MEMS infrared light source and preparation method thereof
Through the enhanced interface binding force of the tungsten-nanomorphic carbon composite thermal resistance material and the Ti/TiN transition layer, and the diamond-like film is prepared in combination with graphite targets, the problems of resistivity drift and high cost of MEMS infrared light sources at high temperatures are solved, and the problem of resistance drift and high cost of MEMS infrared light sources is realized. High efficiency and stable medium and long infrared radiation performance, suitable for infrared gas sensors.
Patent Information
- Application Number
- CN202111067218.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-09-13
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2041-09-13
AI Technical Summary
The existing MEMS infrared light sources have problems of resistivity drift and high cost at high temperatures, and the high stress of the nano-amorphous carbon thin film limits its thickness and interface bonding force, affecting its practicality.
The surface adhesion of the substrate is enhanced by the Ti/TiN transition layer, and the graphite target is used for unbalanced magnetron sputtering. Diamond-like film is prepared using silicon oxide and silicon nitride. The dielectric layer reduces heat conduction loss, integrates infrared radiation, and achieves higher radiation temperature and more stable thermal response.
It achieves higher radiation temperature and more stable thermal response, excellent medium and far infrared radiation performance, and is simple, low-cost and easy to mass production.
Smart Images

Figure CN113791048B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of NDIR gas sensors, and in particular to a MEMS infrared light source and a preparation method thereof. Background Art
[0002] In NDIR gas sensors, infrared light sources emit infrared light, and gas molecules such as carbon dioxide, carbon monoxide, and methane that can produce dipole moment changes are absorbed because they resonate with infrared light. Specific gas molecules will only resonate with infrared light of a specific wavelength. Different gas concentrations will cause different energies of infrared light to be absorbed. Therefore, the detector can detect changes in infrared radiation energy at the other end, and use this to analyze gas composition and calculate gas concentration. Therefore, the performance of infrared light sources directly affects the performance of infrared gas sensors. Compared with the application range of traditional tungsten filament lamps that are limited to wavelengths exceeding 5um, MEMS infrared light sources can achieve broadband infrared emission at infrared wavelengths of 2 to 10um. The development of MEMS technology has realized electrically modulated infrared light sources, and has now become the mainstream technology for manufacturing infrared light sources used in NDIR gas sensors.
[0003] Thermal radiation MEMS infrared light source is a device that converts the thermal energy information of resistor Joule heating into infrared radiation. In the design of infrared light source, thermal resistance materials with both high temperature resistance and high emissivity are the key to the light source. At present, people have conducted a lot of research on infrared light sources based on platinum and polysilicon heating resistors. Platinum is currently a widely used heating material due to its high thermal conductivity, chemical inertness and good temperature stability. However, the resistivity is prone to drift at >550℃. In addition, platinum, as a precious metal material, has a high manufacturing cost. When the temperature of polysilicon is greater than 300℃, the long-term stability is poor, and the resistivity will also drift at high temperature (500℃). In contrast, tungsten has a high melting point (3422℃) and can resist electromigration effects at high temperatures. It has become a replaceable heating material at high temperatures, with long-term stability, low cost and strong process compatibility.
[0004] Nano-amorphous carbon film materials with diamond-like carbon (DLC) structure are composed of a carbon network with a high relative ratio of sp3 and sp2 carbon, and have higher temperature stability, mechanical stability and light absorption transmittance. DLC film has excellent transparency in the entire infrared band. Diamond-like film has a wide optical band gap range, high photoluminescence and electroluminescence rates at room temperature, and can emit light in the entire visible light range, which makes diamond-like film one of the luminescent materials with excellent performance. However, the high stress of amorphous carbon film limits its thickness, interface bonding strength, etc., which seriously affects the practical application of the film. Summary of the invention
[0005] The main purpose of the present invention is to provide a MEMS infrared light source and a preparation method thereof which can achieve a higher radiation temperature and a more stable thermal response in view of the above problems.
