Preparation method of highly stable, compatible and fast-curing potassium silicate inorganic nanomaterial
By adding potassium silicate aqueous solution, water, silica sol, polyether, nano-titanium dioxide, quaternary ammonium salt and caustic soda in an emulsification tank for high-speed dispersion and homogenization, high-stability and fast-curing potassium silicate inorganic nanomaterials are prepared , solves the problems of slow curing speed and poor compatibility of ordinary silicate resin coatings, and achieves efficient and stable coating performance.
Patent Information
- Application Number
- CN202110981288.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-08-25
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-08-25
AI Technical Summary
The inorganic coatings made of ordinary silicate resins currently used in the market cannot be industrialized due to their slow curing speed, poor water washing resistance, and poor compatibility with water-based organic resins.
Using a preparation method of highly stable, compatible and fast-curing potassium silicate inorganic nanomaterials, ordinary potassium silicate aqueous solution, water, silica sol, polyether, nanometer titanium dioxide, quaternary ammonium salt and tablets are added to the emulsification tank at room temperature. Alkali is used for high-speed dispersion and homogenization to form high-stability and fast-curing nano-modified silicate resin.
It achieves the preparation of high stability and fast curing nano-modified silicate resin, improves the compatibility and curing strength with water-based organic resins, extends the storage stability, and can reach 30% in construction and industrial water-based coatings. The added amount has the characteristics of super weather resistance, antibacterial, excellent adhesion, fast curing, acid resistance, chemical solvent resistance, and fire protection.
Smart Images

Figure CN113773678B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of inorganic nano material production, in particular to a method for preparing a highly stable, compatible and fast-curing potassium silicate inorganic nano material. Background Art
[0002] Building wall decoration paints, wood paints, and industrial paints use acrylic resins as the main film-forming substance. However, organic acrylic resins not only consume a large amount of petrochemical resources and produce a large amount of VOC COD emissions, but the paints made from them are of poor quality and are prone to peeling, discoloration, powdering, dirtiness, and poor durability.
[0003] The coatings prepared with highly compatible and fast-curing nano-modified silicate resin as the main film-forming material have the characteristics of super weather resistance, excellent antibacterial adhesion, fast curing, acid resistance, chemical solvent resistance, fire resistance, etc. However, the inorganic coatings made of ordinary silicate resins in the market are currently unable to be industrialized due to problems such as slow curing speed, poor water washing resistance, incompatibility with other resins, and unstable storage.
[0004] To this end, the present invention provides a preparation method of a highly compatible and fast-curing potassium silicate inorganic nanomaterial. Summary of the invention
[0005] The preparation method of the highly stable and compatible and fast-curing potassium silicate inorganic nanomaterial proposed by the invention solves the problems of slow curing, poor water washing resistance and poor compatibility with water-based organic resin in the prior art.
[0006] To achieve the above object, the present invention provides the following technical solution: a method for preparing a highly stable, compatible and fast-curing potassium silicate inorganic nanomaterial, comprising the following steps:
[0007] S1. At room temperature, first add a common potassium silicate aqueous solution into a high-speed homogenization emulsification tank, stir to form a vortex, then add water, silica sol, polyether, nano titanium dioxide, flake caustic soda, quaternary ammonium salt in sequence, and then mix evenly at a certain temperature to obtain a mixture;
[0008] S2. The prefabricated mixture is then heated to 40-80°C in an emulsifying tank, and then at this temperature, a high-speed dispersion homogenization speed of 1500-3000rpm is performed for a homogenization time of 50-100min.
[0009] Preferably, according to S1, the mass ratio of the ordinary potassium silicate aqueous solution, water, silica sol, polyether, nano titanium dioxide, quaternary ammonium salt and flake caustic soda is 100: 5-15: 35-55: 1-5: 0.5-5: 0.1-0.3: 0.5-5, the stirring speed is 1500-3000rmp homogenization, the homogenization temperature is 40-80°C, and the homogenization time is 50-100min.
