a low-temperature etching method for a substrate, wherein the substrate comprises a dielectric material, and the method comprises: a) placing the substrate on a base of a cavity, wherein the base comprises a cooling channel having a flowing coolant therein, b) cooling the substrate to a cooling temperature by the coolant, wherein the cooling temperature is less than or equal to ‑20° C., and c) introducing an etching gas into the cavity to produce plasma, and etching the dielectric material of the substrate, wherein the etching gas comprises a halogen family element or a compound gas thereof. The present invention also discloses an etching device using the above method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a plasma processing method, and in particular to a method and a device for low-temperature etching a medium. Background Art

[0002] When manufacturing semiconductor devices, a frequently performed step is to form a columnar structure in a dielectric layer. This includes, but is not limited to, memory applications such as dynamic access random access memory (DRAM) and 3D NAND structures. For example, the etched layer can be etched to form holes or lines or other features of the memory. Some semiconductor devices can be formed by etching a single silicon dioxide (SiO2) stack to form a capacitor in (DRAM). Other semiconductor devices can also be formed by etching alternating silicon dioxide (oxide) and silicon nitride (nitride) (ONON) or alternating silicon dioxide and polysilicon double-layer stacks. With the development of semiconductor technology, the size of devices has become smaller and smaller, and the stack height has become higher and higher, that is, the aspect ratio of the etched features has become larger and larger. The process challenges of etching extremely high aspect ratio structures have become more and more severe, including the maximum depth that can be etched, the top / bottom critical dimension ratio, the control of the bow dimension, the morphology distortion, the degree of deformation, etc. Summary of the invention

[0003] On the one hand, the present invention provides a low-temperature etching method for a substrate, which includes a dielectric material. The method includes: placing the substrate on a base in a cavity, the base including a cooling channel with a flowing coolant therein; cooling the substrate to a cooling temperature by the coolant, the cooling temperature being less than or equal to -20°C; introducing an etching gas into the cavity to produce plasma, and etching the dielectric material of the substrate, the etching gas including a halogen family gas or a compound thereof.

[0004] Optionally, the temperature of the coolant is less than or equal to -30°C.

[0005] Optionally, the etching gas includes at least one of the following gases: F2, Cl2, HBr, NF3, SF6, and CBrF3.

[0006] Optionally, the cooling temperature is 10° C.-30° C. higher than the condensation temperature of the etching gas.

[0007] Optionally, the cooling temperature is 20° C. higher than the condensation temperature of the etching gas.

[0008] Optionally, the etching gas comprises Cl2, and the cooling temperature is -20°C to -40°C.

[0009] Optionally, the etching gas includes at least one of the following gases: NF3, SF6, CBrF3, and the cooling temperature is -40°C to -60°C.

[0010] Optionally, the etching gas includes at least one of the following gases: HBr, NF3, and the cooling temperature is -60°C to -80°C.

[0011] Optionally, the etching gas further includes at least one of the following gases: F2, CF4, O2, and H-containing gas.

[0012] Optionally, the etching gas includes a H-containing gas, and the H-containing gas includes CHF3 or C3H2F6.

[0013] Optionally, the dielectric material has a stacked structure, and the stacked structure includes at least one layer of silicon nitride, silicon carbide or silicon dioxide.

[0014] Optionally, the dielectric material includes a silicon nitride layer and a silicon dioxide layer, wherein the silicon nitride layer and the silicon dioxide layer are alternately arranged.

[0015] Optionally, the dielectric material includes a silicon dioxide layer and a polysilicon layer, wherein the silicon dioxide layer and the polysilicon layer are alternately arranged.

[0016] Optionally, the aspect ratio of the substrate after etching is greater than 50:1.