[0006] The present invention provides a MEMS infrared light source, which is mainly characterized in that the infrared light source includes a substrate and a front structure supported on the substrate, the front structure includes, from bottom to top, a double-layer dielectric layer, a tungsten heating resistor layer, an adhesion layer, a nano-amorphous carbon layer, and a passivation layer, the tungsten heating resistor layer includes a coiled tungsten structure, a silicon oxide layer deposited in the tungsten structure, and a metal electrode arranged on the tungsten structure.
[0007] Preferably, the double-layer dielectric layer is a silicon oxide dielectric layer and a silicon nitride dielectric layer, and the silicon nitride dielectric layer is disposed on the silicon oxide layer.
[0008] Preferably, the thickness of the silicon oxide dielectric layer is 1500±30 nm; the thickness of the silicon nitride dielectric layer is 1000±30 nm.
[0009] Preferably, the back side of the substrate has a cavity.
[0010] Preferably, the substrate is single crystal silicon; and the nano-amorphous carbon layer is a diamond-like structure.
[0011] Preferably, the adhesion layer is a Ti / TiN layer; and the passivation layer is a silicon nitride layer.
[0012] Preferably, the thickness of the coiled tungsten structure is 300±30nm; the thickness of the silicon oxide layer is 300±10nm; the thickness of the adhesion layer is 20±2nm; the thickness of the nano-amorphous carbon layer is 50±5nm; and the thickness of the passivation layer is 200±20nm.
[0013] Preferably, the coiled tungsten structure is formed by a plurality of embedded circular rings with an outer diameter of 1.3 mm connected in series, the heating wires are spaced 5 um apart, and the distance between the heater edge and the silicon substrate is 315 um; the coiled tungsten structure is annealed under nitrogen protection.
[0014] The present invention also provides a method for preparing a MEMS infrared light source, the method comprising the following steps:
[0015] (1) Thermal oxidation on a single crystal silicon substrate;
[0016] (2) Growth of silicon-rich Si3N4 thin films by low-pressure vapor deposition;
[0017] (3) Forming a tungsten coil structure in the silicon-rich Si3N4 film;
[0018] (4) depositing a silicon oxide layer in the tungsten coil structure;
[0019] (5) deposition of an adhesion layer;
[0020] (6) depositing a nano-amorphous carbon layer;
[0021] (7) evaporating a metal electrode on the coiled tungsten structure;
[0022] (8) depositing a passivation layer on the nano-amorphous carbon layer;
[0023] (9) Etch the back side to release the back cavity.
[0024] Preferably, the thermal oxidation in step (1) is carried out by introducing dry oxygen gas and wet oxygen gas to oxidize the surface of the substrate, and the thickness of the obtained silicon oxide layer is 1500±30nm;
[0025] The reaction gas pressure of the low-pressure vapor deposition in step (2) is 250 mTorr, and the thickness of the obtained silicon-rich Si3N4 film is 1000±30 nm;
[0026] The coiled tungsten structure in step (3) adopts an unbalanced magnetron sputtering equipment system and a metal lift-off process. The coiled tungsten heater is designed to be a plurality of embedded circular rings with an outer diameter of 1.3 mm in series. The heating wires are spaced 5 μm apart, and the distance between the heater and the silicon substrate is 315 μm to better reduce heat loss. The process conditions during sputtering are as follows: the vacuum chamber is evacuated to at least 4×10 -3 Pa, then argon gas 20sccm was introduced to maintain the vacuum degree at 1mTorr, the sputtering power was 1200W, and the negative bias voltage was 300V for 5min. The rotation speed of the sample stage was kept at 5rpm, and then the negative bias voltage was 60V, and the sputtering was carried out for 20min. The thickness of the obtained tungsten disk structure was 300±30nm. In order to improve the stability of the resistor at high temperature, the heating resistor was annealed at 800℃ for 1 hour under nitrogen protection, and the resistance of the obtained tungsten disk hot wire was 40Ω at room temperature.