[0010] Preferably, the modulus of the ordinary potassium silicate aqueous solution is 3.3 to 3.5, the solid content is 38% to 42%, the water is one of deionized water and industrial tap water, the solid content of the silica sol is 26% to 32%, the polyether is the French Sipson Chemical hyperbranched polyether SE10, the nano titanium dioxide has an average particle size of 5nm, and the solid content is 5%, the quaternary ammonium salt is one or more quaternary ammonium salts containing decanyl and dodecyl groups, and the flake caustic soda is industrial grade sodium hydroxide.
[0011] A production device for highly stable, compatible and fast-curing potassium silicate inorganic nanomaterials comprises a working box, an emulsifying tank is installed inside the working box through a supporting mechanism, a rotating box is installed inside the emulsifying tank, a stirring mechanism is installed inside the rotating box, a rotating rod is fixedly connected to the top of the rotating box, one end of the rotating rod passes through the working box and extends to the outside of the working box, a first rotating mechanism for driving the rotating rod to rotate is installed outside the working box, a second rotating mechanism for driving the emulsifying tank to rotate is installed on one side of the working box, a spiral heating tube and a heating box are installed outside the emulsifying tank, and the spiral heating tube is located outside the heating box.
[0012] Preferably, the support mechanism includes a plurality of support rods installed at the bottom of the emulsification tank and a plurality of balls installed at the bottom of the plurality of support rods, an annular groove is provided on the bottom inner wall of the working box, and the plurality of balls are slidably connected inside the annular groove.
[0013] Preferably, the stirring mechanism includes a plurality of movable rods installed inside the emulsification tank and a plurality of stirring rods installed outside the plurality of movable rods, a support plate is installed inside the working box, a threaded rod is fixedly connected to the top of the support plate, the top of the threaded rod passes through the emulsification tank and extends to the inside of the rotating box, and one end of the threaded rod located inside the emulsification tank is fixedly connected to the top inner wall of the rotating box, the external thread of the threaded rod is connected to a threaded sleeve, a plurality of strip openings are opened on the outside of the rotating box, the plurality of movable rods respectively pass through the plurality of strip openings and extend to the inside of the rotating box, and one end of the plurality of movable rods located inside the rotating box is fixedly connected to the outside of the threaded sleeve.
[0014] Preferably, the first rotating mechanism includes a rotating motor installed outside the working box and a rotating disk installed at the output end of the rotating motor, one side of the rotating disk is rotatably connected to a push rod, one end of the push rod is hinged with a rack, a first gear meshing with the rack is installed on the outside of the rotating rod, and a limiting sleeve for limiting the rack is installed on the top of the working box.
[0015] Preferably, the second rotating mechanism includes a connecting rod installed on one side of the working box and a second gear installed at the bottom of the connecting rod, a third gear meshing with the second gear is installed on the outside of the emulsification tank, and the connecting rod and the rotating rod are connected by a transmission mechanism, wherein the transmission mechanism includes two pulleys installed on the outside of the connecting rod and the rotating rod, and the two pulleys are connected by belt rotation.
[0016] Preferably, a feed hopper is installed on the top of the working box, a discharge port is opened at the bottom of the working box, two discharge pipes are installed at the bottom of the emulsification tank, and valves are installed on the outside of the two discharge pipes.
[0017] Technical effects and advantages of the present invention:
[0018] 1. When the rotating rod rotates forward and backward, it will drive the rotating box to rotate forward and backward, so that the multiple moving rods will rotate, and then drive the multiple stirring rods installed on the multiple moving rods to rotate. At this time, the threaded sleeve will move up and down on the outside of the threaded rod, so that the multiple moving rods can move up and down while rotating, so that the multiple stirring rods can move up and down during the rotation process, thus avoiding dead angles in the mixing process of the raw materials and improving the uniformity of the raw material mixing. At the same time, driven by the transmission mechanism, the connecting rod will rotate, and when the connecting rod rotates, the emulsification tank will rotate through the cooperation of the second gear and the third gear. The forward and reverse rotation of the emulsification tank further accelerates the mixing of the raw materials and improves the mixing efficiency of the raw materials.
