Zn-ZSM-5 / ZSM-11 catalyst and preparation method thereof, and method for producing aromatic hydrocarbons
Through the one-step in-situ synthesis of zinc-loaded Zn-ZSM-5/ZSM-11 catalysts, the problem of easy carbon deposition and deactivation of the catalyst and harsh reaction conditions in the aromatization reaction of methanol-coupled light hydrocarbons was solved, and efficient aromatic hydrocarbons were achieved. production, improving product yield and selectivity.
Patent Information
- Application Number
- CN202010466404.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-05-28
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2040-05-28
AI Technical Summary
Existing catalysts are prone to carbon deposition and deactivation in the aromatization reaction of methanol-coupled light hydrocarbons. The reaction conditions are harsh, the product yield is low, and the selectivity is poor. It is difficult to effectively utilize the application value of light hydrocarbons.
The zinc-loaded Zn-ZSM-5/ZSM-11 catalyst was synthesized in situ using a one-step method. By adjusting the molar ratio of silicon source, alkali raw material, aluminum source, template agent and zinc source, hierarchical pores were prepared by hydrothermal crystallization method. Structured catalysts, combined with copper exchange and roasting treatments, improve the activity and stability of the catalyst.
It achieves effective catalysis of the aromatization coupling reaction of methanol and light hydrocarbons under mild reaction conditions, prolongs the service life of the catalyst, improves the yield of the product and the selectivity of aromatic hydrocarbons, and solves the problem of easy carbon deposition and deactivation of the catalyst.
Smart Images

Figure HDA0002512797230000011 
Figure HDA0002512797230000012
Abstract
Description
Technical Field
[0001] The invention relates to a Zn-ZSM-5 / ZSM-11 catalyst and a preparation method thereof, as well as a method for producing aromatic hydrocarbons. The catalyst can be particularly used for catalyzing the aromatization reaction of methanol coupled with light hydrocarbons. Background Art
[0002] As an important basic chemical raw material, the demand for aromatics continues to grow. More than 85% of aromatics in my country come from the petroleum production process, and aromatics preparation technology has also developed rapidly.
[0003] Light hydrocarbons (such as reforming top oil and raffinate produced during oil processing) are by-products of refineries with low added value. They are usually used as raw materials for the production of ethylene and propylene. However, with the lightness of cracking raw materials, the utilization of light hydrocarbons is limited to a certain extent, making it difficult to exert their application value. Light hydrocarbon aromatization technology provides a way for its comprehensive utilization. At present, a variety of light hydrocarbon aromatization technologies have been developed at home and abroad. However, the aromatization process of light hydrocarbons often requires a higher reaction temperature and the product yield is low, resulting in low utilization efficiency. In recent years, with the rapid development of coal chemical industry, methanol production has increased sharply, and the corresponding research on methanol aromatization technology has also been favored by many researchers. However, the methanol aromatization reaction is a highly exothermic reaction, which makes the catalyst easily deactivated by carbon deposition. How to overcome the rapid accumulation of heat during the reaction and extend the life of the catalyst has become a difficult problem that must be solved. Therefore, the technology of preparing aromatics by coupling methanol with light hydrocarbons, which combines the petroleum route and coal chemical industry, has a good development prospect. The same catalyst is used to catalyze the aromatization coupling reaction of methanol and light hydrocarbons (light hydrocarbons are added during the methanol aromatization reaction for aromatization coupling reaction). Thermal coupling is used to make the reaction process mild, extend the service life of the catalyst, and improve the product yield and aromatics selectivity. This is of great significance for the actual production of aromatics.
[0004] In 1972, Mobil Corporation first developed the ZSM-5 molecular sieve, which is a high-silicon five-membered ring zeolite. Its basic structural unit is the TO4 (T is Si or Al atom) tetrahedron, which is composed of eight five-membered rings and has two types of lateral channels: straight cylindrical and "Z"-shaped. ZSM-5 molecular sieve is widely used in various fields of petrochemical industry for its unique channel structure, controllability, ion exchange, thermal stability and excellent catalytic performance; ZSM-11 molecular sieve, another member of the Pentasil family, was developed by Mobil Corporation in the United States in the 1970s. ZSM-11 belongs to the tetragonal crystal system and is composed of three-dimensional cross-sections of ten-membered ring straight channels parallel to the a-axis and b-axis directions. The channel size is Compared with the complex Zig-Zag pores of ZSM-5, the unique straight pore structure of ZSM-11 makes the diffusion distance shorter, making it easier for reactants and products to enter and exit the ZSM-11 pores, and the diffusion rate is faster. At the same time, it also reduces the possibility of side reactions, making ZSM-11 exhibit better catalytic performance in many reactions.
[0005] ZSM-5 / ZSM-11 eutectic molecular sieve is a new type of zeolite molecular sieve with an intermediate structure of ZSM-5 and ZSM-11, which was first disclosed by Mobil Corporation of the United States in 1980 (US4229424). At present, there are few studies and reports on ZSM-5 / ZSM-11 eutectic molecular sieves, and the improvement of its structure and performance, optimization of synthesis methods and application are still in the exploratory stage. Chinese patent CN104624226B discloses a ZSM-5 and ZSM-11 eutectic molecular sieve and its preparation and application. The molecular sieve preparation method is as follows: (1) adding an aluminum source, a portion of an alkali and a ZSM-5 seed crystal to deionized water, and stirring the mixed solution at a constant temperature of 0-30°C for 2-25 hours to obtain a working solution 1; (2) mixing an organic template, a portion of an alkali and deionized water to obtain a working solution 2; (3) adding the working solution 2 to the working solution 1 under continuous stirring to prepare a mixed glue until the mixture is uniformly mixed; (4) stirring the mixed glue for 0.1-5 hours, and then adding a silicon source to the mixed glue. (5) placing the reactor in an oven at 110-140°C for crystallization for 12-36 hours, and continuing to crystallize in an oven at 160-180°C for 12-36 hours under autogenous pressure; (6) rapidly cooling the material after the crystallization reaction to room temperature, separating the solid and the mother liquor, washing with deionized water to a pH of 8-9, and drying at 100°C for 10 hours to obtain a ZSM-5 / ZSM-11 eutectic molecular sieve; wherein the molar ratio of the raw materials is: Al2O3: (60-700)SiO2: (0.08-0.18)TBA + :(0.5-5Wt%)Seeds:(10-20)H2O. The ZSM-5 / ZSM-11 eutectic molecular sieve disclosed in the scheme is used to catalyze methanol and / or dimethyl ether to produce propylene. In one implementation result, the methanol conversion rate is 100%, the light olefin yield is maintained at 55-58%, the propylene yield is 48%, and the P / E ratio is 9.