[0017] On the other hand, the present invention also provides a device for low-temperature etching of a substrate, wherein the substrate includes a dielectric material, and the device includes: a reaction chamber; a base, used to support the substrate and including a cooling channel for accommodating a flowing coolant; a gas inlet, used to introduce an etching gas into the reaction chamber; a plasma source; and a controller, wherein the controller is configured to: cool the substrate to a cooling temperature by means of a coolant, wherein the cooling temperature is less than or equal to -20°C; introduce an etching gas into the chamber to produce plasma, and etch the dielectric material of the substrate, wherein the etching gas includes halogen gas and its compound gas.

[0018] The present invention utilizes the strong polarity of halogen elements, uses single substances or compound gases containing F, Br, etc. as etchants, and utilizes the high adhesion of the reactants to the solid surface at extremely low temperatures to combine with the negative charges on the etched solid surface in a temperature range slightly higher than the condensation point, thereby generating conductivity or providing a charge migration channel. This can greatly improve the accumulation of charges on the etched feature surface, avoid the deflection of the ion bombardment direction caused by the accumulation of anisotropic charges on the side walls during the etching process, thereby increasing the maximum etching depth and improving the structural deformation after etching. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 A flow chart according to an embodiment of the method is shown.

[0020] Figure 2A and2B Schematic cross-sectional views of a substrate 200 before and after etching are shown according to one embodiment.

[0021] Figure 3 A schematic diagram of a plasma etching apparatus that can be used in one embodiment of the method is shown. DETAILED DESCRIPTION

[0022] To make the content of the present invention more clear and understandable, the content of the present invention is further described below in conjunction with the accompanying drawings of the specification. Of course, the present invention is not limited to this specific embodiment, and general replacements known to those skilled in the art are also covered within the protection scope of the present invention.

[0023] With the development of 3D NAND technology, the frequency of the bias RF source used for etching of extremely high aspect ratio media is getting lower and lower, the power is getting higher and higher, and the process time is getting longer and longer, and the charge accumulation problem caused by this is becoming more and more serious. This is because as the frequency of the bias voltage decreases and the power increases, the energy of the bombarding ions is also greater. In the process of etching deep holes or grooves, under the action of the acceleration voltage, these positively charged ions continuously bombard the holes or grooves and accumulate at the bottom, while negatively charged electrons cannot enter the holes or grooves in the same direction (on the contrary, the behavior of electrons is more "isotropic" than positive ions). As a result, as the depth of the holes or grooves increases, the accumulation of positive ions becomes more and more serious, which is called the "electron shielding" phenomenon. It is well known that the conductivity of the medium is extremely low. Etched materials such as silicon dioxide and silicon nitride, as well as byproducts such as fluorocarbon polymers produced during the etching process, are all dielectric materials, and the accumulated charges are difficult to migrate under the existing process conditions. Charge accumulation causes the etching rate of deep holes or trenches to slow down as their depth increases, which is also one of the reasons for the distortion of their characteristic morphology.

[0024] Low temperature etching provides a solution to the above problems. Generally speaking, low temperature etching refers to the operation of etching in an environment with a temperature equal to or lower than -20°C. Low temperature etching can be used for silicon etching or dielectric etching. In silicon etching, the reaction gas and silicon will spontaneously undergo chemical etching to desorb silicon byproducts, such as SiF4 or SiCl2. In dielectric etching, the situation is different. For silicon nitride, nitrogen fluoride can be used for chemical etching; for silicon dioxide, typical spontaneous reaction etching will not be performed, but ion etching will be mainly used, and reactants will be combined to accelerate desorption. Generally speaking, in the case of low temperature etching, halogen elements such as fluorine, chlorine, bromine, and iodine are used to etch silicon components; in the case of low temperature etching, elements such as carbon, hydrogen, sulfur, and nitrogen are used to etch oxygen components in silicon dioxide; and in the case of low temperature etching, elements such as hydrogen and fluorine are used to etch nitrogen elements in silicon nitride.

[0025] Low temperature etching has two properties. Spontaneous chemical etching of the dielectric is suppressed, which has a positive effect on the sidewalls of high aspect ratio contact holes or trenches. Also, the sticking coefficient increases as the temperature decreases. The sticking coefficient plays an important role in where and how reactants and deposits are generated.

