A radar stealth plate surface damage repair material and repair method

Through the specific proportion of structural glue and wave absorbing putty, the technical difficulties of large-area and penetrating damage repair of radar stealth plates are solved, and rapid repair and efficient stealth performance are achieved, which significantly improves the repair efficiency and stealth performance.

CN113754346BActive Publication Date: 2024-12-06TIANNUO PHOTOELECTRIC MATERIAL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110991525.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-08-26
Publication Date
2024-12-06
Estimated Expiration
2041-08-26

AI Technical Summary

Technical Problem

The existing radar stealth plate repair technology cannot effectively repair large-area or penetrating damage, and the curing time is long and the adhesion is poor, making it difficult to maintain stealth performance.

Method used

Structural glue and absorbent putty are mixed in a specific proportion, including ferrite, unsaturated polyester resin and vinyl triamine. It is quickly repaired through simple application and grinding steps, shortening the curing time and enhancing adhesion.

Benefits of technology

It realizes rapid repair of large-area and penetrating damage on the surface of the radar stealth plate. After repair, the stealth performance can reach 85% to 90%, and reduces the repair time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113754346B_ABST
    Figure CN113754346B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of electromagnetic wave absorbing materials, and specifically to a radar stealth plate surface damage repair material and a repair method. The damage repair material comprises a structural adhesive and an absorbing putty; the structural adhesive is composed of a curing agent and a resin in a mass ratio of 1:4-7; the absorbing putty is composed of an absorbent, a resin, and a curing agent in a mass ratio of 75-85:15-20:2-10. The structural adhesive and the absorbing putty of the radar stealth plate surface damage repair material of the present invention are mixed in a specific ratio, which shortens the curing time of the absorbing putty, thereby reducing the repair time of the radar absorbing plate surface damage; the repair material of the present invention has a strong bonding force with the radar stealth plate, and the repair material of the present invention has good absorbing performance, which can be used for the rapid repair of large-area, penetrating and other damages on the surface of the radar stealth plate; after repair, the radar stealth performance can reach 85% to 90% of the state without surface damage.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of electromagnetic wave absorbing materials, and in particular to a material and a method for repairing surface damage of a radar stealth plate. Background Art

[0002] During use, the radar stealth panel will be damaged due to external factors such as bumps and collisions, and needs to be repaired in time. The current common method is to use absorbing putty to repair the damaged part. Although it can ensure the radar stealth performance of the damaged part, it cannot be effectively bonded to the underlying structure, has poor bonding strength, and takes a long time to cure. It can only be used to repair small areas of damaged surfaces.

[0003] Chinese patent application CN110721881A discloses a method for on-site repair of high-temperature radar and infrared compatible stealth coatings, including a patch conductor type high-temperature periodic structural layer repair method, and the specific steps include preparing a conductor coating, the conductor coating is composed of silver powder, glass powder and an organic carrier, and the glass powder is composed of Bi2O3, B2O3, Sb2O3 and SiO2; the conductor coating is applied to the repair area by screen printing, and the repair is completed by drying and sintering with a portable heating device. This method requires additional heating equipment, the operation is relatively complicated, and the method is not suitable for penetrating damage repair. Summary of the invention

[0004] The main purpose of the present invention is to provide a radar stealth panel surface damage repair material and repair method. The repair material can be used to quickly repair large-area, penetrating damage on the surface of the radar stealth panel, the steps are simple, and the radar stealth panel can maintain good stealth performance after repair.

[0005] To achieve the above object, the present invention adopts the following technical solutions:

[0006] The invention provides a radar stealth plate surface damage repair material, which comprises a structural adhesive and a radar absorbing putty; the structural adhesive is composed of a curing agent and a resin in a mass ratio of 1:4-7; the radar absorbing putty is composed of an absorbent, a resin and a curing agent in a mass ratio of 75-85:15-20:2-10.

[0007] Furthermore, the mass ratio of the structural adhesive to the microwave-absorbing putty is 1:3-8.

[0008] Furthermore, the absorber includes one or more of ferrite, polycrystalline iron, metal powder, alloy powder, iron nitride, carbon fiber, carbon black, carbonyl iron powder, acetylene black, carbon nanotubes, barium titanate, zirconium oxide, and zinc oxide; the resin in the absorbing putty includes one or more of unsaturated polyester resin, epoxy resin, and phenolic resin; the curing agent in the absorbing putty includes one or more of vinyltriamine, aminoethylpiperazine, m-phenylenediamine, and diaminodiphenylmethane.

[0009] Furthermore, the curing agent in the structural adhesive is an amine curing agent, including one or more of fatty amines, polyamides, aromatic amines, and alicyclic amines; the resin in the structural adhesive is one or more of glycerol-modified epoxy resins, phenolic-modified epoxy resins, and brominated-modified epoxy resins.

[0010] The present invention also provides a method for quickly repairing surface damage of a radar stealth plate, which comprises the following steps: cleaning the damaged area, evenly applying any of the above-mentioned repair materials to the damaged area, compacting and flattening it; after the repair material is solidified, grinding it flat, and spraying absorbing paint to obtain the product.