[0006] Zinc (Zn) contributes to aromatization. Introducing zinc into some molecular sieves can, to a certain extent, make them exhibit a catalytic effect on aromatization reactions. However, the traditional way of introducing Zn is basically to prepare molecular sieves first and then load zinc. The preparation process is relatively complicated, and the catalytic performance of the prepared catalyst is limited. At present, there are no reports on the one-step in-situ synthesis of ZSM-5 / ZSM-11 eutectic molecular sieve catalysts loaded with Zn (Zn-ZSM-5 / ZSM-11 catalysts) and the use of such catalysts to catalyze the aromatization reaction of methanol coupled to light hydrocarbons. In order to broaden the catalysts used for the aromatization reaction of methanol coupled to light hydrocarbons, and to solve a series of problems such as harsh aromatization reaction conditions, easy carbon deposition and deactivation of catalysts, low product yield / poor selectivity, etc. at this stage, it is an important issue faced by those skilled in the art to optimize the synthesis process and develop new aromatization catalysts. Summary of the invention
[0007] The invention provides a method for preparing a Zn-ZSM-5 / ZSM-11 catalyst. The method adopts a one-step method to in-situ synthesize the Zn-ZSM-5 / ZSM-11 catalyst. The preparation process is simple, and the prepared Zn-ZSM-5 / ZSM-11 catalyst has good catalytic activity and other properties.
[0008] The present invention also provides a Zn-ZSM-5 / ZSM-11 catalyst, which has good catalytic activity and other properties and can effectively catalyze the aromatization coupling reaction of methanol and light hydrocarbons.
[0009] The present invention also provides a method for producing aromatics, which realizes the aromatization coupling reaction of methanol and light hydrocarbons and has a high product yield and aromatics selectivity.
[0010] In one aspect of the present invention, a method for preparing a Zn-ZSM-5 / ZSM-11 catalyst is provided, comprising:
[0011] (1) adding a silicon source and an alkali raw material into water to obtain a mixed solution A;
[0012] (2) adding an aluminum source, a template and a zinc source to the mixed solution A, and refluxing the reaction system at 80-150° C. for 2-8 hours to obtain a mixed solution B;
[0013] (3) allowing the mixed solution B to crystallize at 130-170° C. for 18-96 hours to obtain a mixed solution C;
[0014] (4) cooling the mixed solution C to room temperature, filtering, washing, and drying, and then subjecting the obtained solid product to a first calcination treatment to obtain a catalyst precursor;
[0015] (5) exchanging the catalyst precursor with ammonium, and subjecting the exchange product to a second calcination treatment to obtain a Zn-ZSM-5 / ZSM-11 catalyst;
[0016] Among them, the added amounts of silicon source, alkali raw material, aluminum source, template, zinc source and water are controlled to meet the following molar ratio: SiO2:Na2O:Al2O3:template:Zn:H2O=(30-190):(2.0-15.0):1.0:(0.30-5.00):(0.5-8.0):(1200-4000).
[0017] The catalyst prepared by the preparation method provided by the present invention is a multi-level pore (containing micropores (pore diameter <2μm), mesopores (pore diameter 2-50μm), and macropores (pore diameter >50μm)) Zn-ZSM-5 / ZSM-11 catalyst (a multi-level pore ZSM-5 / ZSM-11 eutectic molecular sieve catalyst loaded with Zn). The present invention adopts a one-step method to in-situ synthesize the catalyst, and the preparation process is simple and efficient, and the catalyst can have excellent properties such as good catalytic activity, which is specifically manifested in that the catalyst can effectively catalyze the aromatization coupling reaction of methanol and light hydrocarbon raw materials (such as reforming top oil, raffinate oil, etc.), is not easy to be deactivated by carbon deposition during the reaction, has a long service life, and can achieve a high liquid yield and aromatics selectivity in the reaction.
[0018] In one embodiment of the present invention, the added amounts of silicon source, alkali raw material, aluminum source, template, zinc source and water can be controlled to satisfy the following molar ratio: SiO2:Na2O:Al2O3:template:Zn:H2O=(40-175):(3.0-10.0):1.0:(0.3-2.5):(1.5-4.0):(1600-3600), which is beneficial to the preparation of the above-mentioned Zn-ZSM-5 / ZSM-11 catalyst and makes the catalyst have more excellent catalytic performance.
[0019] Specifically, in the implementation process of the present invention, in step (1), the silicon source and the alkali raw material can generally be added to water and stirred at 10-50° C. for 2-10 hours to obtain a mixed solution A. This operating condition can disperse and mix the silicon source and the alkali raw material, which is more conducive to obtaining the Zn-ZSM-5 / ZSM-11 catalyst with the above-mentioned excellent performance. Taking into account factors such as catalyst performance and reaction efficiency, the above-mentioned stirring temperature can further be 20-30° C., and the stirring time can further be 2-5 hours or 3-5 hours.
