A method for preparing electromagnetic shielding grid and electromagnetic shielding film
By coating photoresist on transparent substrates, forming patterns, evaporate metal layers and removing photoresist, combined with pulse plating technology, the problems of poor pattern effect and poor conductivity of electromagnetic shielding materials are solved, and the more Good shielding effect.
Patent Information
- Application Number
- CN202111146692.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-09-28
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2041-09-28
AI Technical Summary
The existing electromagnetic shielding materials have poor pattern effect and poor conductivity, which cannot meet the shielding needs of electronic equipment.
The photoresist is coated on the transparent substrate, the pattern is formed by exposure and development, the metal layer is evaporated, and the photoresist is soaked in the N-methylpyrrolidone solution to remove the photoresist, the metal layer is retained, and finally the Au layer is added by pulse plating. Form an electromagnetic shielding grid.
It improves pattern effect and conductivity, and meets the shielding needs of electronic devices.
Smart Images

Figure CN113811172B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electromagnetic shielding, and specifically relates to a method for preparing an electromagnetic shielding grid and an electromagnetic shielding film. Background Art
[0002] With the rapid development of electronic communications and electrical control, mutual interference between electromagnetic signals has increasingly become a key issue threatening the normal operation of electronic equipment. Correspondingly, the pursuit of efficient electromagnetic shielding materials has become more urgent.
[0003] The earliest electromagnetic shielding materials were mainly bulk metals, which used the high conductivity of bulk metals to prevent the entry of electromagnetic waves. Although bulk metals have good shielding effects on electromagnetic waves, they are heavy and opaque, and cannot meet the development requirements of miniaturization, lightweight and transparency of electronic equipment.
[0004] Today's electromagnetic shielding materials are prepared by sequentially placing a photoresist, a conductive layer, etc. on a transparent substrate to achieve the development requirements of miniaturization, lightness, and transparency of electronic equipment, wherein a pattern is formed on the surface of the photoresist through exposure and development.
[0005] Although current electromagnetic shielding materials have solved the problems of miniaturization, lightness and transparency of electronic equipment, the patterns they form have poor effects and poor electrical conductivity. Summary of the invention
[0006] The technical problem to be solved by the present invention is how to provide a method for preparing an electromagnetic shielding grid to solve the problem that the existing electromagnetic shielding materials have poor pattern effects and poor electrical conductivity.
[0007] In order to solve the above technical problems, the present invention provides a method for preparing an electromagnetic shielding grid, comprising the steps of:
[0008] Coating a photoresist on a surface of one side of the transparent substrate;
[0009] Forming a pattern on the surface of the photoresist by exposure and development;
[0010] After forming the pattern, a metal layer is evaporated on the surface of the photoresist;
[0011] Immersing the transparent substrate after evaporating the metal layer in an N-methylpyrrolidone solution to remove the metal layer on the surface of the photoresist and retain the metal layer on the pattern surface, thereby obtaining a prefabricated electromagnetic shielding grid;
[0012] Au is electrodeposited on the surface of the prefabricated electromagnetic shielding grid by pulse electroplating, thereby obtaining the electromagnetic shielding grid.
[0013] Furthermore, the thickness of the photoresist is 2.8-3.2 microns.
[0014] Furthermore, the pattern is a uniformly distributed circular ring structure, and the transparent substrate is one of glass, transparent silica gel and transparent rubber.
[0015] Furthermore, the specific steps of evaporating a metal layer on the surface of the photoresist after forming the pattern include: first evaporating a 0.8-1.2 nanometer Cr adhesion layer on the surface of the photoresist after forming the pattern, and then evaporating a 9.8-10.2 nanometer Au conductive layer on the surface of the Cr adhesion layer.
[0016] Furthermore, the transparent substrate is roughened before being coated with the photoresist.
[0017] Furthermore, the specific steps of the roughening treatment include: firstly setting inwardly concave grooves at intervals on the surface of the transparent substrate where the photoresist needs to be coated, and then filling the grooves with transparent glue, so that the surface of the transparent substrate after filling with the transparent glue is a flat surface.
[0018] Furthermore, it is characterized in that the depth of the groove is one third to one half of the thickness of the transparent substrate.
[0019] Furthermore, the specific steps of the roughening treatment include: firstly setting outwardly protruding portions at intervals on the surface of the transparent substrate where the photoresist needs to be coated, and then filling transparent glue between the protrusions, so that the surface of the transparent substrate after filling with the transparent glue is a flat surface.
