A tool for brazing a water-air thin-wall heat exchanger and a method of using the tool
By designing a tool including an upper pressure rod structure, a lower pressure rod structure, a press plate, a positioning sleeve, a compression spring and a nut, the problem that the traditional overall pressure brazing process cannot ensure the consistency of the fin welding joint compression force consistency is solved. , the quality of fin welding and the prevention of deformation and damage are achieved.
Patent Information
- Application Number
- CN202111163455.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-09-30
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2041-09-30
AI Technical Summary
The traditional overall pressure brazing process cannot effectively ensure the consistency of the compression force at the welding joints of the water-air thin-walled heat exchanger, which makes it difficult to guarantee the welding quality and is prone to damage due to deformation.
A tooling including an upper pressure rod structure, a lower pressure rod structure, a press plate, a positioning sleeve, a compression spring and a nut is designed. Through the combination of an intermediate pressure rod and a screw, the fine compression force adjustment of the fin welding joint is achieved. , and prevent deformation caused by excessive force through high-temperature springs and positioning sleeves.
The compression force adjustment at the fin welding joints is achieved, the welding quality is ensured, damage caused by deformation is prevented, and the stability of the welding process is ensured through the continuous compression force compensation of the spring.
Smart Images

Figure CN113714592B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of welding, and in particular to a tool for brazing a water-air thin-wall heat exchanger and a use method thereof. Background Art
[0002] With the development of microelectronics technology, the power consumption of chips is getting higher and higher. Traditional natural heat dissipation and forced air cooling can no longer solve the heat dissipation problem of chips. Compared with air cooling, liquid cooling is very efficient and is an effective way to solve the heat dissipation of high-power chips. In order to solve the heat dissipation problem of high-power chips, small liquid cooling systems are gradually used on electronic equipment. The pump draws the coolant from the liquid storage tank and flows into the liquid cooling shell of the liquid-cooled electronic board. The coolant absorbs the heat generated by the electronic device and the temperature rises. The coolant with increased temperature flows out of the electronic board and enters the heat exchanger. The air with lower temperature takes away the heat of the coolant during the flow of the heat exchanger, thereby achieving the purpose of reducing the temperature of the coolant. The coolant with reduced temperature flows into the liquid storage tank and enters the next cooling cycle. During the circulation of the small liquid cooling system, the electronic chip on the electronic board is cooled, so that the electronic equipment can work normally and reliably.
[0003] The heat exchanger is a key component in the liquid cooling system and an important component for achieving heat exchange between the coolant and the air. Its function is to exchange heat between the coolant and the air. The coolant with a higher temperature flowing into the heat exchanger becomes the coolant with a lower temperature and then flows out. Fins are welded on the outside of the liquid pipe, and the external cooling air blows towards the fins. When the hot coolant flows in the liquid pipe, the cooling air flows around the fins, and the heat of the coolant is transferred to the fins through the wall of the liquid cooling pipe. The cooling air absorbs this heat, thus achieving the purpose of lowering the coolant temperature.
[0004] The water-air thin-wall heat exchanger is a new type of heat exchanger, the thickness of its fins is only 0.1-0.2mm, and the distance between the fins is only a few millimeters. Because the welding adopts the brazing process, this will result in a lot of points that need to be welded in the entire heat exchanger. And because the brazing process requires the weld gap to be maintained between 0.05 and 0.1mm. Therefore, the traditional overall pressure method during brazing is not advisable and cannot guarantee the quality of the product. Summary of the invention
[0005] In view of this, the present invention provides a tool for brazing a water-air thin-wall heat exchanger and a method for using the tool. The tool can adjust the pressing force at all welding points of the fins to improve the welding quality.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is:
[0007] A tool for brazing a water-air thin-wall heat exchanger, comprising four pressure rod structures, wherein the pressure rod structure comprises a cross rod and a vertical rod; the vertical rod and a sliding rod parallel to the vertical rod are arranged on the cross rod at intervals, and the sliding rod and the vertical rod are perpendicular to the cross rod; the vertical rod is provided with a through hole along its axis; any two pressure rod structures are combined to form a group of pressure rod walls, wherein the sliding rod of one pressure rod structure is located in the through hole of its corresponding pressure rod structure;
[0008] The two groups of pressure rod walls are connected by an intermediate pressure rod; the vertical rod is also provided with a plurality of connecting columns perpendicular thereto, and the connecting columns are perpendicular to the cross rod; countersunk holes for matching the connecting columns are provided at both ends of the intermediate pressure rod;
[0009] The cross bar is also provided with studs, and the studs and vertical bars are respectively located on opposite sides of the cross bar; a pressure plate is arranged between the two groups of pressure bar walls, and both ends of the pressure plate are provided with opening grooves corresponding to the studs, and the pressure plate is installed on the two studs corresponding to the two groups of pressure bar walls through the opening grooves; the pressure plate is fixed by nuts installed on the studs.