[0026] The present invention adopts an extremely low temperature etching technology, and utilizes the characteristics of the highly polar halogen family and its compound gases themselves and / or the byproducts generated by their reaction with the etched material to generate conductivity at extremely low temperatures, thereby alleviating the charge accumulation problem of high depth ratio dielectric etching. The halogen family and its compound gases include F2, Cl2, HBr, NF3, SF6, CBrF3, etc. Since F, Cl, and Br in these substances have strong polarity, at low temperatures, due to the much higher adhesion coefficient than at normal temperatures, when they are adsorbed on the etched material and mask material on the surface of the wafer, they can easily combine with the negative charge on their surface to become negatively charged particles that can move along the sidewalls and bottom of the etched features. When encountering positive ions bombarding the etched features, their positive charges can be neutralized in time, thereby reducing the deformation or distortion of the features caused by charge accumulation. More specifically, during etching, the temperature near the substrate will be cooled to about 10°C-30°C higher than the condensation temperature of the above-mentioned halogen group and its compound gases, thereby forming a conductive film on the inner side walls and bottom walls of the contact hole to reduce the accumulation of charge in these places.

[0027] This low-temperature technology can be applied to the etching of the following structures: the stacking of polysilicon and silicon oxide in 3D NAND, the stacking of silicon oxide and silicon nitride, the memory in DRAM, etc. The aspect ratio of these structures is usually greater than 50:1.

[0028] This method is applicable to both capacitively coupled plasma etching devices and inductively coupled plasma etching devices. At extremely low temperatures, the longitudinal etching rate of the above-mentioned gas is much higher than the lateral etching rate, which has a protective effect on the sidewalls. It does not require the participation of gases such as C4F8 and C4F6 that produce a large amount of non-volatile polymer reactants. Therefore, it does not require very high ion bombardment energy, and etching can be achieved under low to medium ion energy bombardment. This method is also applicable to other types of plasma etching devices, such as electron cyclotron resonance plasma etching devices.

[0029] Figure 1 A flow chart according to an embodiment of the method is shown. In this embodiment, a substrate is placed in a plasma reaction chamber (step 100). The substrate includes a substrate and a dielectric material on the substrate, and the dielectric material includes a laminated structure. The substrate is cooled to a cooling temperature by a coolant (step 102). An etching gas is introduced into the reaction chamber (step 104). A plasma is ignited in the reaction chamber (step 106). The substrate is etched (step 108). A patterned mask is provided on the substrate for selective etching.

[0030] Figure 2A and 2B A schematic cross-sectional view of a substrate 200 before and after etching according to one embodiment is shown. In an exemplary embodiment, the substrate 200 is placed above a susceptor in a reaction chamber (step 100). In this embodiment, the substrate 200 includes a substrate 202 and a stacked structure 204 located above the substrate 202. A patterned mask 206 is provided above the stacked structure 204. In this example, one or more layers may be provided between the substrate 202 and the stacked structure 204 or between the stacked structure 204 and the patterned mask 206. In this example, the patterned mask 206 is a patterned mask containing carbon, such as amorphous carbon. This embodiment does not have a patterned mask containing silicon above the stacked structure 204 or above the patterned mask 206. In this example, the patterned mask pattern provides mask features for high aspect ratio contact holes. In some embodiments, the mask features are formed before the substrate 200 is placed in the reaction chamber. In other embodiments, the mask features are formed while the substrate 200 is in the reaction chamber 209. In this embodiment, the stacked structure 204 is a structure formed by alternating silicon dioxide layers 212 and silicon nitride layers 214 (ONON). In other embodiments, the stacked structure 204 may be a structure formed by alternating silicon dioxide layers and silicon carbide layers, or a structure formed by alternating silicon dioxide layers and polysilicon layers (OPOP). There may also be structures formed by alternating other materials, not limited to the above examples.