[0011] Furthermore, the curing time of the repair material is 10-15 minutes.

[0012] Compared with the prior art, the present invention has the following advantages:

[0013] The structural adhesive of the radar stealth plate surface damage repair material of the present invention is mixed with the absorbing putty in a specific ratio, which shortens the curing time of the absorbing putty, thereby reducing the repair time of the radar absorbing plate surface damage; the repair material of the present invention has a strong bonding force with the radar stealth plate, and the repair material of the present invention has good absorbing performance, and can be used for the rapid repair of large-area, penetrating and other damages on the surface of the radar stealth plate; after repair, the radar stealth performance can reach 85% to 90% of the state without surface damage. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.

[0015] Figure 1 This is a flow chart of the method for quickly repairing the damaged surface of the radar stealth plate described in Example 1 of the present invention;

[0016] Figure 2 This is a physical picture of the radar stealth plate after the surface damage is repaired according to Example 1 of the present invention;

[0017] Figure 3 for Figure 2 Actual picture of the radar stealth panel before its surface is damaged. DETAILED DESCRIPTION

[0018] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.

[0019] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations and / or combinations thereof.

[0020] In order to enable those skilled in the art to more clearly understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below in conjunction with specific embodiments.

[0021] Example 1

[0022] A radar stealth plate surface damage repair material, the material is obtained by mixing structural adhesive and radar absorbing putty in a mass ratio of 1:3 and is in a paste state.

[0023] The surface absorbing putty is obtained by mixing ferrite, unsaturated polyester resin and ethylene triamine in a mass ratio of 76:15:9.

[0024] The structural adhesive is composed of aliphatic amine and glycerin-modified epoxy resin in a mass ratio of 1:4.

[0025] A structural plate with a specification of 300mm*300mm*6mm is selected, and a damage with a size of 100mm*100mm*3mm is set on the surface. This is used as an example to illustrate the method for quickly repairing the damage on the surface of the radar stealth plate.

[0026] like Figure 1 As shown, the rapid repair method for the damaged surface of the radar stealth plate comprises the following steps:

[0027] Step 1. Prepare the above-mentioned repair material into a paste;

[0028] Step 2. Clean the damaged area until there is no dust or oil stain;

[0029] Step 3. Apply the paste obtained in step 1 evenly to the damaged part of the radar stealth plate, compact and flatten it with tools;

[0030] Step 4: Allow the paste to solidify for 10 minutes after application.

[0031] Step 5. After the paste solidifies, use sandpaper to smooth it;

[0032] Step 6. Spray the absorbing material, such as Figure 2 shown.

[0033] After repair, its radar reflectivity (12~18GHz) was tested to be -3.9dB, and before damage (12~18GHz) was -4.4dB. The radar wave reflectivity was 88.6% of the original radar stealth panel.

[0034] Example 2

[0035] A radar stealth plate surface damage repair material, the material is obtained by mixing structural adhesive and radar absorbing putty in a mass ratio of 1:8 and is in a paste state.

[0036] The surface absorbing putty is obtained by mixing alloy powder, epoxy resin and aminoethyl piperazine in a mass ratio of 83:15:2.

[0037] The structural adhesive is composed of polyamide and phenolic modified epoxy resin in a mass ratio of 1:7.

[0038] A structural plate with a specification of 300mm*300mm*6mm is selected, and a damage with a size of 100mm*100mm*3mm is set on the surface. This is used as an example to illustrate the method for quickly repairing the damage on the surface of the radar stealth plate.

[0039] The rapid repair method for the damaged surface of the radar stealth plate comprises the following steps:

[0040] Step 1. Prepare the above-mentioned repair material into a paste;

[0041] Step 2. Clean the damaged area until there is no dust or oil stain;

[0042] Step 3. Apply the paste obtained in step 1 evenly to the damaged part of the radar stealth plate, compact and flatten it with tools;

[0043] Step 4: Allow the paste to solidify for 15 minutes after application.

[0044] Step 5. After the paste solidifies, use sandpaper to smooth it;

[0045] Step 6. Spray the absorbing material.

[0046] After repair, its radar reflectivity (12~18GHz) was tested to be -3.7dB, and before damage (12~18GHz) was -4.4dB. The radar wave reflectivity was 84.1% of the original radar stealth panel.

[0047] Example 3

[0048] A radar stealth plate surface damage repair material, the material is obtained by mixing structural adhesive and radar absorbing putty in a mass ratio of 1:5 and is in a paste state.

[0049] The surface absorbing putty is obtained by mixing carbonyl iron powder, phenolic resin and m-phenylenediamine in a mass ratio of 78:17:5.

[0050] The structural adhesive is composed of aromatic amine and brominated modified epoxy resin in a mass ratio of 1:5.

[0051] A structural plate with a specification of 300mm*300mm*6mm is selected, and a damage with a size of 100mm*100mm*3mm is set on the surface. This is used as an example to illustrate the method for quickly repairing the damage on the surface of the radar stealth plate.

