Silver film etching liquid composition, etching method using the same and metal pattern forming method

By adjusting the ratio of organic acid, inorganic acid and etching initiator in the silver film etching solution, combined with selective residual photoreactive substances and wet etching methods, the problem of residue and re-adsorption in silver film etching is solved, and efficient silver film etching is achieved. Film etching, suitable for high resolution and low power consumption display manufacturing.

CN113718258BActive Publication Date: 2024-10-15DONGWOO FINE CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110824226.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2017-11-17
Filing Date
2018-09-12
Publication Date
2024-10-15
Estimated Expiration
2038-09-12

AI Technical Summary

Technical Problem

The existing technology has problems with residue and re-adsorption when etching the silver film, resulting in uneven side etching, making it difficult to realize a high-resolution and low-power flat panel display device.

Method used

A silver film etching liquid composition is used, containing 40 to 65% by weight of organic acid, 5 to 10% by weight of inorganic acid and 1 to 15% by weight of etching initiator, with an etching termination index of 0.05 to 0.35, through selectivity Residual photoreactive substances and wet etching methods achieve appropriate etching speed and residue-free effects.

Benefits of technology

It effectively reduces side etching, avoids the occurrence of silver residue and indium oxide film residue, and improves the accuracy and efficiency of silver film etching. It is suitable for etching silver or silver alloy single-layer films and multi-layer films, and is suitable for display and other electronic components. manufacture.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003173055750000081
    Figure BDA0003173055750000081
  • Figure BDA0003173055750000101
    Figure BDA0003173055750000101
Patent Text Reader

Abstract

The invention relates to a silver film etching liquid composition, an etching method using the same and a metal pattern forming method. The silver film etching liquid composition comprises an organic acid, an inorganic acid, an etching initiator and a balance of water, and the etching termination index is 0.05 to 0.35.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of a Chinese patent application with an application date of September 12, 2018, application number 201811060633.6, and invention name “Silver film etching liquid composition, etching method using the same, and metal pattern forming method”. Technical Field

[0002] The invention relates to a silver film etching liquid composition, an etching method using the same and a metal pattern forming method. The silver film etching liquid composition comprises an organic acid, an inorganic acid, an etching initiator and water, and the etching termination index is 0.05 to 0.35. Background Art

[0003] As we enter the true information age, the field of displays for processing and displaying large amounts of information has developed rapidly, and in response, a variety of flat panel displays have been developed and attracted attention.

[0004] Examples of such flat panel display devices include liquid crystal display devices (LCD), plasma display panels (PDP), field emission display devices (FED), electroluminescence display devices (ELD), and organic light emitting diodes (OLED). Such flat panel display devices are used in various applications not only in the field of home appliances such as televisions and video recorders but also in computers such as notebooks and mobile phones. These flat panel display devices have rapidly replaced the cathode ray tubes (NITs) used in the past due to their excellent performance such as thinness, lightness, and low power consumption.

[0005] In particular, since OLED (organic light emitting diode) elements emit light themselves and can be driven at low voltage, OLED has been rapidly applied to small display markets such as portable devices in recent years. In addition, OLED is in the process of commercialization beyond small displays to large TVs.

[0006] In addition, conductive metals such as indium tin oxide (ITO) and indium zinc oxide (IZO) have excellent light transmittance and conductivity, and are therefore widely used as electrodes for color filters used in flat panel display devices. However, these metals also have high electrical resistance, which becomes an obstacle to achieving larger and higher resolution flat panel display devices by improving response speed.

[0007] In addition, in the case of reflectors, aluminum (Al) reflectors have been mainly used in products in the past, but in order to achieve low power consumption by increasing brightness, the material is being changed to a metal with higher reflectivity. For this reason, it is intended to achieve large-scale, high-resolution, and low-power consumption of flat-panel display devices by applying silver (Ag: specific resistance is about 1.59 μΩcm) films, silver alloys, or multilayer films containing the silver alloys, which have lower specific resistance and higher brightness than metals used in flat-panel display devices, to color filter electrodes, LCD or OLED wiring, and reflectors. Accordingly, it is required to develop an etching solution for applying the material.