[0031] After the substrate 200 is placed in the reaction chamber, the substrate 200 is cooled using a coolant having a coolant temperature below -20°C (step 102). An etching gas is flowed into the reaction chamber (step 104). In this embodiment, the etching gas is a halogen family or compound gas thereof, such as NF3. In this embodiment, a pressure of 3 to 70 mTorr is provided. The etching gas forms an etching plasma (step 106). This can be achieved by providing an RF source having a frequency of 60 MHz and a power of 100 to 5000 W. The substrate 200 is exposed to the plasma. A bias voltage having an amplitude of at least about 400 volts is provided. In this embodiment, a high bias voltage having a frequency of 400 kHz and a power of 1 kW to 10 kW is provided to the ESC by an RF bias source. The bias voltage accelerates ions to bombard the substrate 200, causing selective etching. The plasma is maintained for 100 to 3000 seconds to etch the silicon dioxide layer 212 and the silicon nitride layer 214. A high aspect ratio etched feature is generated in the stack structure 204 relative to the carbon-containing patterned mask 206. After etching is completed, other processes can be performed on the substrate 200. The substrate 200 is then removed from the reaction chamber. In another embodiment, the frequency of the source power supply is 13.56 MHz, and the frequency of the bias power supply is 400 KHz or 2 MHz or 13.56 MHz, and their power range is 500 W to 10 KW.

[0032] Figure 2B is a schematic cross-sectional view of substrate 200 after etching according to one embodiment. The etched contact hole 220 is a high aspect ratio contact hole. Preferably, the aspect ratio of the height of the high aspect ratio contact hole 220 to the critical dimension (CD) width is greater than 30:1, in this embodiment, the CD is measured at the top of the contact hole. Other embodiments may have an aspect ratio greater than 50:1. The etching process is capable of selectively etching the silicon dioxide layer 212 and the silicon nitride layer 214 relative to the patterned mask 206, and the selectivity may be greater than 5:1 when etching the high aspect ratio contact hole. The resulting contact hole may reduce features such as bending, bowl-shaped, wide mouth and taper. In addition, this embodiment allows the use of a carbon-containing patterned mask, such as amorphous carbon, without the need for a silicon-containing mask such as polysilicon. Not using a silicon-containing mask can reduce costs and defects. Sidewall protection can be provided by polymer deposition. Polymer deposition is controlled by the concentration of carbon and oxygen, wherein a higher concentration of carbon increases sidewall deposition and a higher concentration of oxygen consumes deposited polymer. At the same time, higher oxygen concentration also increases the consumption of the mask.

[0033] In some embodiments, in order to cool the substrate to a temperature below -20°C, the coolant is cooled to a temperature below -30°C. In other embodiments, the coolant is cooled to a temperature between -30°C and -100°C. In other embodiments, the coolant is cooled to a temperature between -40°C and -100°C. In some embodiments, the coolant is cooled to a temperature between -30°C and -200°C. In the specification and claims, the substrate is cooled to "a cooling temperature" is defined as the substrate is etched at a temperature below -20°C, so that the temperature of the etching gas around the substrate to be etched is also below -20°C. Preferably, the substrate is etched at a cooling temperature below -40°C, and more preferably, the substrate is etched at a cooling temperature below -60°C. In other embodiments, the substrate can be etched at a cooling temperature below -100°C. Generally, etching at low temperature is etching at a temperature having one of the above ranges. In some embodiments, operation at low temperature cools the substrate 200 to a cooling temperature below -20° C. during a certain period of operation. In other embodiments, operation at low temperature maintains the substrate 200 at a cooling temperature below -20° C. during the entire operation. Obviously, due to the effect of heat conduction, the temperature of the coolant is lower than the cooling temperature of the substrate.