[0019] 2. First, the obtained prefabricated mixture is subjected to a certain temperature homogenization technology to prepare a high-stability and fast-curing nano-modified silicate resin, and the solid content of the obtained high-stability and fast-curing nano-modified silicate resin reaches 38% to 42%.
[0020] 3. First, heat the prefabricated mixture to 40-80°C, then stir and homogenize at this temperature, and finally obtain highly stable, compatible and fast-curing potassium silicate inorganic nanomaterials in an emulsifying tank. The process steps are simple and easy to operate, and no waste water, waste residue and waste gas are generated, which is beneficial to environmental protection. At the same time, this preparation method is a physical reaction of homogenous stirring, with low energy consumption and high safety.
[0021] 4. Because the preparation method contains multi-branched polyether, this type of polyether not only effectively prevents the high compatibility and fast curing nano-modified silicate resin from destroying the emulsification system of the organic emulsion after high addition in the water paint, and improves its storage stability, but also this type of stabilizer has good stability in the water paint, and has a long stabilizing effect time on the high compatibility and fast curing inorganic nano-resin, so that the storage time of the high stability and fast curing nano-modified silicate resin is longer and the storage stability is better. Therefore, the present invention significantly improves the storage stability of the high stability and fast curing nano-modified silicate resin in the water paint.
[0022] 5. Because the mass ratio of ordinary potassium silicate aqueous solution, water, silica sol, polyether, nano titanium dioxide, quaternary ammonium salt and flake caustic soda in the preparation method is 100: 5-15: 35-55: 1-5: 0.5-5: 0.1-0.3: 0.5-5, the high stability and fast curing nano-modified silicate resin prepared under this ratio can be added in an amount of up to 30% in the formulation of architectural and industrial water-based coatings and can be used as the main film-forming material. Therefore, the product prepared by the present invention has high compatibility with water-based organic resins and fast curing strength.
[0023] 6. Because the preparation method contains quaternary ammonium salt, this type of quaternary ammonium salt can form a stable anchored stable structure in the polysilanol, so that the high-stability and fast-curing nano-modified silicate resin has a longer storage time and better storage stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 It is a schematic diagram of the overall structure of the present invention.
[0025] Figure 2 It is a schematic diagram of the local structure of the present invention.
[0026] Figure 3 It is a schematic diagram of the top structure of the present invention.
[0027] Figure 4 For the present invention Figure 1 Schematic diagram of the enlarged structure at point A in the middle.
[0028] Figure 5 For the present invention Figure 1 Schematic diagram of the enlarged structure at point B in the middle.
[0029] Figure 6 For the present invention Figure 1 Schematic diagram of the enlarged structure at point C in the middle.
[0030] In the figure: 1. working box; 2. emulsifying tank; 3. rotating rod; 4. rack; 5. push rod; 6. limiting sleeve; 7. pulley; 8. belt; 9. connecting rod; 10. second gear; 11. stirring rod; 12. moving rod; 13. strip mouth; 14. threaded rod; 15. feed hopper; 16. heating box; 17. spiral heating tube; 18. third gear; 19. support rod; 20. support plate; 21. discharge port; 22. first gear; 23. rotating disk; 24. rotating motor; 25. rotating box; 26. threaded sleeve; 27. ball; 28. annular groove; 29. discharge pipe. DETAILED DESCRIPTION
[0031] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] The present invention provides Figure 1-6 The preparation method of the highly stable, compatible and fast-curing potassium silicate inorganic nanomaterial comprises the following steps:
[0033] S1. At room temperature, first add ordinary potassium silicate aqueous solution to a high-speed homogenizing emulsification tank, stir to form a vortex, then add water, silica sol, polyether, nano titanium dioxide, flake caustic soda, quaternary ammonium salt in sequence, and then mix evenly at a certain temperature to obtain a mixture. This addition sequence effectively avoids gelation between the raw materials and is conducive to obtaining high-quality products.