[0020] Furthermore, the step of evaporating the metal layer further comprises the following steps:
[0021] Soaking the transparent substrate after forming the pattern in a soluble salt solution at a temperature of 50-70° C. for 8-15 minutes;
[0022] Then, the transparent substrate soaked in the soluble salt solution is soaked in a solution with a copper ion concentration of 0.05-0.12 mol / L at a temperature of 40-60 degrees Celsius for 8-15 minutes.
[0023] The present invention also provides an electromagnetic shielding mesh, which is prepared by the above-mentioned method for preparing the electromagnetic shielding mesh.
[0024] Compared with the prior art, the preparation method of the electromagnetic shielding grid in the present invention includes the following steps: coating a photoresist on the surface of one side of a transparent substrate; forming a pattern on the surface of the photoresist by exposure and development; evaporating a metal layer on the surface of the photoresist after the pattern is formed; immersing the transparent substrate after the metal layer is evaporated in an N-methylpyrrolidone solution to remove the metal layer on the surface of the photoresist and retain the metal layer on the surface of the pattern, thereby obtaining a prefabricated electromagnetic shielding grid; and finally, electrodepositing Au on the surface of the prefabricated electromagnetic shielding grid by pulse electroplating, thereby obtaining an electromagnetic shielding grid. In this way, the effect of the formed pattern can be better, and the overall conductive performance can be improved to better meet the shielding requirements of electronic equipment. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to make the content of the present invention clearer, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative work, among which:
[0026] Figure 1 A schematic diagram of the process steps of a method for preparing an electromagnetic shielding grid provided in an embodiment of the present invention.
[0027] Figure 2 A schematic structural diagram of a transparent substrate after a first roughening treatment in a method for preparing an electromagnetic shielding grid provided in an embodiment of the present invention.
[0028] Figure 3 A schematic structural diagram of a transparent substrate after a second roughening treatment in a method for preparing an electromagnetic shielding grid provided in an embodiment of the present invention.
[0029] Among them, 1. transparent substrate; 2. groove; 3. protrusion; 4. transparent glue. DETAILED DESCRIPTION
[0030] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] Embodiment 1
[0032] The embodiment of the present invention provides a method for preparing an electromagnetic shielding grid. Figure 1 To Attachment Figure 3As shown, the following steps are included:
[0033] S101 , coating a photoresist on the surface of one side of the transparent substrate 1 .
[0034] Specifically, the transparent substrate 1 can be one of glass, transparent silica gel and transparent rubber. Of course, other types of transparent substrates 1 can also be selected according to actual needs.
[0035] Specifically, the transparent substrate 1 may be cleaned with acetone, ethanol, deionized water, potassium permanganate, etc. before use to ensure the cleanliness of the transparent substrate 1.
[0036] Specifically, the transparent substrate 1 is subjected to a roughening treatment before being coated with the photoresist, and there are two ways of the roughening treatment.
[0037] One method comprises the following steps: firstly, inwardly concave grooves 2 are arranged at intervals on the surface of the transparent substrate 1 where the photoresist is to be coated, and then transparent glue 4 is filled in the grooves 2, so that the surface of the transparent substrate 1 is flat after being filled with the transparent glue 4. When the transparent glue 4 solidifies, the photoresist can be coated.
[0038] On the one hand, this roughening treatment method can reduce the rigidity of the transparent substrate 1 by setting the groove 2 to increase its flexibility. On the other hand, it can increase the toughness of the groove 2 by setting the transparent glue 4, and play a certain buffering role to avoid damage to the transparent substrate 1. Since the transparent glue 4 itself has a certain flexibility, it will not destroy the flexibility of the transparent substrate 1 increased by the groove 2. At the same time, the transparent glue 4 can also increase the viscosity between the photoresist and the transparent substrate 1.
[0039] The depth of the groove 2 is one third to one half of the thickness of the transparent substrate 1, so as to avoid the groove 2 being too deep to damage the structural strength of the transparent substrate 1, and to avoid the groove 2 being too shallow to achieve the effect of increasing the flexibility of the transparent substrate 1.
[0040] Another method includes the steps of firstly arranging outwardly protruding portions 3 at intervals on the surface of the transparent substrate 1 to be coated with the photoresist, and then filling transparent glue 4 between the protruding portions 3, so that the surface of the transparent substrate 1 is flat after being filled with the transparent glue 4. When the transparent glue 4 solidifies, the photoresist can be coated.