[0052] The rapid repair method for the damaged surface of the radar stealth plate comprises the following steps:

[0053] Step 1. Prepare the above-mentioned repair material into a paste;

[0054] Step 2. Clean the damaged area until there is no dust or oil stain;

[0055] Step 3. Apply the paste obtained in step 1 evenly to the damaged part of the radar stealth plate, compact and flatten it with tools;

[0056] Step 4: Allow the paste to solidify for 10 minutes after application.

[0057] Step 5. After the paste solidifies, use sandpaper to smooth it;

[0058] Step 6. Spray the absorbing material.

[0059] After repair, its radar reflectivity (12~18GHz) was tested to be -4.1dB, and before damage (12~18GHz) was -4.6dB. The radar wave reflectivity was 89.1% of the original radar stealth panel.

[0060] Example 4

[0061] A radar stealth plate surface damage repair material, the material is obtained by mixing structural adhesive and radar absorbing putty in a mass ratio of 1:5 and is in a paste state.

[0062] The surface absorbing putty is obtained by mixing acetylene carbon black, epoxy resin and triaminodiphenylmethane in a mass ratio of 80:18:2.

[0063] The structural adhesive is composed of alicyclic amine and glycerol-modified epoxy resin in a mass ratio of 1:5.

[0064] A structural plate with a specification of 300mm*300mm*20mm is selected, and a damage with a size of 100mm*100mm*3mm is set on the surface. This is used as an example to illustrate the method for quickly repairing the damage on the surface of the radar stealth plate.

[0065] The rapid repair method for the damaged surface of the radar stealth plate comprises the following steps:

[0066] Step 1. Prepare the above-mentioned repair material into a paste;

[0067] Step 2. Clean the damaged area until there is no dust or oil stain;

[0068] Step 3. Apply the paste obtained in step 1 evenly to the damaged part of the radar stealth plate, compact and flatten it with tools;

[0069] Step 4: Allow the paste to solidify for 15 minutes after application.

[0070] Step 5. After the paste solidifies, use sandpaper to smooth it;

[0071] Step 6. Spray the absorbing material.

[0072] After repair, its radar reflectivity (12~18GHz) was tested to be -15.8dB, and before damage (12~18GHz) was -17.6dB. The radar wave reflectivity was 89.8% of the original radar stealth panel.

[0073] Comparative Example 1

[0074] A structural plate with a specification of 300mm*300mm*6mm was selected, and a damage with a size of 100mm*100mm*3mm was set on the surface. Only radar-absorbing paint was sprayed on it. The radar reflectivity (12~18GHz) of the radar stealth plate obtained after spraying was -0.9dB, and the radar reflectivity (12~18GHz) before damage was -4.1dB. The radar wave reflectivity was 22.0% of the original radar stealth plate.

[0075] Comparative Example 2

[0076] The difference between the radar stealth plate surface damage repair material and the radar stealth plate surface damage repair material described in Example 1 is that the repair material is obtained by mixing structural adhesive and absorbing putty in a mass ratio of 1:10.

[0077] A structural plate with a specification of 300mm*300mm*6mm was selected, and a damage with a size of 100mm*100mm*3mm was set on the surface. The repair material was used to repair the surface damage of the radar stealth plate. The curing time of the repair material was 65min. After the repair, the radar reflectivity (12~18GHz) was tested to be -4.2dB, and the radar reflectivity (12~18GHz) before the damage was -4.6dB, and the radar wave reflectivity was 91.3% of the original radar stealth plate.

[0078] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A radar stealth plate surface damage repair material, characterized in that: It includes structural adhesive and microwave absorbing putty; The structural adhesive is composed of a curing agent and a resin in a mass ratio of 1:4 to 7; The microwave absorbing putty is composed of absorbent, resin and curing agent in a mass ratio of 75-85:15-20:2-10; The mass ratio of structural adhesive to microwave absorbing putty is 1:3-8; The absorbent includes one or more of ferrite, polycrystalline iron, iron nitride, carbon fiber, carbon black, carbonyl iron powder, acetylene black, carbon nanotubes, barium titanate, zirconium oxide, and zinc oxide; the resin in the absorbing putty includes one or more of unsaturated polyester resin, epoxy resin, and phenolic resin; the curing agent in the absorbing putty includes one or more of vinyltriamine, aminoethylpiperazine, m-phenylenediamine, and diaminodiphenylmethane; The curing agent in the structural adhesive is an amine curing agent, including one or more of fatty amines, polyamides, aromatic amines, and alicyclic amines; the resin in the structural adhesive is one or more of glycerol-modified epoxy resins, phenolic-modified epoxy resins, and brominated-modified epoxy resins; the curing time of the repair material is 10-15 minutes.

2. A rapid repair method using the radar stealth plate surface damage repair material as claimed in claim 1, characterized in that: The following steps are involved: Clean the damaged area, apply the radar stealth plate surface damage repair material evenly on the damaged area, compact and scrape it flat; after the repair material is cured for 10-15 minutes, grind it flat and spray the absorbing material to obtain the product.