[0008] However, silver (Ag) has very poor adhesion to lower substrates such as insulating substrates such as glass or semiconductor substrates composed of intrinsic amorphous silicon or doped amorphous silicon, making it difficult to deposit and easily inducing lifting or peeling of wiring. In addition, even when a silver (Ag) conductive layer is deposited on a substrate, an etching liquid is required to pattern the silver conductive layer. When an existing etching liquid is used as such an etching liquid, floating or peeling of wiring occurs due to excessive etching of silver (Ag) or uneven etching of silver (Ag), and the side profile of the wiring is poor.

[0009] Furthermore, there are difficulties in performing a low skew implementation process for achieving high resolution.

[0010] In particular, silver (Ag) is a metal that is easily reduced. Due to its fast etching speed, silver can be etched without producing residue. However, due to the fast etching speed of silver, there is no difference in etching speed between the upper and lower parts, and it is difficult to form a taper angle after etching and to ensure the straightness of each pattern. Therefore, there are many limitations when applying silver to wiring.

[0011] When the metal film stands vertically without a taper angle, gaps may occur between silver (Ag) and the insulating film or wiring when an insulating film or subsequent wiring is formed in a subsequent process, and such gaps may cause defects such as electrical short circuits.

[0012] Therefore, research for improving etching characteristics is actively conducted. As a representative example, Korean Patent No. 10-579421 proposes a silver etching liquid composition containing nitric acid, phosphoric acid, acetic acid, an auxiliary oxide dissolving agent, a fluorine-containing carbon-based surfactant and water. However, the problem of Ag over-etching and re-adsorption cannot be completely solved in this technical field. Therefore, the development of an etching liquid composition capable of improving the etching characteristics of silver is required, and active research is conducted in response to the requirements, but an etching liquid composition having significantly improved etching characteristics compared with the prior art has not yet been proposed.

[0013] Prior art literature

[0014] Patent Literature

[0015] Patent Document 1: Korean Patent No. 10-0579421 Summary of the invention

[0016] Technical issues

[0017] The present invention aims to provide a silver thin film etching liquid composition for etching a single-layer film composed of silver or a silver alloy or a multi-layer film composed of the single-layer film and an indium oxide film, which has an appropriate etching rate without the problem of residue (e.g., silver residue and / or indium oxide film residue) and the problem of silver re-adsorption, thereby reducing side etching.

[0018] In addition, the present invention provides an etching method using the silver thin film etching solution composition.

[0019] In addition, the present invention provides a metal pattern forming method using the silver thin film etching solution composition.

[0020] Means used to solve problems

[0021] In order to achieve the above object, the present invention relates to a silver thin film etching liquid composition and an etching method using the same. More specifically, a silver thin film etching liquid composition is provided, which comprises, relative to the total weight of the composition, 40 to 65 weight % of an organic acid, 5 to 10 weight % of an inorganic acid, 1 to 15 weight % of an etching initiator, and water in an amount such that the total weight of the composition becomes 100 weight %.

[0022] In addition, the present invention provides an etching method, comprising the following steps: forming a single-layer film composed of silver or a silver alloy or a multi-layer film composed of the single-layer film and an indium oxide film on a substrate; selectively leaving a photoreactive substance on the single-layer film composed of silver or a silver alloy or a multi-layer film composed of the single-layer film and an indium oxide film; and etching the single-layer film composed of silver or a silver alloy or a multi-layer film composed of the single-layer film and an indium oxide film using the silver thin film etching liquid composition.

[0023] In addition, the present invention provides a method for forming a metal pattern, comprising the following steps: forming a single-layer film composed of silver or a silver alloy or a multi-layer film composed of the single-layer film and an indium oxide film; selectively leaving a photoreactive substance on the single-layer film composed of silver or a silver alloy or a multi-layer film composed of the single-layer film and an indium oxide film; and etching the single-layer film composed of silver or a silver alloy or a multi-layer film composed of the single-layer film and an indium oxide film using the silver thin film etching solution composition.

[0024] Effects of the Invention

[0025] The silver thin film etching liquid composition of the present invention has an appropriate etching rate without causing problems of residue (e.g., silver residue and / or indium oxide film residue) and silver re-adsorption, and thus has an effect of reducing side etching. Accordingly, the silver thin film etching liquid composition has an excellent effect as a silver thin film etching liquid composition for etching a single-layer film composed of silver or a silver alloy or a multi-layer film composed of the single-layer film and an indium oxide film. DETAILED DESCRIPTION

[0026] Hereinafter, the present invention will be described in more detail.