[0020] Furthermore, in the above step (2), the aluminum source, template and zinc source are added to the mixed solution A, and the mixture can be stirred at 10-50°C and then the reaction system is refluxed, which is conducive to the sufficient contact reaction of the raw materials. In specific operations, the stirring time can generally be 2-6 hours. For example, in one embodiment of the present invention, the aluminum source, template and zinc source are added to the mixed solution A, and the mixture can be stirred at 20-45°C or 20-30°C, and the specific stirring time can be 2-4 hours.
[0021] In addition, the present invention can further optimize the following conditions to facilitate the synthesis of the above-mentioned Zn-ZSM-5 / ZSM-11 catalyst with excellent performance: in step (2), the reaction system can be refluxed at 90-120°C for 2-5 hours to obtain a mixed solution B; and / or, in step (3), the mixed solution B is crystallized at 140-170°C for 18-72 hours, and further crystallized at 150-170°C for 20-36 hours to obtain a mixed solution C.
[0022] In the present invention, the silicon source can generally be selected from at least one of silica sol, silica gel and tetraethyl orthosilicate, and / or the alkali raw material can be selected from at least one of sodium hydroxide, potassium hydroxide and calcium hydroxide. Generally, the silicon source and the alkali raw material can be directly added to water for mixed reaction, or the silicon source and the aqueous solution containing the alkali raw material can be added to water for mixed reaction.
[0023] Further, the aluminum source can be selected from at least one of aluminum sulfate, sodium aluminate, aluminum chloride, aluminum nitrate, aluminum isopropoxide, and aluminum hydroxide, and / or the template can be selected from at least one of tetrabutylammonium hydroxide, tetrabutylammonium bromide, and n-hexylamine, and / or the zinc source can be selected from at least one of zinc nitrate, zinc chloride, and zinc sulfate.
[0024] Generally, in step (4), the mixed solution C is cooled to room temperature, filtered, and the filter cake is washed to a pH of 8-9, and then dried to obtain the above-mentioned solid product; wherein the drying temperature can be 80-120° C. and the drying time can be 4-8 hours.
[0025] Specifically, in the present invention, the catalyst precursor obtained in step (4) is a Zn-NaZSM-5 / ZSM-11 molecular sieve (i.e., a sodium-type ZSM-5 / ZSM-11 eutectic molecular sieve loaded with Zn). In specific implementation, the first calcination treatment can generally include: heating the solid product to 500-550°C and calcining for 4-6 hours to obtain a catalyst precursor; wherein the heating rate is controlled to be 1-5°C / min, and can further be 2-3°C / min.
[0026] The above catalyst precursor is subjected to ammonium exchange to achieve conversion from sodium type to hydrogen type. In the specific implementation process of the present invention, ammonium exchange can generally be carried out using an ammonium salt solution, the concentration of the ammonium salt solution can be 0.5-1 mol / L, the ammonium exchange temperature can be 70-90° C., and the ammonium exchange time is 2-6 hours. Among them, the ammonium salt can be a commonly used ammonium salt in the art, such as ammonium nitrate, ammonium chloride, etc.
[0027] After the ammonium exchange is completed, the exchange product can generally be dried first, for example, at 80-120° C. for 4-8 hours. In specific operations, the above ammonium exchange + drying steps can generally be performed 1-3 times, and then the exchange product is subjected to a second calcination treatment.
[0028] After ammonium exchange and a second calcination treatment, a Zn-HZSM-5 / ZSM-11 molecular sieve catalyst (i.e., a hydrogen-type ZSM-5 / ZSM-11 eutectic molecular sieve loaded with Zn) is obtained. Specifically, in the implementation process of the present invention, the second calcination treatment generally may include: heating the exchange product to 500-550°C and calcining for 4-6h to obtain a Zn-ZSM-5 / ZSM-11 catalyst; wherein the heating rate is controlled to be 1-5°C / min, and may further be 2-3°C / min.
[0029] Generally, the molecular sieve can also be subjected to molding processing, such as mixing the molecular sieve with additives such as a binder and then extruding it into strips, so as to facilitate its use. In one embodiment of the present invention, it can also specifically include: after subjecting the exchange product to a second calcination treatment, mixing the second calcination product with a binder to form the product, drying the formed product at 80-120°C for 4-8 hours, and then calcining it at 500-550°C for 4-6 hours to obtain a Zn-ZSM-5 / ZSM-11 catalyst product; wherein the binder can be pseudo-boehmite and / or silica sol, and the mass ratio of the second calcination product to the binder can be 7:(2-4), for example, 7:3.
[0030] Another aspect of the present invention provides a Zn-ZSM-5 / ZSM-11 catalyst prepared according to the above preparation method.
[0031] The catalyst of the present invention is a multi-level porous ZSM-5 / ZSM-11 eutectic molecular sieve catalyst loaded with Zn. The catalyst has excellent properties such as high catalytic activity. According to tests, it can effectively catalyze the aromatization coupling reaction of methanol and light hydrocarbon raw materials, improve the reaction efficiency, liquid yield and aromatics selectivity, and is not prone to carbon deposition and deactivation during the reaction process, and has a long service life.
[0032] In another aspect of the present invention, a method for producing aromatics is provided, comprising: using the above-mentioned Zn-ZSM-5 / ZSM-11 catalyst to catalyze the aromatization reaction of methanol and light hydrocarbon feedstock to obtain aromatics products.
[0033] Specifically, the aromatization reaction conditions are generally as follows: temperature of 300-500°C, further 350-450°C, such as 400°C, pressure of 0.1-1MPa, such as 0.5MPa, feed mass space velocity of 1.0-2.0h -1 , for example, it can be 1.5h -1 The mass ratio of methanol to light hydrocarbon feedstock can generally be 1:9-9:1 (i.e., the mass ratio of the two is calculated based on 10 parts of methanol + light hydrocarbon feedstock), for example, it can be 5:5. Among them, the light hydrocarbon feedstock can generally include reforming top oil and raffinate oil, and of course, it can also be other lighter hydrocarbon feedstocks, such as one or a mixture of alkanes below C10, cycloalkanes, etc.