[0010] Furthermore, the vertical rod and the sliding rod are located on the same side of the cross rod.
[0011] Furthermore, a compression spring is provided on the stud, and the compression spring is located between the pressure plate and the nut.
[0012] Furthermore, the compression spring jacket is provided with a positioning sleeve, and the inner diameter of the positioning sleeve is smaller than the outer diameter of the nut.
[0013] A method for using a water-air thin-wall heat exchanger brazing tool, using the water-air thin-wall heat exchanger brazing tool as described above, specifically comprising the following steps:
[0014] Step 1, inserting the middle pressure rods between the fins of the thin-wall heat exchanger in sequence;
[0015] Step 2, sequentially assembling the pressure rod structure, the pressure plate and the nut to complete the fixation between the tooling and the thin-wall heat exchanger;
[0016] Step 3, placing the thin-wall exchanger with the fixture fixed thereon into a brazing furnace for brazing;
[0017] Step 4, take out the brazed workpiece and remove the tooling to obtain a thin-wall heat exchanger.
[0018] Furthermore, the step 2 specifically includes: the first step, positioning the sliding rod of one of the pressure rod structures in the through hole of its corresponding pressure rod structure to complete the assembly of the pressure rod wall; the second step, installing the pressure rod wall onto the middle pressure rod of the step 1; the third step, installing the pressure plate and tightening the nut.
[0019] The beneficial effects of the above technical solution of the present invention are:
[0020] 1. The present invention can adjust the pressing force at all welding points of the fin to ensure the welding quality of the product.
[0021] 2. The positioning sleeve of the present invention can prevent excessive force from being applied to the workpiece during welding, which may cause damaging deformation of the workpiece. In addition, as the brazing material melts during welding, the compression spring begins to extend to provide continuous compression force compensation to the middle pressure rod, preventing insufficient compression force due to shrinkage of the workpiece, so that the middle pressure rod continues to compress the fins within a reliable range. This design can cope with the unbalanced deformation or local slight deformation of the workpiece during brazing, thereby enabling brazing to proceed smoothly and normally, ensuring the effect of brazing while also effectively preventing damage to the workpiece caused by deformation. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 It is a schematic structural diagram of an embodiment of the present invention.
[0023] Figure 2 2 is a schematic diagram of the structure of the pressure rod in an embodiment of the present invention.
[0024] Figure 3 Schematic diagram of the structure of the compression rod wall in an embodiment of the present invention.
[0025] Figure 4 It is a structural schematic diagram of a water-air thin-wall heat exchanger.
[0026] Figure 5 yes Figure 4 Schematic diagram of the internal structure.
[0027] In the figure: 1. upper pressure rod structure, 2. lower pressure rod structure, 3. pressure plate, 4. positioning sleeve, 5. clamping spring, 6. gasket, 7. clamping nut, 8. middle pressure rod, 9. fin, 10. micro-thin-wall copper tube, 121. pull beam, 122. slide rail, 123. pull rod, 124. connecting column, 125. screw. DETAILED DESCRIPTION
[0028] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments.