[0027] The invention relates to a silver film etching liquid composition. The silver film etching liquid composition comprises, relative to the total weight of the composition, 40 to 65 weight % of an organic acid, 5 to 10 weight % of an inorganic acid, 1 to 15 weight % of an etching initiator and a balance of water such that the total weight of the composition becomes 100 weight %.

[0028] The present invention has an appropriate etching rate without the problem of residue (e.g., silver residue and / or indium oxide film residue) and the problem of silver re-adsorption, thereby reducing side etching (Side Etch), and exhibits excellent effects as a silver thin film etching liquid composition for etching a single-layer film composed of silver or a silver alloy or a multi-layer film composed of the single-layer film and an indium oxide film, thereby completing the present invention.

[0029] Specifically, the etching liquid composition of the present invention is characterized in that the etching termination index calculated as follows is 0.05 to 0.35,

[0030] Etch stop index = (inorganic acid + initiator) / (organic acid + water).

[0031] The etching stop index is an index of the ratio of the content of the inorganic acid and initiator used to accelerate the etching rate (Etch rate) to the organic acid used to chelate the metal. It has been experimentally confirmed that when the etching stop index is 0.05 to 0.35, when a single-layer film composed of silver or a silver alloy or a multi-layer film composed of the single-layer film and an indium oxide film is etched, an appropriate etching rate is achieved without problems with residue (for example, silver residue and / or indium oxide film residue) and silver re-adsorption, thereby having the effect of reducing side etching.

[0032] The silver thin film etching liquid composition of the present invention is characterized in that it can etch a single-layer film composed of silver (Ag) or a silver alloy or a multi-layer film composed of the single-layer film and an indium oxide film, and the silver thin film etching liquid composition can etch the multi-layer film simultaneously.

[0033] The silver alloy has silver as the main component and may have various forms including alloys of other metals such as Nd, Cu, Pd, Nb, Ni, Mo, Ni, Cr, Mg, W and Ti, and silver nitride, silicide, carbide and oxide forms, but is not limited to these.

[0034] In addition, the indium oxide is at least one selected from the group consisting of indium tin oxide (ITO), indium zinc oxide (IZO), indium tin zinc oxide (ITZO), and indium gallium zinc oxide (IGZO).

[0035] In addition, the multilayer film can be a multilayer film formed by indium oxide film / silver, indium oxide film / silver alloy, indium oxide film / silver / indium oxide film, or indium oxide film / silver alloy / indium oxide film. When the silver thin film etching liquid composition of the present invention is used, it has an appropriate etching rate without the problem of residue (for example, silver residue and indium oxide film residue) and the problem of silver re-adsorption, so it will not cause side etching and can be effectively applied to wet etching.

[0036] The organic acid contained in the silver thin film etching solution composition of the present invention is a component used as a main oxidant, and performs wet etching by oxidizing silver (Ag) and the transparent conductive film in the transparent conductive film / Ag / transparent conductive film.

[0037] The silver thin film etching solution composition contains 40 to 65 wt % of the organic acid, preferably 43 to 63 wt % of the organic acid, relative to the total weight of the silver thin film etching solution composition.

[0038] When the content of the organic acid is less than 40 wt % relative to the total weight of the composition, there may be disadvantages caused by a decrease in the silver etching rate and the generation of silver residues. When the content of the organic acid is greater than 65 wt % relative to the total weight of the composition, there may be a disadvantage that the etching rate of the transparent conductive film and the silver etching rate are too fast, resulting in over-etching, which may cause problems in subsequent processes.

[0039] The organic acid contained in the silver thin film etching solution of the present invention can be one or more selected from the group consisting of acetic acid, butyric acid, citric acid, formic acid, gluconic acid, glycolic acid, malonic acid, oxalic acid, valeric acid, methanesulfonic acid, benzenesulfonic acid, sulfosuccinic acid, sulfophthalic acid, salicylic acid, sulfosalicylic acid, benzoic acid, lactic acid, glyceric acid, succinic acid, malic acid, tartaric acid, isocitric acid, acrylic acid, iminodiacetic acid and ethylenediaminetetraacetic acid, and more preferably acetic acid and citric acid can be contained.