[0034] According to tests, the method for producing aromatics of the present invention can generally achieve a liquid yield of more than 85% and an aromatics selectivity of more than 40%.
[0035] In the implementation process of the present invention, the above aromatization reaction can generally be carried out in a fixed bed reactor. In specific implementation, the materials to be reacted (methanol and light hydrocarbon raw materials) can be mixed with diluent gas and introduced into a fixed bed reactor filled with a catalyst for aromatization reaction, wherein the flow rate of the diluent gas can be controlled to be 15-25 ml / min, for example, 20 ml / min. The present invention does not impose any particular restrictions on the diluent gas used, and it can be a commonly used diluent gas in the art, such as nitrogen (N2), etc.
[0036] The implementation of the present invention has at least the following beneficial effects:
[0037] The invention provides a method for preparing a Zn-ZSM-5 / ZSM-11 catalyst, which adopts an in-situ hydrothermal crystallization method to synthesize a multi-level porous Zn-ZSM-5 / ZSM-11 eutectic molecular sieve catalyst in one step, and has the advantages of simple preparation process and high efficiency, and the prepared catalyst has good catalytic activity and other properties.
[0038] The Zn-ZSM-5 / ZSM-11 catalyst provided by the present invention has excellent properties such as high catalytic activity, and can effectively catalyze the aromatization coupling reaction of methanol and light hydrocarbon raw materials, thereby improving the liquid yield and aromatics selectivity.
[0039] The method for producing aromatics provided by the present invention adopts the above-mentioned Zn-ZSM-5 / ZSM-11 catalyst to catalyze the aromatization coupling reaction of methanol and light hydrocarbon raw materials to prepare aromatic products. The reaction conditions are mild and a high liquid yield and aromatics selectivity can be achieved. The technical problems existing in the prior art such as harsh aromatization reaction conditions, easy carbon deposition and deactivation of the catalyst, low product yield / poor selectivity, etc. can be effectively solved. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 is the XRD spectrum of Zn-ZSM-5 / ZSM-11 prepared by the present invention;
[0041] Figure 2 It is a N2 adsorption-desorption curve diagram of Zn-ZSM-5 / ZSM-11 prepared in the present invention, wherein the ordinate is the adsorption volume (Volume) and the abscissa is the relative pressure (P / P0). DETAILED DESCRIPTION
[0042] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0043] Example 1
[0044] 1. Preparation of Zn-ZSM-5 / ZSM-11 catalyst (cat1)
[0045] Add 100 g of silica sol and 12 ml of 4 mol / L sodium hydroxide solution into 200 g of deionized water, and stir at 25°C for 2 h to obtain a mixed solution A1;
[0046] Add 5 ml of 1.2 mol / L aluminum sulfate solution, 1.54 g of tetrabutylammonium hydroxide and 2.75 g of zinc nitrate to the mixed solution A1, stir at 25°C for 2 h, and then reflux at 90°C for 4 h to obtain a mixed solution B1 (the molar ratio of SiO2:Na2O:Al2O3:template:Zn:H2O is about 83.3:4.0:1.0:0.98:1.54:1851);
[0047] The mixed solution B1 was transferred to a crystallization reactor with a polytetrafluoroethylene liner and hydrothermally crystallized at 150°C for 36 hours to obtain a mixed solution C1;
[0048] The mixed solution C1 was cooled to room temperature, filtered, washed to pH=8-9, and dried at 100°C for 6 hours. The obtained solid product was placed in a muffle furnace and calcined at 550°C from room temperature at a heating rate of 2-3°C / min for 4 hours to obtain Zn-NaZSM-5 / ZSM-11 molecular sieve;
[0049] The Zn-NaZSM-5 / ZSM-11 molecular sieve was immersed in a 1 mol / L ammonium chloride solution, exchanged at 85°C for 2 hours, filtered and washed, and dried at 100°C for 6 hours, and repeated three times (i.e., the exchange, filtration, washing and drying process was performed three times). The exchange product was placed in a muffle furnace, and the temperature was increased from room temperature to 550°C at a rate of 2-3°C / min for 4 hours to obtain a Zn-HZSM-5 / ZSM-11 molecular sieve;
[0050] The Zn-HZSM-5 / ZSM-11 molecular sieve and pseudo-boehmite were uniformly mixed in a ratio of 7:3 (mass ratio) and then extruded into strips. The molded product was dried at 100°C for 6 hours and then calcined at 550°C for 4 hours to obtain a Zn-ZSM-5 / ZSM-11 catalyst, which was recorded as cat1.
[0051] 2. Aromatization reaction
[0052] Using cat1 as catalyst, the aromatization coupling reaction of methanol and raffinate oil was carried out in a fixed bed reactor. The reaction conditions were: the mass ratio of methanol to raffinate oil was 5:5, the reaction temperature was 400℃, the pressure was 0.5MPa, the nitrogen flow rate was 20ml / min, and the total feed mass space velocity was 1.5h -1 ; Samples were taken for analysis after 48 hours of reaction.
[0053] The analysis results show that the methanol conversion rate is basically 100%, the liquid yield is 89.51%, and the aromatics selectivity is 49.31%.
[0054] In the following Examples 2 to 10, unless otherwise specified, the conditions for the ammonium exchange step to obtain the Zn-ZSM-5 / ZSM-11 catalyst are the same as those in Example 1 and are not described in detail.