[0029] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0030] The fins of the water-to-air thin-wall heat exchanger are thin, which makes them easy to deform during welding. In addition, many welding points are required. The traditional overall pressure method during brazing cannot ensure effective connection at each welding point, and the quality of the product cannot be guaranteed. This embodiment creatively proposes this structure, which consists of an upper pressure rod structure 1, a lower pressure rod structure 2, a pressure plate 3, a positioning sleeve 4, a clamping spring 5, a gasket 6, a clamping nut 7, and an intermediate pressure rod 8.
[0031] Reference Figures 1 to 3 The upper pressure rod structure 1 is composed of an upper pressure rod structure left branch and an upper pressure rod structure right branch. The structures of the upper pressure rod structure left branch and the upper pressure rod structure right branch are the same.
[0032] The right branch of the upper pressure rod structure is composed of a tension beam 121, a slide rail 122, a tension rod 123, a connecting column 124 and a screw 125. The connecting columns 124 in the left branch and the right branch of the upper pressure rod structure are symmetrically distributed and respectively inserted into the two ends of the middle pressure rod 8, so that the middle pressure rod 8 can be driven to move up and down with the upper pressure rod structure or the lower pressure rod structure.
[0033] The screw rod 125 in the upper pressure rod structure passes through the pressure plate 3 and is connected to the clamping nut 7. A positioning sleeve 4 and a clamping spring 5 are provided between the pressure plate 3 and the clamping nut 7, both of which are provided on the screw rod 125. The clamping spring adopts a high-temperature spring, and the positioning sleeve can undergo a certain deformation in the up and down directions. Among them, the positioning sleeve 4 can be used to protect the clamping spring 5. The clamping spring 5 is located in the positioning sleeve 4. A gasket 6 is provided at the upper end of the positioning sleeve 4, and the gasket 6 is used to evenly transmit the pressure of the clamping nut 7 to the positioning sleeve 4 and the clamping nut 7.
[0034] The slide rail 122 in the upper pressure rod structure 1 cooperates with the pull rod 123 in the lower pressure rod structure 2 on the same side, and the slide rail 122 is embedded in the pull rod 123 to guide the slide rail 122 to move up and down. The distance that the pull rod 123 drives the middle pressure rod 8 to move up and down can be adjusted according to actual needs.
[0035] The connection between the various parts is achieved by precision cold welding technology.
[0036] Figure 4 It is a water-air thin-wall heat exchanger. This heat exchanger uses water channel thin-wall copper tubes to replace the traditional water cooling plate, which not only meets the requirements of use, but also greatly saves costs. Figure 5This is the structural layout diagram of the thin-walled copper tube 10 and the fin 9 on the water channel side and the air side. Because the brazing process is used, and the process requires the weld gap to be maintained between 0.05 and 0.1 mm. In addition, the wall thickness of the thin-walled water channel pipe is 0.6 mm, while the thickness of the wind side fin is only 0.2 mm, which belongs to the category of microchannels. Therefore, this will result in a lot of points that need to be welded in the entire heat exchanger. Therefore, it is not advisable to use the traditional overall pressure method during brazing, and the quality of the product cannot be guaranteed. Therefore, it is necessary to design a separate tooling for vacuum brazing of water-air thin-walled heat exchangers.
[0037] Figure 1 The design drawing of the tooling for brazing of water-air thin-walled heat exchanger is shown in the figure. The structure consists of an upper pressure rod structure 1, a lower pressure rod structure 2, a pressure plate 3, a positioning sleeve 4, a clamping spring 5, a gasket 6, a clamping nut 7, and an intermediate pressure rod 8. The core problem of the design of the tooling for brazing of water-air thin-walled heat exchanger is how to ensure that the two can ensure effective contact at the welding points where the thin-walled fins of the air duct and the thin-walled copper tube of the water duct contact each other. The direction of the force they receive at the adjacent welding points on the thin-walled fins of the air duct is opposite. Therefore, we first thought of applying a pressure rod between each thin-walled fin of the air duct so that it can apply the expected pressure to the thin-walled fin of the air duct according to the design requirements. There are two types of pressure rods, namely, an upper pressure rod and a lower pressure rod. The so-called upper pressure rod is a pressure rod that provides an upward pressure on the thin-walled fin of the air duct. The explanation of the lower pressure rod refers to the upper pressure rod. Therefore, we put forward a conception, which is to design the upper pressure rod structure 1 and the lower pressure rod structure 2 respectively.
