UV-curable high-fluorine-content anti-fingerprint resin and its preparation method and application

By UV curing anti-fingerprint resin with high fluorine content, combined with spin coating and UV curing technology, it solves the problems of VOC emissions and high energy consumption of spray-type anti-fingerprint coating liquids, and achieves low surface tension, strong hydrophobic coating and Efficient production.

CN113817138BActive Publication Date: 2024-10-01CHANGSHA SONGRUN NEW MATERIAL CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202111005820.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-08-30
Publication Date
2024-10-01
Estimated Expiration
2041-08-30

AI Technical Summary

Technical Problem

The existing spray-type anti-fingerprint coating solution emits large amounts of VOC, pollutes the environment and affects the health of construction workers, and the heat curing method consumes high energy and affects production efficiency.

Method used

Using UV-cured anti-fingerprint resin with high fluorine content, through a combination of fluorinated epoxy resin, perfluorocarboxylic acid, fluorinated anhydride and (meth)acrylic glycidyl ether, combined with spin coating and UV curing technology , forming a low surface tension, strong hydrophobic coating.

Benefits of technology

It significantly reduces VOC emissions, improves production efficiency, forms an anti-fingerprint coating with lower surface tension and better hydrophobicity, enhances anti-fingerprint ability, and meets environmental protection and health standards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003237190660000061
    Figure BDA0003237190660000061
  • Figure BDA0003237190660000071
    Figure BDA0003237190660000071
  • Figure BDA0003237190660000081
    Figure BDA0003237190660000081
Patent Text Reader

Abstract

The invention discloses a UV-curable anti-fingerprint resin with a high fluorine content, which comprises the following components by weight: 20 to 60 parts of fluorinated epoxy resin, 10 to 50 parts of perfluorocarboxylic acid, 5 to 30 parts of fluorinated anhydride, 8 to 35 parts of (methyl) acrylic acid glycidyl ether, 0.05 to 0.5 parts of quaternary ammonium (phosphonium) salt, and 0.05 to 0.2 parts of inhibitor. The UV-curable anti-fingerprint resin with a high fluorine content of the invention contains both UV-curable acryloxy groups and a large number of highly hydrophobic fluorocarbon groups. By adopting a rotary coating method and coordinating with UV curing, the problem that the spray-type AF liquid commonly used in the market adopts a thermal curing method, which has high energy consumption, large VOC emissions, environmental pollution, and affects the health of employees is solved. At the same time, the production efficiency is significantly improved by using UV curing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of anti-fingerprint, in particular, to a UV-curable anti-fingerprint resin with a high fluorine content. In addition, the present invention also relates to a preparation method and application of the UV-curable anti-fingerprint resin with a high fluorine content. Background Art

[0002] Anti-fingerprint coating (AFC) refers to a very thin layer of coating with very low surface energy that is applied to the surface of ceramics, glass and other materials by evaporation or spraying, so that the surface of the product is not easily left with traces of water stains, grease, dust and the like after being touched by hands, or even if stains are left, they can be easily wiped off. Anti-fingerprint coatings are mainly used in the electronics industry. With the rapid development of the global electronics industry, the anti-fingerprint coating industry has also developed rapidly. Anti-fingerprint coatings are mainly used in the screens of modern electronic products. In recent years, the electronics industry has been on a growth trend, so the demand for anti-fingerprint coatings has shown a steady growth trend. In terms of production, there are currently no leading companies in the anti-fingerprint coating market, the market concentration is low, the industry lacks standards, and the industry development is relatively chaotic.

[0003] There are many anti-fingerprint coating preparation technologies, which can be divided into two categories: dry method and wet method. The dry method mainly includes vacuum evaporation, vacuum sputtering, and chemical vapor deposition, and the wet method mainly includes AF spraying. AF spraying uses high pressure to evenly spray AF solution on the surface of the substrate to form a thin film. The cost is relatively low and the operation is simple, so it is more popular in the market. However, the spray-type AF solution has high VOC emissions, which affects the environment and the health of employees. Summary of the invention

[0004] The invention provides a UV-curable anti-fingerprint resin with high fluorine content and a preparation method and application thereof, so as to solve the technical problems that the spray-type AF solution commonly used on the market has large VOC emissions, pollutes the environment, and affects the health of construction workers.

[0005] The technical solution adopted by the present invention is as follows:

[0006] A UV-curable anti-fingerprint resin with a high fluorine content comprises the following components in parts by weight: 20 to 60 parts of fluorinated epoxy resin, 10 to 50 parts of perfluorocarboxylic acid, 5 to 30 parts of fluorinated acid anhydride, 8 to 35 parts of (meth) acrylic acid glycidyl ether, 0.05 to 0.5 parts of quaternary ammonium (phosphonium) salt, and 0.05 to 0.2 parts of an inhibitor.