[0040] The inorganic acid contained in the silver thin film etching solution composition of the present invention is a component used as an etching improving agent, and performs wet etching by oxidizing silver (Ag) and the transparent conductive film in the transparent conductive film / Ag / transparent conductive film.

[0041] The silver thin film etching solution composition contains 5 to 10 wt % of the inorganic acid, preferably 6 to 9 wt % of the inorganic acid, relative to the total weight of the silver thin film etching solution composition.

[0042] When the content of the inorganic acid is less than 5 wt % relative to the total weight of the composition, the etching rates of silver (Ag) and the transparent conductive film are reduced, thereby deteriorating the etching uniformity in the substrate and causing streaks. When the content of the inorganic acid is greater than 10 wt % relative to the total weight of the composition, there is a disadvantage that over-etching occurs due to the accelerated etching rates of the upper and lower transparent conductive films and the Ag film, resulting in pattern loss.

[0043] The inorganic acid contained in the silver thin film etching solution of the present invention may be one or more selected from the group consisting of nitric acid, sulfuric acid and hydrochloric acid.

[0044] The etching initiator contained in the silver thin film etching solution composition of the present invention is a component used as an etching rate regulator, and plays a role in accelerating the etching rate of oxides and Ag metal.

[0045] The etching initiator is contained in an amount of 1 to 15 wt % relative to the total weight of the silver thin film etching solution composition, and preferably 3 to 12 wt % of the etching initiator.

[0046] When the content of the etching initiator is less than 1 wt % relative to the total weight of the composition, the etching rate is slow. When the content of the etching initiator is greater than 15 wt % relative to the total weight of the composition, the etching rate may increase and a tip of the upper transparent conductive film may occur, causing problems in subsequent processes.

[0047] The etching initiator contained in the silver thin film etching solution of the present invention may be one or more selected from the group consisting of peroxide initiators, alkali metal initiators and transition metal initiators.

[0048] The peroxide initiator may be one or more selected from the group consisting of sodium persulfate, ammonium persulfate, potassium persulfate, potassium permonosulfate complex salt and oxalic acid.

[0049] The alkali metal initiator may be at least one selected from the group consisting of sodium nitrate, potassium nitrate, calcium nitrate, sodium sulfate, potassium sulfate, calcium sulfate, sodium chloride, calcium chloride, and potassium chloride.

[0050] The transition metal initiator may be one or more selected from the group consisting of ferrous nitrate, ferric nitrate, ferrous sulfate, and ferric sulfate.

[0051] As water contained in the silver thin film etching solution composition of the present invention, deionized water for semiconductor processes can be used, preferably water with an ion concentration of 18 MΩ / cm or more, and water is contained in an amount equal to 100% by weight of the total weight of the composition.

[0052] The silver thin film etching liquid composition of the present invention can be effectively used as a wet etching liquid using a single-layer film of silver / silver alloy or a multilayer structure using two or more films such as the single-layer film and an indium oxide film, wherein the single-layer film and the multilayer structure are widely used to form TFT array substrates, TSP (touch screen panel) trace wiring and flexible nanowire wiring for displays (OLED, LCD, etc.). In addition, in addition to the above-mentioned displays and TSPs, it can also be used for electronic component materials using the metal film quality of semiconductors, etc.

[0053] Furthermore, the present invention relates to an etching method comprising the following steps:

[0054] forming a single-layer film composed of silver or a silver alloy or a multi-layer film composed of the single-layer film and an indium oxide film on a substrate;

[0055] selectively leaving a photoreactive substance on the single-layer film composed of silver or a silver alloy or a multi-layer film composed of the single-layer film and an indium oxide film; and

[0056] The silver thin film etching solution composition is used to etch the single-layer film composed of silver or a silver alloy or the multi-layer film composed of the single-layer film and an indium oxide film.

[0057] Furthermore, the present invention relates to a method for forming a metal pattern, comprising the following steps:

[0058] forming a single-layer film composed of silver or a silver alloy or a multi-layer film composed of the single-layer film and an indium oxide film; and

[0059] The silver thin film etching solution composition is used to etch the single-layer film composed of silver or a silver alloy or the multi-layer film composed of the single-layer film and an indium oxide film.