[0038] The upper pressure rod structure 1 is composed of an upper pressure rod structure left branch and an upper pressure rod structure right branch. Figure 2 The structure of the left branch of the upper pressure rod structure is the same as that of the right branch of the upper pressure rod structure, and the middle pressure rod 8 is a 4×4×1 mm stainless steel square tube.
[0039] The right support of the upper pressure rod structure is composed of a tension beam 121, a slide rail 122, a tension rod 123, a connecting column 124 and a screw rod 125. Figure 2 The connecting columns 124 in the left and right branches of the upper pressure rod structure are symmetrically distributed and respectively inserted into the two ends of the middle pressure rod 8, so as to drive the middle pressure rod 8 to move up and down together with the structure.
[0040] The screw rod 125 in the upper pressure rod structure passes through the pressure plate 3 and is connected to the compression nut 7. Figure 1 As shown. Between the pressure plate 3 and the compression nut 7, there are provided a positioning sleeve 4 and a compression spring 5, both of which are inserted into the screw 125. The compression spring is a high-temperature spring, and the positioning sleeve can undergo certain deformation in the up and down directions. Among them, the positioning sleeve 4 can be used to protect the compression spring 5. The compression spring 5 is located in the positioning sleeve 4. A gasket 6 is provided at the upper end of the positioning sleeve 4, and the gasket 6 is used to evenly transmit the pressure of the compression nut 7 to the positioning sleeve 4 and the compression nut 7.
[0041] The positioning sleeve 4 can prevent excessive force from being applied to the workpiece during welding, which may cause damaging deformation of the workpiece. In addition, as the brazing material melts during welding, the compression spring begins to extend to provide continuous compression force compensation to the middle pressure rod, preventing insufficient compression force due to the contraction of the workpiece, so that the middle pressure rod continues to compress the fins within a reliable range. This design can cope with the uneven deformation or local slight deformation of the workpiece during brazing, so that brazing can proceed smoothly and normally, ensuring the effect of brazing while effectively preventing damage to the workpiece caused by deformation.
[0042] The slide rail 122 in the upper pressure rod structure 1 cooperates with the pull rod 123 in the lower pressure rod structure 2 on the same side. The slide rail 122 is embedded in the pull rod 123 to guide the slide rail 122 to move up and down. The distance that the pull rod 123 drives the middle pressure rod 8 to move up and down can be adjusted according to actual needs. In this example, the screw rod is an M6 screw rod, the pull beam is a 6×6×1mm stainless steel square tube, the pull rod is a 4×4×1mm stainless steel square tube, and the slide rail and the connecting column can be realized by an M2 stainless steel cylindrical pin. The connection between each part is realized by a precision cold welding process.
[0043] The specific brazing steps of the use method of this embodiment are as follows:
[0044] 1. Assembly of tooling:
[0045] The first step is to position the sliding rod of one of the pressure rod structures in the through hole of its corresponding pressure rod structure to complete the assembly of the pressure rod wall; the second step is to install the pressure rod wall onto the middle pressure rod; the third step is to insert the positioning sleeve, the compression spring, and the gasket into the screw rod in sequence and tighten them with the compression nut.
[0046] 2. Welding sequence:
[0047] ① If solder paste is used for soldering, the following steps are used:
[0048] 1) The intermediate pressure rod 8 is inserted into the fins in sequence, and the tooling is assembled according to the assembly steps of the above workpieces;
[0049] 2) After the above step 1) is completed, solder paste is applied to the welds of the fins in sequence;
[0050] 3) After the above step 2) is completed, put it into a brazing furnace for brazing;
[0051] 4) Take it out after welding, disassemble the tooling, and obtain a water-air thin-wall heat exchanger.