[0055] Example 2
[0056] 1. Preparation of Zn-ZSM-5 / ZSM-11 catalyst (cat2)
[0057] Add 210 g of silica sol and 15 ml of 4 mol / L sodium hydroxide solution into 180 g of deionized water, and stir at 25° C. for 3 h to obtain a mixed solution A2;
[0058] Add 5 ml of 1.2 mol / L aluminum sulfate solution, 2.86 g of tetrabutylammonium hydroxide and 2.75 g of zinc nitrate to the mixed solution A2, stir at 30°C for 3.5 h, and then reflux at 90°C for 4 h to obtain a mixed solution B2 (the molar ratio of SiO2:Na2O:Al2O3:template:Zn:H2O is about 175.0:5.0:1.0:1.84:1.54:1666.7);
[0059] The mixed solution B2 was transferred to a crystallization reactor with a polytetrafluoroethylene lining and hydrothermally crystallized at 150°C for 36 hours to obtain a mixed solution C2;
[0060] The mixed solution C2 was cooled to room temperature, filtered, washed to pH=8-9, and dried at 100°C for 6h. The obtained solid product was placed in a muffle furnace and calcined at 550°C from room temperature at a heating rate of 2-3°C / min for 4h to obtain Zn-NaZSM-5 / ZSM-11 molecular sieve;
[0061] After ammonium exchange and molding treatment, a Zn-ZSM-5 / ZSM-11 catalyst was obtained, which was denoted as cat2.
[0062] 2. Aromatization reaction
[0063] Using cat2 as the catalyst, an aromatization coupling reaction of methanol and raffinate oil (mass ratio 5:5) was carried out according to the reaction conditions of Example 1, and samples were taken for analysis after 48 hours of reaction.
[0064] The analysis results show that the methanol conversion rate is basically 100%, the liquid yield is 87.67%, and the aromatics selectivity is 44.26%.
[0065] Example 3
[0066] 1. Preparation of Zn-ZSM-5 / ZSM-11 catalyst (cat3)
[0067] Add 48 g of silica sol and 9 ml of 4 mol / L sodium hydroxide solution into 200 g of deionized water, and stir at 25°C for 3 h to obtain a mixed solution A3;
[0068] Add 5 ml of 1.2 mol / L aluminum sulfate solution, 1.47 g of tetrabutylammonium hydroxide and 2.75 g of zinc nitrate to the mixed solution A3, stir at 45°C for 3.5 h, and then reflux at 100°C for 5 h to obtain a mixed solution B3 (the molar ratio of SiO2:Na2O:Al2O3:template:Zn:H2O is about 40.0:3.0:1.0:0.94:1.54:1851);
[0069] The mixed solution B3 was transferred to a crystallization reactor with a polytetrafluoroethylene lining and hydrothermally crystallized at 150°C for 36 hours to obtain a mixed solution C3;
[0070] The mixed solution C3 was cooled to room temperature, filtered, washed to pH=8-9, and dried at 100°C for 6h. The obtained solid product was placed in a muffle furnace and calcined at 550°C from room temperature at a heating rate of 2-3°C / min for 4h to obtain Zn-NaZSM-5 / ZSM-11 molecular sieve;
[0071] After ammonium exchange and molding treatment, a Zn-ZSM-5 / ZSM-11 catalyst was obtained, which was denoted as cat3.
[0072] 2. Aromatization reaction
[0073] Using cat3 as a catalyst, an aromatization coupling reaction of methanol and raffinate oil (mass ratio 5:5) was carried out according to the reaction conditions of Example 1, and samples were taken for analysis after 48 hours of reaction.
[0074] The analysis results show that the methanol conversion rate is basically 100%, the liquid yield is 90.12%, and the aromatics selectivity is 52.68%.
[0075] Example 4
[0076] 1. Preparation of Zn-ZSM-5 / ZSM-11 catalyst (cat4)
[0077] Add 100 g of silica sol and 12 ml of 4 mol / L sodium hydroxide solution into 200 g of deionized water, and stir at 25° C. for 4 h to obtain a mixed solution A4;
[0078] Add 5 ml of 1.2 mol / L aluminum sulfate solution, 2.54 g of tetrabutylammonium hydroxide and 2.75 g of zinc nitrate to the mixed solution A4, stir at 25°C for 3 h, and then reflux at 90°C for 3 h to obtain a mixed solution B4 (the molar ratio of SiO2:Na2O:Al2O3:template:Zn:H2O is about 83.3:4.0:1.0:1.63:1.54:1851);
[0079] The mixed solution B4 was transferred to a crystallization reactor with a polytetrafluoroethylene lining and hydrothermally crystallized at 170°C for 24 hours to obtain a mixed solution C4;
[0080] The mixed solution C4 was cooled to room temperature, filtered, washed to pH=8-9, and dried at 100°C for 6h. The obtained solid product was placed in a muffle furnace and calcined at 550°C from room temperature at a heating rate of 2-3°C / min for 4h to obtain Zn-NaZSM-5 / ZSM-11 molecular sieve;
[0081] After ammonium exchange and molding treatment, a Zn-ZSM-5 / ZSM-11 catalyst was obtained, which was denoted as cat4.
[0082] 2. Aromatization reaction
[0083] Using cat4 as a catalyst, an aromatization coupling reaction of methanol and raffinate oil (mass ratio 5:5) was carried out according to the reaction conditions of Example 1, and samples were taken for analysis after 48 hours of reaction.
[0084] The analysis results show that the methanol conversion rate is basically 100%, the liquid yield is 88.35%, and the aromatics selectivity is 46.47%.
[0085] Example 5
[0086] 1. Preparation of aromatic catalyst (cat5)
[0087] Add 100 g of silica sol and 12 ml of 4 mol / L sodium hydroxide solution into 200 g of deionized water, and stir at 25° C. for 2.5 h to obtain a mixed solution A5;
[0088] Add 5 ml of 1.2 mol / L aluminum sulfate solution, 2.54 g of tetrabutylammonium hydroxide and 2.75 g of zinc nitrate to the mixed solution A5, stir at 25°C for 3 h, and then reflux at 90°C for 3 h to obtain a mixed solution B5 (the molar ratio of SiO2:Na2O:Al2O3:template:Zn:H2O is about 83.3:4.0:1.0:1.63:1.54:1851);
[0089] The mixed solution B5 was transferred to a crystallization reactor with a polytetrafluoroethylene liner and hydrothermally crystallized at 140°C for 72 hours to obtain a mixed solution C5;
[0090] The mixed solution C5 was cooled to room temperature, filtered, washed to pH=8-9, and dried at 100°C for 6h. The obtained solid product was placed in a muffle furnace and calcined at 550°C from room temperature at a heating rate of 2-3°C / min for 4h to obtain Zn-NaZSM-5 / ZSM-11 molecular sieve;
[0091] After ammonium exchange and molding treatment, a Zn-ZSM-5 / ZSM-11 catalyst was obtained, which was denoted as cat5.