[0060] Below, the present invention is described in more detail by examples. However, the following examples are used to more specifically illustrate the present invention, and the scope of the present invention is not limited by the following examples. Those skilled in the art can appropriately modify and change the following examples within the scope of the present invention.

[0061] <Preparation of Silver Thin Film Etching Solution Composition>

[0062] Examples 1 to 7 and Comparative Examples 1 to 3

[0063] The silver thin film etching solution composition was prepared by including the corresponding components in the amounts described in the following Table 1. Etch stop refers to an etching stop phenomenon in which no further etching occurs when the conditions of the etching solution composition are changed, and is a parameter that can predict that the value of side etching will not increase before SEM (scanning electron microscope) measurement.

[0064] The etching termination index of the present invention is (inorganic acid + initiator) / (organic acid + water), and the preferred range of the etching termination index is 0.05 to 0.35. The etching termination index is an index of the ratio of the content of the inorganic acid and the initiator used to accelerate the etching rate (Etch rate) to the organic acid used to chelate the metal, and it can predict in advance whether the S / E increases due to the result based on the ratio.

[0065] [Table 1]

[0066] (Unit: weight %)

[0067]

[0068] Experimental Example 1. Performance test of silver etching solution composition

[0069] An ITO / Ag / ITO triple film is formed on a substrate, and an etching process is performed using an experimental device (model name: ETCHER (TFT), SEMES company) of a jet etching method. The silver etching liquid compositions of the above-mentioned embodiments 1 to 7 and comparative examples 1 to 3 are added to the experimental device respectively, and the temperature is set to 40°C and then heated up, and then when the temperature reaches 40±0.1°C, the etching process of the ITO / Ag / ITO triple film is performed. The total etching time is set to 60 seconds and implemented. In the experiment, after evaluating the silver etching liquid composition using the initial time (0 time), the same silver etching composition is used for re-evaluation after 12 hours and 24 hours respectively.

[0070] 1. Measuring Silver Residue

[0071] The silver etching liquid compositions of Examples 1 to 7 and Comparative Examples 1 to 3 were added to a jet etching experimental device (model name: ETCHER (TFT), SEMES), respectively, and the temperature was set to 40° C. and then raised. When the temperature reached 40±0.1° C., the etching process of the test piece was performed. The total etching time was set to 60 seconds.

[0072] After placing the substrate in the experimental device, spraying was started. When the etching time of 60 seconds was up, the substrate was taken out and washed with deionized water, dried with a hot air drying device, and the photoresist was removed with a photoresist stripper (PRstripper). After washing and drying, the phenomenon that silver (Ag) remained in the part not covered by the photoresist without being etched was measured using an electron scanning microscope (SEM; model name: SU-8010, manufactured by Hitachi) and the residue was evaluated using the following standards. The results are shown in the following Table 2.

[0073] <Residue measurement evaluation criteria>

[0074] ○: Good [no residue]

[0075] ×: Defective [Residue occurs]

[0076] 2. Measuring Silver Re-adsorption

[0077] The silver etching liquid compositions of Examples 1 to 7 and Comparative Examples 1 to 3 were added to a jet etching experimental device (model name: ETCHER (TFT), SEMES), respectively, and the temperature was set to 40° C. and then raised. When the temperature reached 40±0.1° C., the etching process of the test piece was performed. The total etching time was set to 60 seconds.

[0078] After placing the substrate in the experimental device, spraying was started. When the etching time of 60 seconds was up, the substrate was taken out and washed with deionized water, and then dried using a hot air drying device. After washing and drying, the substrate was cut and the cross section was measured using an electron scanning microscope (SEM; model name: SU-8010, manufactured by Hitachi). The number of Ag adsorbed on the upper Ti of Ti / Al / Ti in the S / D part was measured and evaluated using the following criteria. The results are shown in the following Table 2.

[0079] <Silver Re-adsorption Evaluation Criteria>

[0080] ○: Good [less than 50]

[0081] ×: Defective [more than 50 pieces]

[0082] 3. Measure the etching rate EPD

[0083] Regarding the etching rate EPD, the time from when the substrate was exposed to the chemical reagent to when the metal portion of the substrate was etched away was measured using a timer, and the results are shown in Table 2 below.