[0034] S2, then the prefabricated mixture is heated to 40-80°C in an emulsification tank. In order to ensure that the nanoparticles and the quaternary ammonium salt between the raw materials remain anchored during the entire process, the present invention first heats the prefabricated mixture to 40-80°C, and then at this temperature, high-speed dispersion and homogenization are performed at a speed of 1500-3000rpm, and the homogenization time is 50-100min.
[0035] According to S1, the mass ratio of ordinary potassium silicate aqueous solution, water, silica sol, polyether, nano titanium dioxide, quaternary ammonium salt and caustic soda is 100: 5-15: 35-55: 1-5: 0.5-5: 0.1-0.3: 0.5-5, the stirring speed is 1500-3000rmp homogenization, the homogenization temperature is 40-80°C, and the homogenization time is 50-100min. Since the drop amount of quaternary ammonium salt is very important for the rapid curing of high-stability rapid-curing inorganic potassium silicate resin, the drop amount of quaternary ammonium salt is controlled to 0.1-0.3 in the present invention.
[0036] The modulus of ordinary potassium silicate aqueous solution is 3.3 to 3.5, the solid content is 38% to 42%, the water is deionized water or industrial tap water, and the solid content of silica sol is 26% to 32%, by adding silica sol, the influence of excessive potassium ions in potassium silicate on water resistance can be reduced, and the hardness and curing speed of the coating can be quickly improved. The polyether is the hyperbranched polyether SE10 of France Sipusen Chemical, the average particle size of nano titanium dioxide is 5nm, and the solid content is 5%. Nano titanium dioxide is used to catalyze the organic matter in the coating through ultraviolet rays in natural light to produce high concentrations of carbon dioxide to accelerate the silanol polycondensation curing in the inorganic nano silicate resin. The quaternary ammonium salt is one or more quaternary ammonium salts containing decanyl and dodecyl groups, and the flake alkali is industrial grade sodium hydroxide. Due to the strong alkalinity and strong electrolyte properties of the highly stable and fast-curing nano-modified silicate resin in water, it is easy to cause the emulsifier of the acrylic emulsion to produce an electrolyte reaction, causing the emulsion to break and making the inorganic coating unable to be stored. Therefore, an appropriate stabilizer should be selected to extend its storage time. By selecting the multi-branched polyether quaternary ammonium salt flake alkali as a co-stabilizer, the co-stabilizer is easy to form silanol anchoring under a temperature and homogeneous conditions, which reduces the reaction activity and ensures that the highly stable and fast-curing modified silicate resin is stored stably for a long time in the coating formula.
[0037] A production device for highly stable, compatible and fast-curing potassium silicate inorganic nanomaterials includes a working box 1, an emulsifying tank 2 is installed inside the working box 1 through a supporting mechanism, a rotating box 25 is installed inside the emulsifying tank 2, a stirring mechanism is installed inside the rotating box 25, a rotating rod 3 is fixedly connected to the top of the rotating box 25, one end of the rotating rod 3 passes through the working box 1 and extends to the outside of the working box 1, a first rotating mechanism for driving the rotating rod 3 to rotate is installed outside the working box 1, a second rotating mechanism for driving the emulsifying tank 2 to rotate is installed on one side of the working box 1, a spiral heating tube 17 and a heating box 16 are installed outside the emulsifying tank 2, and the spiral heating tube 17 is located outside the heating box 16.
[0038] The supporting mechanism includes a plurality of supporting rods 19 installed at the bottom of the emulsifying tank 2 and a plurality of balls 27 installed at the bottom of the plurality of supporting rods 19 . An annular groove 28 is provided on the bottom inner wall of the working box 1 , and the plurality of balls 27 are slidably connected inside the annular groove 28 .