[0027] The thickness of the silicon oxide layer in step (4) is 300±10 nm;
[0028] In the step (5), an unbalanced magnetron sputtering device system is used to deposit the Ti / TiN adhesion layer. Before the deposition, the vacuum chamber is evacuated to at least 4x10 -3Pa, then argon was introduced, the vacuum was maintained at 0.2Pa, and bombarded for 30min under a negative bias of 500V, and then a layer of pure Ti film was deposited under a negative bias of 200V, the deposition time was 1min, and the current was 0.8A; then the pressure remained unchanged, and a gas with a ratio of argon to nitrogen of 2:3 was introduced, the power was 100W, and the deposition time was 4min; the thickness of the obtained adhesion layer was 20±2nm;
[0029] In the step (6), an unbalanced magnetron sputtering device system is used to deposit the aC diamond-like amorphous carbon layer. Before the deposition, the vacuum chamber is evacuated to at least 4x10 -3 Pa, then argon was introduced, the vacuum degree was maintained at 0.67 Pa, the sputtering power was 150 W, the pre-sputtering was 5 min, and the deposition time was 70 min; the thickness of the obtained nano amorphous carbon layer was 50 ± 5 nm;
[0030] In the step (7), the metal electrodes are Ni and Au electrodes respectively;
[0031] The thickness of the passivation layer in step (8) is 200±20nm.
[0032] The MEMS infrared light source and its preparation method of the present invention are adopted, and a tungsten-nano amorphous carbon composite thermal resistance material is adopted. The nano amorphous carbon is a diamond-like carbon (DLC) structure. The surface adhesion of the substrate is enhanced by a Ti / TiN transition layer, which can effectively reduce the internal stress of the DLC and improve the DLC interface bonding force. The diamond-like film is prepared by unbalanced magnetron sputtering using a graphite target; a buffer stress layer silicon oxide (SiO2) and a silicon-rich silicon nitride (Si3N4) double-layer dielectric layer are used as a supporting film layer; the suspended film structure can reduce the heat conduction loss, and the infrared radiation integrated on the surface of the heating resistor composite material can improve the radiation efficiency of the infrared light source. The infrared light source device of the present invention has a radiation self-enhancement effect, can achieve a higher radiation temperature and a more stable thermal response, and achieve excellent mid- and far-infrared radiation performance. In addition, the process preparation is simple, low-cost, and easy to mass produce. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] like Figures 1-1 to 1-10 It is a schematic diagram of the method for preparing the MEMS infrared light source of the present invention.
[0034] Figure 2 This is a diagram showing the results of an AFM atomic force microscope analysis of the quality of the tungsten coating in an embodiment of the MEMS infrared light source of the present invention.
[0035] Figure 3 This is the Raman spectrum of diamond-like carbon of the embodiment of the MEMS infrared light source of the present invention.
[0036] Figure 4It is a schematic structural diagram of the coiled tungsten structure in the MEMS infrared light source of the present invention.
[0037] Figure 5a The figure is a relationship diagram between the current and resistance of the infrared light source device of the MEMS infrared light source of the present invention.
[0038] Figure 5b The figure is a relationship diagram between power consumption and temperature of the infrared light source device using the MEMS infrared light source of the present invention.
[0039] Figure 6 This is a diagram showing the resistance drift of an infrared light source device using the MEMS infrared light source of the present invention. DETAILED DESCRIPTION
[0040] The scheme of the present invention will be explained below in conjunction with the embodiments. It will be appreciated by those skilled in the art that the following embodiments are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. If no specific techniques or conditions are specified in the embodiments, the techniques or conditions described in the literature in this area or the product instructions are used. The reagents or instruments used are conventional products that can be obtained commercially without specifying the manufacturer. The experimental methods used are conventional methods unless otherwise specified.