[0034] In some embodiments, the etching gas comprises one or more of F2, Cl2, HBr, NF3, SF6, CBrF3. In one embodiment, the etching gas is Cl2 combined with CF4, O2, and hydrogen-containing carbon fluoride gas (such as CHF3, C3H2F6, etc.). The temperature of Cl2 is between -20°C and -40°C. This temperature is about 20°C higher than the condensation temperature of the etching gas, so that a negatively charged conductive film is formed on the hole wall and the bottom of the contact hole to neutralize the positive ions accumulated by bombarding the substrate. In another embodiment, the etching gas is at least one of NF3, SF6, CBrF3 combined with O2 and hydrogen-containing carbon fluoride gas (such as CHF3, etc.), wherein the temperature of NF3, SF6, CBrF3 is between -40°C and -60°C. In another embodiment, the etching gas is at least one of HBr and NF3 combined with hydrogen-containing carbon fluoride gas (such as CHF3, etc.), wherein the temperature of HBr and NF3 is between -40°C and -60°C. In other embodiments, the etching gas further comprises at least one of the following gases: F2, CF4, O2, and H-containing gas, wherein the H-containing gas comprises CHF3 or C3H2F6.

[0035] When manufacturing a 3D NAND memory device, the ONON stacked structure can be etched to form features such as contact holes or trenches. Other embodiments can be used for etching of DRAM capacitors. Other embodiments can be used to etch silicon dioxide and polysilicon stacked structures (OPOP). Other embodiments provide an etching depth greater than 20 microns. In other embodiments, the etching depth is greater than 3 microns. In one embodiment, at least 96 layers of silicon dioxide and silicon nitride stacked structures are etched in a single etching step. In addition, the contact hole preferably has an aspect ratio greater than 30:1.

[0036] In the above embodiment, a bias voltage with a magnitude of 200 volts was used. It has been found that a bias voltage with a magnitude of 1000 volts will provide improved etching. And a bias voltage with a magnitude of 2000 volts will provide further improved etching. Higher bias voltages will produce higher aspect ratio etching.

[0037] In some embodiments, liquid nitrogen is used as a coolant that flows through cooling channels in the susceptor to cool the substrate. In other embodiments, other coolants may also be used for substrate cooling.

[0038] Figure 3 A schematic diagram of a plasma etching device that can be used in an embodiment is shown. The etching device is an inductively coupled plasma etching device, comprising a vacuum reaction chamber 100, the vacuum reaction chamber comprising a roughly cylindrical reaction chamber side wall 105 made of a metal material, an insulating material window 130 is arranged above the reaction chamber side wall 105, an inductor coil 140 is arranged above the insulating material window 130, and the inductor coil 140 is connected to a source radio frequency power source 145. Optionally, a heater layer 170 can be arranged between the insulating material window 130 and the inductor coil 140. A gas inlet 150 is arranged at one end of the reaction chamber side wall 105 close to the insulating material window 130, and the gas inlet 150 is connected to a gas supply device 10. A base 110 is arranged at a downstream position of the vacuum reaction chamber 100, and an electrostatic chuck 115 is placed on the base 110 for supporting and fixing a substrate 120. An exhaust pump 125 is also arranged below the vacuum reaction chamber 100 to discharge reaction byproducts from the vacuum reaction chamber.

[0039] Before the treatment process begins, the substrate 120 is transferred to the electrostatic chuck 115 above the base and fixed, the reaction gas in the gas supply device 10 enters the vacuum reaction chamber through the gas inlet 150, and then the source RF power source 145 is applied to the inductive coil 140. In the conventional technology, the inductive coupling coil is a multi-turn coil structure. The high-frequency alternating current output by the source RF power source 145 flows through the coupling coil and generates a changing magnetic field passing through the insulating material window 130. The changing magnetic field will generate a changing electric field in the vacuum reaction chamber 100, so that the reaction gas in the chamber is ionized to generate plasma 160. In the plasma etching process, the source power source 145 is applied to the inductive coupling coil assembly 140, mainly for controlling plasma dissociation or plasma density. The RF bias power source 146 applies bias power to the base 110 through the matching network 200. The role of the bias power source is to control the ion energy and its energy distribution.