[0084] 4. Measure Side Etch

[0085] After cleaning and drying, the substrate was cut and the cross section was measured using a scanning electron microscope (SEM; model name: SU-8010, manufactured by Hitachi, Ltd.) At this time, the distance from the patterned PR terminal to the etched metal terminal was measured, and the results are shown in Table 2 below.

[0086] [Table 2]

[0087]

[0088] When the examples and comparative examples of the present invention are examined, in the composition within the content range, the S / E increases as the etching time increases, and it is found that the etching end index derived as follows deviates from 0.05 to 0.35.

[0089] Etching termination index = (inorganic acid + initiator) / (organic acid + water)

[0090] Furthermore, it was confirmed that the etching solution composition of the present invention has an excellent effect as an etching solution composition due to reduction of silver (Ag) residue, silver (Ag) re-adsorption, or reduction of side etching caused by an appropriate etching rate.

Claims

1. A silver film etching liquid composition, wherein the silver film etching liquid composition comprises an organic acid, an inorganic acid, an etching initiator and water, and an etching stop index is 0.05 to 0.35, wherein the etching stop index is calculated according to the following formula: Etching termination index = (content of inorganic acid + content of etching initiator) / (content of organic acid + content of water), wherein the organic acid comprises acetic acid and citric acid, and The silver film etching solution composition comprises 5 wt % to 10 wt % of the inorganic acid relative to the total weight of the silver film etching solution composition, wherein the inorganic acid is nitric acid.

2. The silver thin film etching liquid composition according to claim 1, wherein The silver thin film etching solution composition comprises, relative to the total weight of the composition, 40 wt % to 65 wt % of an organic acid, 5 wt % to 10 wt % of an inorganic acid, 1 wt % to 15 wt % of an etching initiator, and a balance of water such that the total weight of the composition is 100 wt %.

3. The silver thin film etching liquid composition according to claim 1, characterized in that, The etching initiator includes at least one selected from the group consisting of a peroxide initiator, an alkali metal initiator, and a transition metal initiator.

4. The silver thin film etching liquid composition according to claim 3, characterized in that, The peroxide initiator includes at least one selected from the group consisting of sodium persulfate, ammonium persulfate, potassium persulfate, potassium permonosulfate composite salt and oxalic acid.

5. The silver thin film etching liquid composition according to claim 3, characterized in that, The alkali metal initiator includes at least one selected from the group consisting of sodium nitrate, potassium nitrate, calcium nitrate, sodium sulfate, potassium sulfate, calcium sulfate, sodium chloride, calcium chloride, and potassium chloride.

6. The silver thin film etching liquid composition according to claim 3, characterized in that: The transition metal initiator includes at least one selected from the group consisting of ferrous nitrate, ferric nitrate, ferrous sulfate, and ferric sulfate.

7. The silver thin film etching liquid composition according to claim 1, characterized in that, The silver thin film etching solution composition can simultaneously etch a single-layer film composed of silver or a silver alloy or a multi-layer film composed of the single-layer film and an indium oxide film.

8. The silver thin film etching liquid composition according to claim 7, characterized in that, The indium oxide film is one or more selected from the group consisting of indium tin oxide, indium zinc oxide, indium tin zinc oxide, and indium gallium zinc oxide.

9. The silver thin film etching liquid composition according to claim 7, characterized in that, The multilayer film composed of the single layer film and the indium oxide film is indium oxide film / silver, indium oxide film / silver alloy, indium oxide film / silver / indium oxide film, or indium oxide film / silver alloy / indium oxide film.

10. An etching method comprising the following steps: forming a single-layer film composed of silver or a silver alloy or a multi-layer film composed of the single-layer film and an indium oxide film on a substrate; selectively leaving a photoreactive substance on the single-layer film composed of silver or a silver alloy or a multi-layer film composed of the single-layer film and an indium oxide film; as well as The single-layer film composed of silver or a silver alloy or a multi-layer film composed of the single-layer film and an indium oxide film is etched using the composition according to claim 1.

11. A method for forming a metal pattern, comprising the following steps: forming a single-layer film composed of silver or a silver alloy or a multi-layer film composed of the single-layer film and an indium oxide film; as well as The single-layer film composed of silver or a silver alloy or a multi-layer film composed of the single-layer film and an indium oxide film is etched using the composition according to claim 1.