[0041] like Figures 1-1 to 1-10 As shown, a method for preparing a MEMS infrared light source provided by the present invention comprises the following steps:
[0042] (1) Figure 1-1 show <100> The crystal orientation of the single crystal silicon substrate 1, <100> The monocrystalline silicon substrate 1 is thermally oxidized to obtain a silicon dioxide dielectric layer 2. Figure 1-2 The structure shown;
[0043] Thermal oxidation is mainly prepared by introducing dry + wet oxygen gas to oxidize the silicon surface under high temperature conditions. At a high temperature of 1100°C, 1.5L / min O2 is introduced for 20 minutes and dry oxygen is carried out for 150 minutes to prepare silicon oxide with a thickness of 1500±30nm.
[0044] (2) Low-pressure vapor deposition grows a silicon-rich Si3N4 film to obtain a silicon nitride dielectric layer 3, which can be referred to as Figure 1-3 The structure shown;
[0045] Low stress silicon-rich Si3N4 thin films are prepared by LPCVD. The pressure in the reaction chamber is reduced to increase the mean free path of process gas molecules, so that enough reactants can reach the surface of the silicon wafer to deposit into a film.
[0046] The specific process conditions are: 865±5℃ at the furnace tail, 850±5℃ in the furnace, 750±5℃ at the furnace mouth, 200sccm of dichlorosilane, 40sccm of ammonia, 250mTorr of reaction gas pressure, 180 minutes of growth, to prepare silicon-rich silicon nitride with a thickness of 1000±30nm.
[0047] The silicon-rich silicon nitride layer has strong infrared absorption characteristics in the mid- and far-infrared bands, which can effectively reduce the loss of front radiation caused by the heating light source penetrating at the bottom.
[0048] Buffer stress layer silicon oxide (SiO2) and silicon-rich silicon nitride (S i 3N4) The overall stress of the double-layer dielectric layer is ≈87MPa.
[0049] (3) Forming a tungsten coil structure 4 on a silicon-rich Si3N4 film, as shown in FIG. Figure 1-4 The structure shown;
[0050] like Figure 4 As shown in the figure, the coiled tungsten heater structure is designed to be composed of multiple embedded circular rings with an outer diameter of 1.3 mm in series. The heating wires are spaced 5 μm apart, and the distance between the heater and the silicon substrate is 315 μm to better reduce heat loss. The unbalanced magnetron sputtering equipment system is used, and the vacuum in the vacuum chamber before deposition is at least 4x10 -3 Pa, and then 20sccm of argon was introduced to maintain the vacuum degree at 1mTorr. In order to remove impurities on the surface of the substrate, the sputtering power was 1200W, and the bombardment was carried out under a negative bias voltage of 300V for about 5min. The rotation speed of the sample stage was maintained at about 5rpm, and then sputtering was carried out under a negative bias voltage of 60V for 20min. The metal stripping lift-off process was used to obtain a 300±30nm thick coiled tungsten heating resistor. The resistance of the obtained low-power tungsten coil heating wire at room temperature was 40Ω.
[0051] The coating quality was analyzed by AFM atomic force microscopy, and the results were as follows: Figure 2 As shown, the surface roughness RMS = 3.51 nm, the roughness is small, and the film is relatively smooth.
[0052] (4) Figure 1-5 As shown, a silicon oxide layer 5 is deposited in the coil-like tungsten structure 4;
[0053] PECVD plasma was used to deposit SiO2 dielectric film to separate the tungsten resistance wire from the Ti / TiN adhesion layer to avoid short circuit. The specific process conditions were: growth temperature 300℃, N2O:SiH4 gas flow ratio 11:5, RF power 150W, reaction gas pressure 200Pa, deposition time 15min, and growth thickness 300±10nm.