[0040] The cooler 280 is connected to the cooling channel 270 in the susceptor 10, and provides a cooling liquid such as liquid nitrogen to the cooling channel to cool the upper substrate 120. The temperature controller 260 is connected to the cooler 280. In other embodiments, other types of plasma etching devices may also be used, such as a capacitive coupled plasma etching device, an electron cyclotron resonance plasma etching device, etc.

[0041] Although the present invention has been disclosed as above with preferred embodiments, the embodiments are merely examples for the convenience of description and are not intended to limit the present invention. Those skilled in the art may make several changes and modifications without departing from the spirit and scope of the present invention. The scope of protection claimed by the present invention shall be based on the claims.

Claims

1. A low temperature etching method for a substrate, wherein the substrate comprises a dielectric material and a patterned mask, the method comprising: a) placing the substrate on a susceptor in a chamber, the susceptor comprising a cooling channel having a coolant flowing therein, b) cooling the substrate to a cooling temperature by a coolant, wherein the cooling temperature is less than or equal to -20°C, c) introducing an etching gas into the chamber to generate plasma and etch the dielectric material of the substrate; The etching gas includes at least one of the following gases: F2, Cl2, NF3, SF6, CBrF3; The cooling temperature is 10°C-30°C higher than the condensation temperature of the etching gas; In the low temperature etching method, a bias voltage with an amplitude of at least 400 V and a pressure of 3 to 70 mTorr are provided in the chamber.

2. The method according to claim 1, characterized in that The temperature of the coolant is less than or equal to -30°C.

3. The method according to claim 1, characterized in that: The cooling temperature is 20° C. higher than the condensation temperature of the etching gas.

4. The method according to claim 1, characterized in that: The etching gas includes Cl2, and the cooling temperature is -20°C to -40°C.

5. The method according to claim 1, characterized in that The etching gas includes at least one of the following gases: NF3, SF6, CBrF3, and the cooling temperature is -40°C to -60°C.

6. The method according to any one of claims 4 to 5, characterized in that: The etching gas also includes at least one of the following gases: CF4, C2F6, O2, and H-containing gas.

7. The method according to claim 6, characterized in that The etching gas includes a H-containing gas, and the H-containing gas includes CHF3 or C3H2F6.

8. The method according to claim 1, characterized in that: The dielectric material has a stacked structure, and the stacked structure includes at least one layer of silicon nitride, silicon carbide or silicon dioxide.

9. The method according to claim 1, characterized in that: The dielectric material includes a silicon nitride layer and a silicon dioxide layer, wherein the silicon nitride layer and the silicon dioxide layer are alternately arranged.

10. The method according to claim 1, characterized in that The dielectric material includes a silicon dioxide layer and a polysilicon layer, wherein the silicon dioxide layer and the polysilicon layer are alternately arranged.

11. The method according to claim 1, characterized in that: The depth-to-width ratio of the substrate after etching is greater than 50:

1.

12. A device for low temperature etching of a substrate, the substrate comprising a dielectric material, the device comprising: Reaction chamber; a base for supporting the substrate and including a cooling channel for containing a flowing coolant; A gas inlet, used for introducing etching gas into the reaction chamber; Plasma source; and A controller, the controller being configured to: Cooling the substrate to a cooling temperature by a coolant, wherein the cooling temperature is less than or equal to -20°C; Introducing an etching gas into the reaction chamber to produce plasma and etch the dielectric material of the substrate; The etching gas includes at least one of the following gases: F2, Cl2, NF3, SF6, CBrF3; The cooling temperature is 10°C-30°C higher than the condensation temperature of the etching gas; During the low temperature etching process, a bias voltage with a magnitude of at least 400 volts and a pressure of 3 to 70 mTorr are provided in the chamber.