[0052] ② If welding is performed using welding pieces, the following steps are used:
[0053] 1) Place the welding piece on the fin to be welded, and then insert them into the heat exchanger together;
[0054] 2) Then insert the intermediate pressure rod 8 into the fins in sequence, and assemble the tooling according to the assembly steps of the workpiece;
[0055] 3) Then the whole assembly is placed in a brazing furnace for brazing;
[0056] 4) Take it out after welding, disassemble the tooling, and obtain a water-air thin-wall heat exchanger.
[0057] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A tool for brazing a water-air thin-wall heat exchanger, characterized in that: The invention comprises four compression rod structures, wherein the compression rod structures comprise a horizontal rod and a vertical rod; the vertical rod and a sliding rod parallel to the vertical rod are arranged on the horizontal rod at intervals, and the sliding rod and the vertical rod are perpendicular to the horizontal rod; the vertical rod is provided with a through hole along its axis; any two compression rod structures are combined to form a group of compression rod walls, wherein the sliding rod of one compression rod structure is located in the through hole of its corresponding compression rod structure; The two groups of pressure rod walls are connected by an intermediate pressure rod; the vertical rod is also provided with a plurality of connecting columns perpendicular thereto, and the connecting columns are perpendicular to the cross rod; countersunk holes for matching the connecting columns are provided at both ends of the intermediate pressure rod; The cross bar is also provided with studs, and the studs and the vertical bars are respectively located on opposite sides of the cross bar; a pressure plate is arranged between the two groups of pressure bar walls, and both ends of the pressure plate are provided with opening grooves corresponding to the studs, and the pressure plate is installed on the two studs corresponding to the two groups of pressure bar walls through the opening grooves; the pressure plate is fixed by nuts installed on the studs; The upper pressure rod structure is composed of a left support and a right support of the upper pressure rod structure, and the right support of the upper pressure rod structure is composed of a tension beam (121), a slide rail (122), a tension rod (123), a connecting column (124) and a screw rod (125); the left support of the upper pressure rod structure and the connecting column (124) of the right support are symmetrically distributed and respectively inserted into the two ends of the middle pressure rod (8); the screw rod (125) in the upper pressure rod structure passes through the pressure plate (3) and is connected to the clamping nut (7); a positioning sleeve (4) and a clamping spring (5) are provided between the pressure plate (3) and the clamping nut (7), both of which are inserted into the screw rod (125); the clamping spring adopts a high-temperature spring, and the positioning sleeve can undergo a certain deformation in the up and down directions; the clamping spring (5) is located in the positioning sleeve (4).
2. A tool for brazing a water-air thin-wall heat exchanger according to claim 1, characterized in that: The vertical rod and the sliding rod are located on the same side of the cross rod.
3. The tooling for brazing a water-air thin-wall heat exchanger according to claim 1, characterized in that: The stud is also provided with a compression spring, and the compression spring is located between the pressure plate and the nut.
4. The tooling for brazing a water-air thin-wall heat exchanger according to claim 3, characterized in that: The compression spring outer sleeve is provided with a positioning sleeve, and the inner diameter of the positioning sleeve is smaller than the outer diameter of the nut.
5. A method for using a tool for brazing a water-air thin-wall heat exchanger, characterized in that: Using a water-air thin-wall heat exchanger brazing tool as claimed in any one of claims 1 to 4, specifically The following steps are included: Step 1, inserting the middle pressure rods between the fins of the thin-wall heat exchanger in sequence; Step 2, sequentially assembling the pressure rod structure, the pressure plate and the nut to complete the fixation between the tooling and the thin-wall heat exchanger; Step 3, placing the thin-wall exchanger with the fixture fixed thereon into a brazing furnace for brazing; Step 4, take out the brazed workpiece and remove the tooling to obtain a thin-wall heat exchanger.
6. The method for using a water-air thin-wall heat exchanger brazing tool according to claim 5, characterized in that: The step 2 specifically includes: the first step is to insert the sliding rod of one of the pressure rod structures into the through hole of its corresponding pressure rod structure to complete the assembly of the pressure rod wall; the second step is to install the two sets of pressure rod walls to the two sides of the middle pressure rod of the step 1 respectively; the third step is to install the pressure plate and tighten the nut.