[0054] (5) Figure 1-6As shown, an adhesion layer 6 is deposited;
[0055] The Ti / TiN adhesion layer was deposited using an unbalanced magnetron sputtering system. Before deposition, the vacuum chamber was evacuated to at least 4x10 -3 Pa, then argon is introduced, and the vacuum is maintained at 0.2Pa. In order to remove impurities on the substrate surface, it is bombarded for about 30 minutes under a negative bias of 500V; then a layer of pure Ti film is deposited under a negative bias of 200V, the deposition time is about 1 minute, and the current is 0.8A; then the pressure remains unchanged, and a gas with a ratio of argon:nitrogen of 2:3 is introduced, the power is 100W, and the deposition time is 4 minutes; a metal lift-off process is used to obtain an adhesion layer with a thickness of 20±2nm. Through the metal lift-off process, the adhesion layer can be made into a square pattern to expose the tungsten disk hot wire connected to the electrode.
[0056] (6) Figure 1-7 As shown, a nano-amorphous carbon layer 7 is deposited;
[0057] Nano-amorphous carbon films usually have three phases, one is diamond-like, one is graphite-like, and one is polymer-like. Different types of amorphous carbon films have different SP3 contents, film hardness, internal stress and optical band gap. Diamond-like films have the characteristics of wide optical band gap range and highest infrared transmittance, high infrared selectivity, i.e. infrared anti-reflection, while nano-amorphous carbon films with diamond-like structures are not easy to prepare.
[0058] Only by preparing a diamond-like structure can the conditions of self-enhancement and high emissivity of infrared light sources be met. The nano-amorphous carbon containing a Ti / TiN adhesion layer provided by the present invention can be deposited in an unbalanced magnetron sputtering device system. Before deposition, the vacuum chamber is evacuated to at least 4x10 -3 Pa, then argon was introduced, the vacuum was maintained at 5mTorr, the sputtering power was 200W, the pre-sputtering was 5min, impurities such as oxidation on the target surface were removed, and the deposition time was 70min; a 50±5nm thick diamond amorphous carbon film was obtained by the metal lift-off process. The metal lift-off process made the nano amorphous carbon layer and the adhesion layer have the same pattern.
[0059] The peak position of Raman spectrum is between 1200 and 1450 cm -1 The D peak is located at 1500-1700 cm -1 The G peak of the amorphous carbon is used to confirm that the amorphous carbon has a diamond-like structure. Figure 3 The Raman spectrum of the diamond-like carbon obtained in the embodiment of the present invention is shown in FIG. 2 . Two peak positions are obtained by fitting the test results, wherein the D peak is located at 1350.4 cm -1 , G peak is located at 1549.8cm-1 .
[0060] (7) Figure 1-8 As shown, a metal electrode 8 is evaporated on the coiled tungsten structure;
[0061] The vacuum in the evaporation vacuum chamber should be at least 1.5x10 -3 Pa, evaporated Ni 150±10nm, Au 150±10nm, evaporation rate 2A / s;
[0062] After the gold-nickel composite metal film is evaporated, a photolithography mask can be used to protect the electrode area, and the areas outside are wet-etched by preparing a 6% FeCl3 solution and a KI:I:H2O (=4:1:28) solution to etch the Ni and Au electrode films.
[0063] (8) Figure 1-9 As shown, a passivation layer 9 is deposited on the nano-amorphous carbon layer;
[0064] PECVD plasma can be used to deposit Si3N4 thin film as the passivation layer. Silicon nitride itself has strong infrared absorption characteristics. The passivation layer is heated by the electrode to assist in exciting infrared light.
[0065] The specific process conditions are: growth temperature 300°C, NH3:SiH4 gas flow ratio 2:3, RF power 500W, reaction gas pressure 200Pa, deposition time 2.5min, and growth thickness 200±20nm.