[0092] 2. Aromatization reaction
[0093] Using cat5 as the catalyst, an aromatization coupling reaction of methanol and raffinate oil (mass ratio 5:5) was carried out according to the reaction conditions of Example 1, and samples were taken for analysis after 48 hours of reaction.
[0094] The analysis results show that the methanol conversion rate is basically 100%, the liquid yield is 89.62%, and the aromatics selectivity is 47.83%.
[0095] Example 6
[0096] 1. Preparation of Zn-ZSM-5 / ZSM-11 catalyst (cat6)
[0097] Add 100 g of silica sol and 12 ml of 4 mol / L sodium hydroxide solution into 200 g of deionized water, and stir at 25°C for 4 h to obtain a mixed solution A6;
[0098] Add 5 ml of 1.2 mol / L aluminum sulfate solution, 3.54 g of tetrabutylammonium hydroxide and 4.15 g of zinc nitrate to the mixed solution A6, stir at 25°C for 3 h, and then reflux at 90°C for 3 h to obtain a mixed solution B6 (the molar ratio of SiO2:Na2O:Al2O3:template:Zn:H2O is about 83.3:4.0:1.0:2.27:2.3:1851);
[0099] The mixed solution B6 was transferred to a crystallization reactor with a polytetrafluoroethylene liner and hydrothermally crystallized at 150°C for 36 hours to obtain a mixed solution C6;
[0100] The mixed solution C6 was cooled to room temperature, filtered, washed to pH=8-9, and dried at 100°C for 6h. The obtained solid product was placed in a muffle furnace and calcined at 550°C from room temperature at a heating rate of 2-3°C / min for 4h to obtain Zn-NaZSM-5 / ZSM-11 molecular sieve;
[0101] After ammonium exchange and molding treatment, a Zn-ZSM-5 / ZSM-11 catalyst was obtained, which was denoted as cat6.
[0102] 2. Aromatization reaction
[0103] Using cat6 as a catalyst, an aromatization coupling reaction of methanol and raffinate oil (mass ratio 5:5) was carried out according to the reaction conditions of Example 1, and samples were taken for analysis after 48 hours of reaction.
[0104] The analysis results show that the methanol conversion rate is basically 100%, the liquid yield is 86.23%, and the aromatics selectivity is 51.16%.
[0105] Example 7
[0106] 1. Preparation of Zn-ZSM-5 / ZSM-11 catalyst (cat7)
[0107] Add 80 g of ethyl orthosilicate and 12 ml of 4 mol / L sodium hydroxide solution to 200 g of deionized water, and stir at 25°C for 4.5 h to obtain a mixed solution A7;
[0108] Add 5 ml of 1.2 mol / L aluminum sulfate solution, 1.89 g of tetrabutylammonium bromide and 2.75 g of zinc nitrate to the mixed solution A7, stir at 25°C for 3 h, and then reflux at 90°C for 3 h to obtain a mixed solution B7 (the amount of each raw material added satisfies the molar ratio of SiO2:Na2O:Al2O3:template:Zn:H2O of approximately 64:4.0:1.0:0.98:1.54:1851);
[0109] The mixed solution B7 was transferred to a crystallization reactor with a polytetrafluoroethylene liner and hydrothermally crystallized at 150°C for 36 hours to obtain a mixed solution C7;
[0110] The mixed solution C7 was cooled to room temperature, filtered, washed to pH=8-9, and dried at 100°C for 6h. The obtained solid product was placed in a muffle furnace and calcined at 550°C from room temperature at a heating rate of 2-3°C / min for 4h to obtain Zn-NaZSM-5 / ZSM-11 molecular sieve;
[0111] After ammonium exchange and molding treatment, a Zn-ZSM-5 / ZSM-11 catalyst was obtained, which was denoted as cat7.
[0112] 2. Aromatization reaction
[0113] Using cat7 as a catalyst, an aromatization coupling reaction of methanol and raffinate oil (mass ratio 5:5) was carried out according to the reaction conditions of Example 1, and samples were taken for analysis after 48 hours of reaction.
[0114] The analysis results show that the methanol conversion rate is basically 100%, the liquid yield is 88.12%, and the aromatics selectivity is 54.56%.
[0115] Example 8
[0116] 1. Preparation of Zn-ZSM-5 / ZSM-11 catalyst (cat8)
[0117] Add 100 g of ethyl orthosilicate and 12 ml of 4 mol / L sodium hydroxide solution into 200 g of deionized water, and stir at 25° C. for 5 h to obtain a mixed solution A8;
[0118] Add 5 ml of 1.2 mol / L aluminum sulfate solution, 0.98 g of tetrabutylammonium bromide, 0.98 g of tetrabutylammonium hydroxide and 2.75 g of zinc nitrate to the above mixed solution A8, stir at 25°C for 3 h, and then reflux at 90°C for 3 h to obtain a mixed solution B8 (the amount of each raw material added satisfies the molar ratio of SiO2:Na2O:Al2O3:template:Zn:H2O of approximately 80:4.0:1.0:1.35:1.54:1851);
[0119] The mixed solution B8 was transferred to a crystallization reactor with a polytetrafluoroethylene liner and hydrothermally crystallized at 150°C for 36 hours to obtain a mixed solution C8;
[0120] The mixed solution C8 was cooled to room temperature, filtered, washed to pH=8-9, and dried at 100°C for 6h. The obtained solid product was placed in a muffle furnace and calcined at 550°C from room temperature at a heating rate of 2-3°C / min for 4h to obtain Zn-NaZSM-5 / ZSM-11 molecular sieve;
[0121] After ammonium exchange and molding treatment, a Zn-ZSM-5 / ZSM-11 catalyst was obtained, which was denoted as cat8.