[0039] The stirring mechanism includes a plurality of moving rods 12 installed inside the emulsification tank 2 and a plurality of stirring rods 11 installed outside the plurality of moving rods 12. A support plate 20 is installed inside the working box 1. A threaded rod 14 is fixedly connected to the top of the support plate 20. The top of the threaded rod 14 passes through the emulsification tank 2 and extends to the inside of the rotating box 25. One end of the threaded rod 14 located inside the emulsification tank 2 is fixedly connected to the top inner wall of the rotating box 25. The external thread of the threaded rod 14 is connected to a threaded sleeve 26. The external of the rotating box 25 is provided with a plurality of strip openings 13. The plurality of moving rods 12 respectively pass through the plurality of strip openings 13 and extend to the inside of the rotating box 25. One end of each moving rod 12 located inside the rotating box 25 is fixedly connected to the outside of the threaded sleeve 26. When the rotating rod 3 rotates forward and backward, it will drive the rotating box 25 to rotate forward and backward, so that the multiple moving rods 12 will rotate, and then drive the multiple stirring rods 11 installed on the multiple moving rods 12 to rotate. At this time, the threaded sleeve 26 will move up and down on the outside of the threaded rod 14, so that the multiple moving rods 12 can move up and down while rotating, so that the multiple stirring rods 11 can move up and down during the rotation process, thereby avoiding dead corners in the process of mixing the raw materials and improving the uniformity of the raw material mixing.
[0040] The first rotating mechanism includes a rotating motor 24 installed on the outside of the working box 1 and a rotating disk 23 installed on the output end of the rotating motor 24. A push rod 5 is rotatably connected to one side of the rotating disk 23. A rack 4 is hinged at one end of the push rod 5. A first gear 22 meshing with the rack 4 is installed on the outside of the rotating rod 3. A limiting sleeve 6 for limiting the rack 4 is installed on the top of the working box 1.
[0041] The second rotating mechanism includes a connecting rod 9 installed on one side of the working box 1 and a second gear 10 installed at the bottom of the connecting rod 9. A third gear 18 meshing with the second gear 10 is installed on the outside of the emulsification tank 2. The connecting rod 9 and the rotating rod 3 are connected by a transmission mechanism, wherein the transmission mechanism includes two pulleys 7 installed on the outside of the connecting rod 9 and the rotating rod 3, and the two pulleys 7 are rotatably connected by a belt 8. Driven by the transmission mechanism, the connecting rod 9 will rotate. When the connecting rod 9 rotates, the emulsification tank 2 will rotate through the cooperation of the second gear 10 and the third gear 18. The forward and reverse rotation of the emulsification tank 2 further accelerates the mixing of the raw materials and improves the mixing efficiency of the raw materials.
[0042] A feed hopper 15 is installed on the top of the working box 1, a discharge port 21 is opened at the bottom of the working box 1, and two discharge pipes 29 are installed at the bottom of the emulsification tank 2, and valves are installed outside the two discharge pipes 29.
[0043] Embodiment 1: At room temperature, first, a common potassium silicate aqueous solution with a modulus of 3.3 and a solid content of 39.8% is added to the emulsification tank 2 through the feed hopper 15. At this time, the rotary motor 24 can be started. When the rotary motor 24 rotates, deionized water, silica sol with a solid content of 38%, polyether, and nano titanium dioxide can be added to the emulsification tank 2 through the feed hopper 15 in sequence, and finally a quaternary ammonium salt is added dropwise, wherein the mass ratio of the common potassium silicate aqueous solution, water, silica sol, polyether, nano titanium dioxide, dodecahydrate, and caustic soda is 100: 7.5: 36: 1.5: 2: 0.3:1.0, when the rotating motor 24 rotates, the rotating disk 23 can be driven to rotate, when the rotating disk 23 rotates, the moving rod 5 can be driven to move, when the moving rod 5 moves, the rack 4 can be driven to move, through the cooperation of the rack 4 and the first gear 22, the rotating rod 3 can be driven to rotate, when the rack 4 moves to the left, the rotating rod 3 will rotate forward, when the rack 4 moves to the right, it will drive the rotating rod 3 to rotate in the opposite direction, thereby driving the rotating box 25 to rotate forward and