[0066] (9) Figure 1-10 As shown, the back surface is etched to release the back cavity 10;
[0067] Back-side patterning is used for DRIE deep silicon etching. The specific process conditions are: C4F8 80sccm, SF6280sccm, O2 28sccm, RF etching upper power 35w, ICP etching upper power 1500w, ICP etching lower power 800w, and etching rate 4-5μm / min.
[0068] When the infrared light source device of the present invention is subjected to an external voltage, the resistance value increases as the current increases. Figure 5a As shown, the relationship between the power consumption of the six heating temperature points is as follows: Figure 5b As shown in the figure, when the heating temperature is ≤600℃, the required power is <250mW. In addition, in order to improve the stability of the resistor at high temperature, the heating resistor is annealed at 800℃ for 1 hour under nitrogen protection. It has been verified that annealing at 800℃ for 1 hour can ensure that the resistor does not drift under long-term heating conditions. Figure 6 As shown, the infrared light source is guaranteed to radiate stably. Therefore, the infrared light source device of the present invention has the characteristics of low power consumption and stable resistance value at high temperature.
[0069] The present invention uses a composite thermal resistance material composed of a tungsten disk hot wire and nano-amorphous carbon to prepare a MEMS infrared light source. Based on the heating and radiating infrared light, through the infrared anti-reflection effect of the nano-amorphous carbon film, the infrared absorption and anti-reflection of the composite film finally present a radiation self-enhancement effect, producing a high-emissivity composite material. The embodiment of the present invention shows an infrared absorption rate of more than 70% in the 3-10um mid-infrared band, which can be achieved at low cost, easy to mass produce, and has excellent infrared radiation performance.
[0070] The present invention adopts a composite thermal resistance material composed of tungsten disk hot wire and nano amorphous carbon to obtain a new infrared light source device with radiation self-enhancement effect, which can achieve higher radiation temperature and more stable thermal response, and achieve excellent mid- and far-infrared radiation performance. The MEMS infrared light source is integrated into the infrared gas sensing system and is the core component of the infrared gas detection device. It solves the problem of traditional sensors being poisoned or having reduced sensitivity due to direct contact with gas, and has great application value in environmental detection and industrial and mining production safety.
[0071] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A MEMS infrared light source, It is characterized in that The infrared light source comprises a substrate and a front structure supported on the substrate. The front structure comprises, from bottom to top, a double-layer dielectric layer, a tungsten heating resistor layer, an adhesion layer, a nano-amorphous carbon layer, and a passivation layer. The tungsten heating resistor layer comprises a coiled tungsten structure, a silicon oxide layer deposited in the tungsten structure, and a metal electrode arranged on the tungsten structure. The adhesion layer is a Ti / TiN layer, the nano-amorphous carbon layer is a diamond-like structure, the coiled tungsten structure and the nano-amorphous carbon layer form a composite thermal resistance material. Through the infrared transmittance-enhancing effect of the nano-amorphous carbon layer, the infrared absorption and transmittance-enhancing effect of the composite thermal resistance material present a radiation self-enhancement effect.
2. The MEMS infrared light source according to claim 1, It is characterized in that The double-layer dielectric layer is a silicon oxide dielectric layer and a silicon nitride dielectric layer, and the silicon nitride dielectric layer is arranged on the silicon oxide layer.
3. The MEMS infrared light source according to claim 2, It is characterized in that The thickness of the silicon oxide dielectric layer is 1500±30nm; the thickness of the silicon nitride dielectric layer is 1000±30nm.
4. The MEMS infrared light source according to claim 1, It is characterized in that The back side of the substrate has a cavity.
5. The MEMS infrared light source according to claim 1, It is characterized in that The substrate is single crystal silicon.
6. The MEMS infrared light source according to claim 1, It is characterized in that The passivation layer is a silicon nitride layer.
7. The MEMS infrared light source according to claim 1, It is characterized in that The thickness of the coiled tungsten structure is 300±30nm; the thickness of the silicon oxide layer is 300±10nm; the thickness of the adhesion layer is 20±2nm; the thickness of the nano-amorphous carbon layer is 50±5nm; and the thickness of the passivation layer is 200±20nm.