[0122] 2. Aromatization reaction
[0123] Using cat8 as a catalyst, an aromatization coupling reaction of methanol and raffinate oil (mass ratio 5:5) was carried out according to the reaction conditions of Example 1, and samples were taken for analysis after 48 hours of reaction.
[0124] The analysis results show that the methanol conversion rate is basically 100%, the liquid yield is 88.97%, and the aromatics selectivity is 50.52%.
[0125] Example 9
[0126] 1. Preparation of Zn-ZSM-5 / ZSM-11 catalyst (cat2)
[0127] Add 60 g of ethyl orthosilicate and 12 ml of 4 mol / L sodium hydroxide solution into 160 g of deionized water, and stir at 25°C for 3.5 h to obtain a mixed solution A9;
[0128] Add 5 ml of 1.0 mol / L aluminum hydroxide solution, 1.98 g of tetrabutylammonium bromide and 2.75 g of zinc nitrate to the mixed solution A9, stir at 25°C for 3 h, and then reflux at 90°C for 3 h to obtain a mixed solution B9 (the amount of each raw material added satisfies the molar ratio of SiO2:Na2O:Al2O3:template:Zn:H2O of approximately 115:9.6:1.0:2.46:3.70:3556);
[0129] The mixed solution B9 was transferred to a crystallization reactor with a polytetrafluoroethylene liner and hydrothermally crystallized at 160°C for 36 hours to obtain a mixed solution C9;
[0130] The mixed solution C9 was cooled to room temperature, filtered, washed to pH=8-9, and dried at 100°C for 6h. The obtained solid product was placed in a muffle furnace and calcined at 550°C from room temperature at a heating rate of 2-3°C / min for 4h to obtain Zn-NaZSM-5 / ZSM-11 molecular sieve;
[0131] After ammonium exchange and molding treatment, a Zn-ZSM-5 / ZSM-11 catalyst was obtained, which was denoted as cat9.
[0132] 2. Aromatization reaction
[0133] Using cat9 as a catalyst, an aromatization coupling reaction of methanol and raffinate oil (mass ratio 5:5) was carried out according to the reaction conditions of Example 1, and samples were taken for analysis after 48 hours of reaction.
[0134] The analysis results show that the methanol conversion rate is basically 100%, the liquid yield is 85.26%, and the aromatics selectivity is 40.38%.
[0135] Example 10
[0136] 1. Preparation of Zn-ZSM-5 / ZSM-11 catalyst (cat2)
[0137] Add 100 g of silica sol and 12 ml of 4 mol / L sodium hydroxide solution to 220 g of deionized water, and stir at 25° C. for 4 h to obtain a mixed solution A10;
[0138] Add 5 ml of 1.2 mol / L aluminum sulfate solution, 1.86 g of tetrabutylammonium hydroxide and 3.75 g of zinc nitrate to the mixed solution A10, stir at 25°C for 3 h, and then reflux at 90°C for 4 h to obtain a mixed solution B10 (the amount of each raw material added satisfies the molar ratio of SiO2:Na2O:Al2O3:template:Zn:H2O of approximately 83.3:4.0:1.0:1.2:2.1:2037);
[0139] The mixed solution B10 was transferred to a crystallization reactor with a polytetrafluoroethylene liner and hydrothermally crystallized at 160°C for 36 hours to obtain a mixed solution C10;
[0140] The mixed solution C10 was cooled to room temperature, filtered, washed to pH=8-9, and dried at 100°C for 6h. The obtained solid product was placed in a muffle furnace and calcined at 550°C from room temperature at a heating rate of 2-3°C / min for 4h to obtain Zn-NaZSM-5 / ZSM-11 molecular sieve;
[0141] After ammonium exchange and molding treatment, a Zn-ZSM-5 / ZSM-11 catalyst was obtained, which was denoted as cat10.
[0142] 2. Aromatization reaction
[0143] Using cat10 as a catalyst, an aromatization coupling reaction of methanol and raffinate oil (mass ratio 5:5) was carried out according to the reaction conditions of Example 1, and samples were taken for analysis after 48 hours of reaction.
[0144] The analysis results show that the methanol conversion rate is basically 100%, the liquid yield is 86.58%, and the aromatics selectivity is 52.08%.
[0145] The XRD patterns and N2 adsorption curves of the Zn-HZSM-5 / ZSM-11 molecular sieves of Example 1 and Example 2 are respectively as follows: Figure 1 and Figure 2 As shown (the detection results of other embodiments are similar).
[0146] Depend on Figure 1 It can be found that there are three diffraction peaks at 2θ=23-25° and the rightmost peak is weak, and a diffraction peak appears at about 2θ=45° and the diffraction single and double peaks are not obvious (that is, it is not obvious to belong to a single shoulder peak or a double shoulder peak), indicating that Example 1 prepared ZSM-5 and ZSM-11 cocrystal molecular sieves (usually, ZSM-5 has 3 obvious diffraction peaks near 2θ of about 23-25°, and ZSM-11 has only two diffraction peaks near 2θ of about 23-25°; ZSM-5 has obvious double shoulder peaks near 2θ of about 45°, and ZSM-11 has a single shoulder peak near 2θ of about 45°, and the appearance of Figure 1 The characteristic peaks shown are diffraction peaks of ZSM-5 / ZSM-11 eutectic molecular sieve).