reversely, driven by the rotation of the rotating box 25, the multiple moving rods 12 will rotate, thereby driving the multiple stirring rods 11 installed on the multiple moving rods 12 to rotate, and at the same time, the threaded sleeve 26 will move up and down outside the threaded rod 14, so that the multiple moving rods 12 can move up and down while rotating, so that the multiple stirring rods 11 can move up and down during the rotation, Avoid dead angles in the process of mixing raw materials, improve the uniformity of raw material mixing, when the rotating rod 3 rotates, it will drive one of the belt wheels 7 to rotate, through the cooperation of the two belt wheels 7 and the belt 8, the connecting rod 9 will rotate, when the connecting rod 9 rotates, it will drive the second gear 10 to rotate, through the cooperation of the second gear 10 and the third gear 18, the emulsification tank 2 will rotate, through the positive and negative rotation of the emulsification tank 2 and the stirring of the stirring mechanism, the mixing of the raw materials is further accelerated, and the efficiency of raw material mixing is improved. When the raw materials are evenly mixed, a prefabricated mixture can be obtained. At this time, the spiral heating tube 17 can be started, and the prefabricated mixture can be heated to 65°C through the spiral heating tube 17. Then, at this temperature, the heated prefabricated mixture is stirred and homogenized at 2000rmp, and the stirring time of the mixture is 60min. Finally, the product modified silicate resin is obtained, and then the modified silicate resin is applied to the following coating formula:
[0044] Product name and model Addition amount water 30.0 Defoamer SD250 0.2 Wetting and dispersing agent Disperbx s60 / 100 0.6 Anionic cellulose ether S30000YP2 0.3 AMP95C 0.2 Titanium Dioxide 15 Calcium carbonate 25 Acrylic Emulsion 5.0 Silicone water repellent SI50 1.0 Modified silicate resin 20
[0045] The coating was prepared according to the chart, and then the coating plate was cured under standard experimental conditions for 7 days. The relevant properties of the coating were tested and the conclusions were obtained:
[0046] The solid content of modified silicate resin in the coating is 39.65%. The viscosity change of the formula according to the application is 10KU, and the washing resistance is 11000 times.
[0047] Embodiment 2: According to the same operating steps as in embodiment 1, the mass ratio of ordinary potassium silicate aqueous solution, water, silica sol, polyether, nano titanium dioxide, dodecaquaternary ammonium salt and flake caustic soda is changed to 100:7.5:36:2.5:2:0.3:1.0, and then a prefabricated mixture is prepared, and the prefabricated mixture is heated to 75°C. The heated prefabricated mixture is stirred at 2200rmp for homogenization, and the stirring time of the mixture is 70min.
[0048] The same coating was prepared according to the same formula as in Example 1, and then the performance of the coating was tested in the same manner as in Example 1, and the conclusion was:
[0049] The solid content of the modified silicate resin in the coating is 39.6%, the viscosity change of the coating prepared by the product is 5KU, and the washing resistance is 11000 times.
[0050] Embodiment 3: According to the same operating steps as in embodiment 1, the mass ratio of ordinary potassium silicate aqueous solution, water, silica sol, polyether, nano titanium dioxide, dodecaquaternary ammonium salt and flake caustic soda is changed to 100: 7.5: 36: 2.5: 2: 0.25: 1.0, and then a prefabricated mixture is prepared, and the prefabricated mixture is heated to 85° C. The heated prefabricated mixture is stirred at 2500 rpm for homogenization, and the stirring time of the mixture is 80 min.
[0051] The same coating was prepared according to the same formula as in Example 1, and then the performance of the coating was tested in the same manner as in Example 1, and the conclusion was:
[0052] The solid content of the modified silicate resin in the coating is 39.1%, the viscosity change of the coating prepared by the product is 8KU, and the washing resistance is 14000 times.
[0053] Embodiment 4: According to the same operating steps as in embodiment 1, the mass ratio of ordinary potassium silicate aqueous solution, water, silica sol, polyether, nano titanium dioxide, dodecaquaternary ammonium salt and flake caustic soda is changed to 100: 7.5: 38: 2.5: 2: 0.25: 1.0, and then a prefabricated mixture is prepared, and the prefabricated mixture is heated to 70° C. The heated prefabricated mixture is stirred at 1800 rpm for homogenization, and the stirring time of the mixture is 80 min.