8. The MEMS infrared light source according to claim 1, It is characterized in that The coiled tungsten structure is composed of a plurality of embedded circular rings with an outer diameter of 1.3 mm connected in series, the heating wires are spaced 5 um apart, and the distance between the heater edge and the silicon substrate is 315 um; the coiled tungsten structure is annealed under nitrogen protection.
9. A method for preparing a MEMS infrared light source, It is characterized in that The preparation method comprises the following steps: (1) Thermal oxidation on a single crystal silicon substrate; (2) Low-pressure vapor deposition growth of silicon-rich Si 3 N 4 film; (3) In silicon-rich Si 3 N 4 The film forms a coiled-wire tungsten structure; (4) depositing a silicon oxide layer in the tungsten coil structure; (5) Deposition of adhesion layer; (6) depositing a nano-amorphous carbon layer; (7) evaporating a metal electrode on the coiled tungsten structure; (8) depositing a passivation layer on the nano-amorphous carbon layer; (9) Etch the back side to release the back cavity.
10. The method for preparing the MEMS infrared light source according to claim 9, It is characterized in that The thermal oxidation in step (1) is carried out by introducing dry oxygen gas and wet oxygen gas to oxidize the surface of the substrate, and the thickness of the obtained silicon oxide layer is 1500±30nm; The reaction gas pressure of the low-pressure vapor deposition in step (2) is 250 mTorr, and the obtained silicon-rich Si 3 N 4 The thickness of the film is 1000 ± 30 nm; The coiled tungsten structure in step (3) is formed by an unbalanced magnetron sputtering equipment system and a metal lift-off process. The coiled tungsten structure is formed by a plurality of embedded circular rings with an outer diameter of 1.3 mm in series. The heating wires are spaced 5 μm apart, and the distance between the edge of the heater and the silicon substrate is 315 μm. The process conditions during sputtering are as follows: the vacuum chamber is evacuated to at least 4×10 -3 Pa, then argon gas was introduced at 20 sccm to maintain the vacuum degree at 1 mTorr, the sputtering power was 1200 W, and the sample stage was sputtered at a negative bias voltage of 300 V for 5 min, and the rotation speed of the sample stage was kept at 5 rpm, and then sputtered at a negative bias voltage of 60 V for 20 min; the thickness of the obtained tungsten filament structure was 300 ± 30 nm; the obtained tungsten filament structure was annealed at 800 ° C for 1 hour under nitrogen protection; The thickness of the silicon oxide layer in step (4) is 300±10 nm; In the step (5), an unbalanced magnetron sputtering device system is used to deposit the Ti / TiN adhesion layer. Before the deposition, the vacuum chamber is evacuated to at least 4x10 -3 Pa, then argon was introduced, the vacuum was maintained at 0.2Pa, and bombarded for 30min under a negative bias of 500V, and then a layer of pure Ti film was deposited under a negative bias of 200V, the deposition time was 1min, and the current was 0.8A; then the pressure remained unchanged, and a gas with a ratio of argon to nitrogen of 2:3 was introduced, the power was 100W, and the deposition time was 4min; the thickness of the obtained adhesion layer was 20±2nm; In the step (6), an unbalanced magnetron sputtering device system is used to deposit the aC diamond-like amorphous carbon layer. Before the deposition, the vacuum chamber is evacuated to at least 4x10 -3 Pa, then argon was introduced, the vacuum degree was maintained at 0.67 Pa, the sputtering power was 150 W, the pre-sputtering was 5 min, and the deposition time was 70 min; the thickness of the obtained nano amorphous carbon layer was 50 ± 5 nm; In the step (7), the metal electrodes are Ni and Au electrodes respectively; The thickness of the passivation layer in step (8) is 200±20nm.