[0147] like Figure 2 As shown in the figure, the N2 adsorption-desorption curve of Zn-HZSM-5 / ZSM-11 shows separation (i.e., hysteresis loop or hysteresis loop) at a relative pressure (P / P0) of about 0.6-0.9, and then closes without an obvious saturated adsorption platform, which is similar to the H3 type hysteresis loop adsorption curve in the International Union of Pure and Cited Chemistry (IUPAC) classification, indicating that the molecular sieve contains micropores, mesopores, and macropores, that is, a multi-level pore structure.
[0148] ICP-OES was also used to detect the Zn-HZSM-5 / ZSM-11 of Examples 1-10. The results showed that the catalysts prepared in Examples 1-10 all contained Zn, that is, they were Zn-loaded Zn-5 / ZSM-11 eutectic molecular sieve catalysts (the ICP-OES test results of Examples 1 and 2 are shown in Table 1).
[0149] Table 1 ICP-OES test results of Zn-HZSM-5 / ZSM-11
[0150] sample Si / Al Si(mg / g) Al(mg / g) Zn(mg / g) Example 1 40.3 652.9 16.2 16.8 Example 2 85.6 1275.4 14.9 9.8
[0151] The above test results show that Example 1-10 adopts a one-step method to in situ synthesize a Zn-loaded ZSM-5 / ZSM-11 eutectic molecular sieve catalyst, and the above aromatization test shows that the catalyst has good catalytic activity and other properties, can catalyze the aromatization coupling reaction of light hydrocarbon feedstocks such as methanol and raffinate oil, is not prone to carbon deposition and deactivation during the reaction, has a long service life, and can achieve a high liquid yield and aromatics selectivity.
Claims
1. A method for preparing a Zn-ZSM-5 / ZSM-11 catalyst, It is characterized in that include: (1) Adding a silicon source and an alkali raw material into water to obtain a mixed solution A; (2) adding an aluminum source, a template agent and a zinc source to the mixed solution A, and refluxing the reaction system at 80-150° C. for 2-8 hours to obtain a mixed solution B; wherein the zinc source is selected from at least one of zinc nitrate, zinc chloride and zinc sulfate, and the template agent is selected from at least one of tetrabutylammonium hydroxide, tetrabutylammonium bromide and n-hexylamine; (3) allowing the mixed solution B to crystallize at 130-170° C. for 18-96 hours to obtain a mixed solution C; (4) Cooling the mixed solution C to room temperature, filtering, washing, and drying, and then subjecting the obtained solid product to a first calcination treatment to obtain a catalyst precursor; (5) exchanging the catalyst precursor with ammonium, and subjecting the exchange product to a second calcination treatment to obtain a Zn-ZSM-5 / ZSM-11 catalyst; Wherein, the alkali raw material is sodium hydroxide; the addition amounts of the silicon source, alkali raw material, aluminum source, template agent, zinc source, and water are controlled to satisfy the following molar ratio: SiO 2 :Na 2 O:Al 2 O 3 :Template agent:Zn :H 2 O=(30-190):(2.0-15.0):1.0:(0.30-5.00):(0.5-8.0):(1200-4000).
2. The preparation method according to claim 1, It is characterized in that In step (2), the reaction system is refluxed at 90-120° C. for 2-5 hours to obtain a mixed solution B; and / or, in step (3), the mixed solution B is crystallized at 140-170° C. for 18-72 hours to obtain a mixed solution C.
3. The preparation method according to claim 1, It is characterized in that The silicon source is selected from at least one of silica sol, silica gel and tetraethyl orthosilicate.
4. The preparation method according to claim 2, It is characterized in that The silicon source is selected from at least one of silica sol, silica gel and tetraethyl orthosilicate.
5. The preparation method according to claim 1, It is characterized in that The aluminum source is selected from at least one of aluminum sulfate, sodium aluminate, aluminum chloride, aluminum nitrate, aluminum isopropoxide, and aluminum hydroxide.
6. The preparation method according to claim 2, It is characterized in that The aluminum source is selected from at least one of aluminum sulfate, sodium aluminate, aluminum chloride, aluminum nitrate, aluminum isopropoxide, and aluminum hydroxide.
7. The preparation method according to any one of claims 1 to 6, It is characterized in that The first calcination treatment comprises: heating the solid product to 500-550° C. and calcining for 4-6 hours to obtain a catalyst precursor; wherein the heating rate is controlled to be 1-5° C. / min.
8. The preparation method according to any one of claims 1 to 6, It is characterized in that The ammonium exchange is carried out using an ammonium salt solution, wherein the concentration of the ammonium salt solution is 0.5-1 mol / L, the ammonium exchange temperature is 70-90° C., and the ammonium exchange time is 2-6 hours.
9. The preparation method according to claim 8, It is characterized in that The ammonium salts include ammonium nitrate and ammonium chloride.
10. The preparation method according to any one of claims 1 to 6, It is characterized in that The second calcination treatment includes: heating the exchange product to 500-550° C. and calcining for 4-6 hours to obtain a Zn-ZSM-5 / ZSM-11 catalyst; wherein the heating rate is controlled to be 1-5° C. / min.
11. A Zn-ZSM-5 / ZSM-11 catalyst, It is characterized in that Prepared according to the preparation method according to any one of claims 1 to 10.
12. A method for producing aromatic hydrocarbons, It is characterized in that include: The Zn-ZSM-5 / ZSM-11 catalyst according to claim 11 is used to catalyze the aromatization reaction of methanol and light hydrocarbon raw materials to obtain aromatic hydrocarbon products.
Citation Information
Patent Citations
A ZSM-5 and ZSM-11 eutectic zeolite molecular sieve, their preparation and application
CN104624226B
Crystalline zeolite product constituting ZSM-5 / ZSM-11 intermediates
US4229424A
Preparation method of small crystal grain ZSM-5 / ZSM-11 composite zeolite
CN102745715A
Preparation method of nano hierarchical-pore ZSM-11 / ZSM-5 eutectic zeolite
CN103539153A
ZSM-5 and ZSM-11 eutectic zeolite molecular sieve and preparation method and application thereof