[0054] The same coating was prepared according to the same formula as in Example 1, and then the performance of the coating was tested in the same manner as in Example 1, and the conclusion was:
[0055] The solid content of the modified silicate resin in the coating is 39.5%, the viscosity change of the coating prepared by the product is 10KU, and the washing resistance is 15,000 times.
[0056] Example 5: According to the same operating steps as in Example 1, the mass ratio of ordinary potassium silicate aqueous solution, water, silica sol, polyether, nano titanium dioxide, dodecaquaternary ammonium salt, and flake caustic soda is replaced with 100: 9.5: 38: 2.5: 2: 0.25: 1.0, and then a prefabricated mixture is prepared, and the prefabricated mixture is heated to 85° C. The heated prefabricated mixture is stirred at 3000 rpm for homogenization, and the stirring time of the mixture is 70 min.
[0057] The same coating was prepared according to the same formula as in Example 1, and then the performance of the coating was tested in the same manner as in Example 1, and the conclusion was:
[0058] The solid content of the modified silicate resin in the coating is 39.1%, the viscosity change of the coating prepared by the product is 10KU, and the washing resistance is 13000 times.
[0059] Example 6: According to the same operating steps as in Example 1, the mass ratio of ordinary potassium silicate aqueous solution, water, silica sol, polyether, nano titanium dioxide, dodecaquaternary ammonium salt, and flake caustic soda is replaced with 100: 10: 38: 2.5: 2: 0.25: 1.0, and then a prefabricated mixture is prepared, and the prefabricated mixture is heated to 85° C. The heated prefabricated mixture is stirred at 2600 rpm for homogenization, and the stirring time of the mixture is 80 min.
[0060] The same coating was prepared according to the same formula as in Example 1, and then the performance of the coating was tested in the same manner as in Example 1, and the conclusion was:
[0061] The solid content of the modified silicate resin in the coating is 39.2%, the viscosity change of the coating prepared by the product is 4KU, and the washing resistance is 14500 times.
[0062] Example 7: According to the same operating steps as in Example 1, the mass ratio of ordinary potassium silicate aqueous solution, water, silica sol, polyether, nano titanium dioxide, dodecaquaternary ammonium salt, and flake caustic soda is replaced with 100: 7.5: 50: 2.5: 2: 0.25: 1.0, and then a prefabricated mixture is prepared, and the prefabricated mixture is heated to 48° C. The heated prefabricated mixture is stirred at 1500 rpm for homogenization, and the stirring time of the mixture is 50 min.
[0063] The same coating was made according to the same formula as in Example 1, and then the performance of the coating was tested in the same way as in Example 1, and the conclusion was:
[0064] The solid content of modified silicate resin in the coating is 39.20%. The coating prepared by the product has a viscosity change of 12KU and a washability of 12500 times.
[0065] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A production device for a method for preparing a highly stable and compatible potassium silicate inorganic nanomaterial, comprising a working box (1), an emulsifying tank (2) being installed inside the working box (1) via a supporting mechanism, a rotating box (25) being installed inside the emulsifying tank (2), a stirring mechanism being installed inside the rotating box (25), a rotating rod (3) being fixedly connected to the top of the rotating box (25), one end of the rotating rod (3) passing through the working box (1) and extending to the outside of the working box (1), a first rotating mechanism for driving the rotating rod (3) to rotate being installed outside the working box (1), a second rotating mechanism for driving the emulsifying tank (2) to rotate being installed on one side of the working box (1), a spiral heating tube (17) and a heating box (16) being installed outside the emulsifying tank (2), and the spiral heating tube (17) being located outside the heating box (16); The support mechanism comprises a plurality of support rods (19) mounted on the bottom of the emulsification tank (2) and a plurality of balls (27) mounted on the bottom of the plurality of support rods (19); an annular groove (28) is provided on the inner wall of the bottom of the working box (1); and the plurality of balls (27) are slidably connected inside the annular groove (28); The stirring mechanism comprises a plurality of movable rods (12) installed inside the emulsification tank (2) and a plurality of stirring rods (11) installed outside the plurality of movable rods (12); a support