[0041] On the one hand, this roughening treatment method can increase the rigidity of the transparent substrate 1 by setting the protrusion 3 to increase its structural strength. On the other hand, it can increase its flexibility by setting the transparent glue 4 and play a certain buffering role to avoid damage to the transparent substrate 1. Since the transparent glue 4 itself has a certain toughness, it will not make the transparent substrate 1 too soft. At the same time, the transparent glue 4 can also increase the viscosity between the photoresist and the transparent substrate 1.
[0042] The height of the protrusion 3 is less than half of the thickness of the transparent substrate 1 , so that the protrusion 3 is not too high and affects the use of the transparent substrate 1 .
[0043] Specifically, the photoresist is applied by spin coating, and the positions where the photoresist is dropped are spaced 3-5 cm apart from each other on the transparent substrate 1 during spin coating, so that the photoresist can be more evenly coated on the surface of the transparent substrate 1. Of course, according to actual needs, the positions where the photoresist is dropped can be spaced closer or farther apart on the transparent substrate 1.
[0044] Specifically, the thickness of the photoresist is 2.8-3.2 microns, and in this embodiment, the thickness of the photoresist is 3 microns. Of course, the thickness of the photoresist can also be adjusted according to actual needs.
[0045] S102, forming a pattern on the surface of the photoresist by exposure and development.
[0046] Specifically, the exposure is performed using a contact ultraviolet lithography machine.
[0047] Specifically, the pattern is a uniformly distributed circular ring structure. Of course, according to actual needs, the pattern can also be set to other structures, such as a square ring structure, a strip structure, an elliptical ring structure, etc., which are not listed one by one here.
[0048] S103, evaporating a metal layer on the surface of the photoresist after the pattern is formed.
[0049] Specifically, after step S102 and before step S103, a further step may be added: soaking the transparent substrate 1 after forming the pattern in a soluble salt solution at a temperature of 50-70°C for 8-15 minutes; and then soaking the transparent substrate 1 after soaking in the soluble salt solution in a solution with a copper ion concentration of 0.05-0.12 mol / L at a temperature of 40-60°C for 8-15 minutes. In this way, the evaporated metal layer and the electrodeposited Cu in step S105 can be more uniform and the adhesion effect can be improved.
[0050] Of course, the temperature and time of the above two soakings can also be adjusted according to actual needs.
[0051] The soluble salt solution includes one or more of a soluble ammonium salt solution, a soluble thiocyanate solution, a soluble thiosulfate solution, a soluble sulfite solution, a soluble ethylenediaminetetraacetic acid disalt solution and a soluble citrate solution.
[0052] Specifically, the specific steps of evaporating the metal layer include: first evaporating a 0.8-1.2 nanometer Cr adhesion layer on the surface of the photoresist after the pattern is formed, and then evaporating a 9.8-10.2 nanometer Au conductive layer on the surface of the Cr adhesion layer. This can increase the conductivity in the structural area.
[0053] Of course, the evaporated metal layer is evaporated on the surface of the photoresist after the above two immersions.
[0054] Specifically, the thickness of the Cr adhesion layer and the Au conductive layer is controlled by adjusting the pulse plating current and the plating time.
[0055] S104, immersing the transparent substrate 1 after the metal layer is evaporated in an N-methylpyrrolidone solution, thereby obtaining a prefabricated electromagnetic shielding grid.
[0056] The soaking time is set according to actual needs. For example, the concentration of N-methylpyrrolidone in the N-methylpyrrolidone solution, the temperature and other conditions are factors that affect the soaking time.
[0057] Specifically, the transparent substrate 1 after the metal layer is evaporated is immersed in an N-methylpyrrolidone solution to remove the metal layer on the surface of the photoresist and retain the metal layer on the pattern surface to enhance the display effect of the pattern and prevent the pattern from being affected by subsequent steps.
[0058] S105 , electrodepositing Au on the surface of the prefabricated electromagnetic shielding grid by pulse electroplating, thereby obtaining an electromagnetic shielding grid.
[0059] The thickness of the electrodeposited Au is set according to actual needs and will not be described here.
[0060] Specifically, Au is electro-deposited on the surface of the prefabricated electromagnetic shielding grid where the pattern is formed.
[0061] Specifically, Au is electrodeposited on the surface of the prefabricated electromagnetic shielding grid by pulse electroplating, thereby further improving the conductive performance of the electromagnetic shielding grid.