plate (20) is installed inside the working box (1); a threaded rod (14) is fixedly connected to the top of the support plate (20); the top of the threaded rod (14) passes through the emulsification tank (2) and extends to the inside of the rotating box (25); one end of the threaded rod (14) located inside the emulsification tank (2) is fixedly connected to the top inner wall of the rotating box (25); the outer thread of the threaded rod (14) is connected to a threaded sleeve (26); a plurality of strip openings (13) are provided on the outside of the rotating box (25); the plurality of movable rods (12) respectively pass through the plurality of strip openings (13) and extend to the inside of the rotating box (25); and one end of the plurality of movable rods (12) located inside the rotating box (25) is fixedly connected to the outside of the threaded sleeve (26); The method for preparing the highly stable, compatible and fast-curing potassium silicate inorganic nanomaterial is characterized in that: The steps include: S1. At room temperature, first add a common potassium silicate aqueous solution into a high-speed homogenization emulsification tank, stir to form a vortex, then add water, silica sol, polyether, nano titanium dioxide, flake caustic soda, quaternary ammonium salt in sequence, and then mix evenly at a certain temperature to obtain a mixture; S2, then heating the prefabricated mixture to 40-80°C in an emulsifying tank, and then performing high-speed dispersion and homogenization at this temperature at a speed of 1500-3000rpm for a homogenization time of 50-100min; Wherein, the mass ratio of the common potassium silicate aqueous solution, water, silica sol, polyether, nano titanium dioxide, quaternary ammonium salt, and caustic soda in step S1 is 100: 5-15: 35-55: 1-5: 0.5-5: 0.1-0.3: 0.5-5, the stirring speed is 1500-3000rmp homogenization, the homogenization temperature is 40-80°C, the homogenization time is 50-100min, the modulus of the common potassium silicate aqueous solution is 3.3-3.5, the solid content is 38%-42%, the water is one of deionized water and industrial tap water, the solid content of the silica sol is 26%- 32%, the polyether is the hyperbranched polyether SE10 produced by France Sipusen Chemical, the average particle size of the nano titanium dioxide is 5nm, the solid content is 5%, the quaternary ammonium salt is one or more quaternary ammonium salts containing decanyl and dodecyl groups, and the flake caustic soda is industrial grade sodium hydroxide.
2. The production device for the preparation method of a highly stable, compatible and fast-curing potassium silicate inorganic nanomaterial according to claim 1, characterized in that: The first rotating mechanism comprises a rotating motor (24) mounted on the outside of the working box (1) and a rotating disk (23) mounted on the output end of the rotating motor (24); a push rod (5) is rotatably connected to one side of the rotating disk (23); a rack (4) is hingedly connected to one end of the push rod (5); a first gear (22) meshing with the rack (4) is mounted on the outside of the rotating rod (3); and a limiting sleeve (6) for limiting the position of the rack (4) is mounted on the top of the working box (1).
3. The production device for the preparation method of a highly stable, compatible and fast-curing potassium silicate inorganic nanomaterial according to claim 1, characterized in that: The second rotating mechanism comprises a connecting rod (9) mounted on one side of the working box (1) and a second gear (10) mounted at the bottom of the connecting rod (9); a third gear (18) meshing with the second gear (10) is mounted on the outside of the emulsification tank (2); the connecting rod (9) and the rotating rod (3) are connected to each other through a transmission mechanism, wherein the transmission mechanism comprises two pulleys (7) mounted on the outside of the connecting rod (9) and the rotating rod (3); the two pulleys (7) are connected in rotation through a belt (8).
4. The production device for the preparation method of a highly stable, compatible and fast-curing potassium silicate inorganic nanomaterial according to claim 1, characterized in that: A feed hopper (15) is installed on the top of the working box (1), a discharge port (21) is provided at the bottom of the working box (1), and two discharge pipes (29) are installed at the bottom of the emulsification tank (2), and valves are installed on the outside of the two discharge pipes (29).
Citation Information
Patent Citations
Organic and inorganic compound waterborne paint for exterior walls and preparation method thereof
CN107083135A
Inorganic liquid coating and preparation method thereof
CN112876888A