[0062] The preparation method of the electromagnetic shielding grid in this embodiment includes the following steps: coating a photoresist on the surface of one side of a transparent substrate 1; forming a pattern on the surface of the photoresist by exposure and development; evaporating a metal layer on the surface of the photoresist after the pattern is formed; immersing the transparent substrate 1 after the metal layer is evaporated in an N-methylpyrrolidone solution to remove the metal layer on the surface of the photoresist and retain the metal layer on the surface of the pattern, thereby obtaining a prefabricated electromagnetic shielding grid; and finally, electrodepositing Au on the surface of the prefabricated electromagnetic shielding grid by pulse electroplating, thereby obtaining an electromagnetic shielding grid. This can make the effect of the formed pattern better and improve the overall conductive performance to better meet the shielding requirements of electronic equipment.
[0063] Specifically, according to actual needs, a layer of transparent glue may be coated on the surface edge of the electromagnetic shielding grid to facilitate pasting.
[0064] Specifically, according to actual needs, a layer of transparent glue may be coated on the periphery of the electromagnetic shielding grid to protect the periphery of the electromagnetic shielding grid and prevent the edge from detaching.
[0065] Embodiment 2
[0066] This embodiment provides an electromagnetic shielding mesh, which is prepared by the method for preparing the electromagnetic shielding mesh of the first embodiment.
[0067] The electromagnetic shielding film in this embodiment is prepared by the preparation method of the electromagnetic shielding grid in the first embodiment, so that the effect of the formed pattern can be better and the overall conductive performance can be improved to better meet the shielding requirements of electronic equipment.
[0068] The above embodiments are only examples for clearly explaining the present invention and are not intended to limit the implementation methods. The scope of the present invention includes but is not limited to the above embodiments, and any equivalent changes made to the shape and structure of the present invention are included in the protection scope of the present invention.
Claims
1. A method for preparing an electromagnetic shielding grid, It is characterized in that Includes steps: Coating a photoresist on a surface of one side of a transparent substrate; the transparent substrate is roughened before coating the photoresist; The specific steps of the roughening treatment include: firstly, setting inwardly concave grooves at intervals on the surface of the transparent substrate where the photoresist is to be coated, and then filling the grooves with transparent glue, so that the surface of the transparent substrate after the transparent glue is filled is a flat surface; or, firstly, setting outwardly protruding portions at intervals on the surface of the transparent substrate where the photoresist is to be coated, and then filling transparent glue between the protruding portions, so that the surface of the transparent substrate after the transparent glue is filled is a flat surface; Forming a pattern on the surface of the photoresist by exposure and development; After forming the pattern, a metal layer is evaporated on the surface of the photoresist; Immersing the transparent substrate after evaporating the metal layer in an N-methylpyrrolidone solution to remove the metal layer on the surface of the photoresist and retain the metal layer on the pattern surface, thereby obtaining a prefabricated electromagnetic shielding grid; Au is electrodeposited on the surface of the prefabricated electromagnetic shielding grid by pulse electroplating, thereby obtaining the electromagnetic shielding grid.
2. The method for preparing the electromagnetic shielding grid according to claim 1, It is characterized in that The thickness of the photoresist is 2.8-3.2 microns.
3. The method for preparing the electromagnetic shielding grid according to claim 1, It is characterized in that The pattern is a uniformly distributed circular ring structure, and the transparent substrate is one of glass, transparent silica gel and transparent rubber.
4. The method for preparing the electromagnetic shielding grid according to claim 1, It is characterized in that The specific step of evaporating a metal layer on the surface of the photoresist after forming the pattern includes: first evaporating a 0.8-1.2 nanometer Cr adhesion layer on the surface of the photoresist after forming the pattern, and then evaporating a 9.8-10.2 nanometer Au conductive layer on the surface of the Cr adhesion layer.
5. The method for preparing the electromagnetic shielding grid according to claim 1, It is characterized in that The depth of the groove is one third to one half of the thickness of the transparent substrate.
6. The method for preparing the electromagnetic shielding grid according to claim 1, It is characterized in that The step of evaporating the metal layer also includes: Soaking the transparent substrate after forming the pattern in a soluble salt solution at a temperature of 50-70° C. for 8-15 minutes; Then, the transparent substrate after being immersed in the soluble salt solution is immersed in a solution with a copper ion concentration of 0.05-0.12 mol / L, the immersion temperature is 40-60 degrees Celsius, and the time is 8-15 minutes.
7. An electromagnetic shielding film, It is characterized in that The electromagnetic shielding film is prepared by the method for preparing the electromagnetic shielding mesh according to any one of claims 1 to 6 and obtained by treatment.