[0007] Furthermore, the fluorinated epoxy resin is 25 to 56 parts, the perfluorocarboxylic acid is 12 to 48 parts, the fluorinated acid anhydride is 8 to 29 parts, the (meth) acrylic acid glycidyl ether is 11 to 30 parts, the quaternary ammonium (phosphonium) salt is 0.08 to 0.4 parts, and the inhibitor is 0.08 to 0.15 parts.

[0008] Furthermore, the epoxy value of the fluorinated epoxy resin is 0.20 to 0.60, and includes one or more of perfluorobisphenol A diglycidyl ether, 1,3-bis(3-glycidyl tetrafluorophenoxy)-2-hydroxypropane, 1,4-bis(hydroxyhexafluoroisopropyl)benzene diglycidyl ether, 1,3-bis(hydroxyhexafluoroisopropyl)benzene diglycidyl ether, 1,3-bis(hydroxyhexafluoroisopropyl)-5-perfluoropropylbenzene diglycidyl ether, 1,4-bis(hydroxyhexafluoroisopropyl)tetrafluorobenzene diglycidyl ether, 4,4′-dihydroxyoctafluorobiphenyl diglycidyl ether, and 4,4′-bis(hydroxyhexafluoroisopropyl)octafluorobiphenyl diglycidyl ether.

[0009] Furthermore, the perfluorocarboxylic acid includes one or more of trifluoroacetic acid, perfluoropropionic acid, perfluorobutyric acid, perfluoropentanoic acid, perfluorohexanoic acid, perfluoroheptanoic acid, perfluorooctanoic acid, perfluorononanoic acid, perfluorodecanoic acid, perfluoroundecanoic acid, perfluorododecanoic acid, perfluorotridecanoic acid, and perfluorotetradecanoic acid.

[0010] Further, the fluorinated acid anhydride includes: one or more of monofluorobenzoic anhydride, difluorobenzoic anhydride, tetrafluorobenzoic anhydride, and difluoromaleic anhydride; and / or, the (meth)acrylic glycidyl ether includes: one or more of acrylic acid glycidyl ether, methacrylic acid glycidyl ether, hydroxyethyl acrylate glycidyl ether, hydroxyethyl methacrylate glycidyl ether, hydroxypropyl acrylate glycidyl ether, and hydroxypropyl methacrylate glycidyl ether.

[0011] Further, the quaternary ammonium (phosphonium) salt includes: one or more of benzyltrimethylammonium chloride, benzyltriethylammonium chloride, benzyltrimethylammonium bromide, benzyltriethylammonium bromide, pyridine hydrochloride and butyltriphenylphosphonium chloride, benzyltriphenylphosphonium chloride, benzyltriphenylphosphonium bromide; and / or, the inhibitor includes: p-tert-butylcatechol, p-hydroxyanisole, 2,6-di-tert-butyl-p-cresol, tris(N-nitroso-N-phenylhydroxylamine)aluminum.

[0012] According to another aspect of the present invention, there is also provided a method for preparing the above-mentioned UV-curable high-fluorine-content anti-fingerprint resin, comprising the following steps:

[0013] S1, mixing the fluorinated epoxy resin, the perfluorocarboxylic acid and part of the quaternary ammonium (phosphonium) salt uniformly, heating to react, measuring the acid value until the acid value is less than or equal to 20, then heating to react until the acid value is less than or equal to 0.5, cooling to obtain a mixture A;

[0014] S2, adding fluorinated anhydride to mixture A, controlling the temperature to react, measuring the acid value until the acid value is 70-120, adding part of the polymerization inhibitor and stirring evenly to obtain mixture B;

[0015] S3, the remaining polymerization inhibitor, the remaining quaternary ammonium (phosphonium) salt and the (meth) acrylic acid glycidyl ether are mixed uniformly to obtain a mixture C, the mixture C is slowly added dropwise to the mixture B, the temperature is controlled to react, the acid value is measured until the acid value is less than or equal to 0.5, and the temperature is lowered to obtain a UV-curable anti-fingerprint resin with a high fluorine content.

[0016] Further, in step S1, the heating temperature is 80°C to 90°C, the heating reaction time is greater than or equal to 4 hours, the temperature is raised to 100°C to 130°C for reaction, and the temperature is lowered to 80°C to 95°C; and / or, in step S2, the temperature is controlled to 80°C to 97°C, and the reaction time is greater than or equal to 4 hours; and / or, in step S3, the mixture C is slowly added dropwise within 4 hours, the temperature is controlled to 95°C to 97°C, the heating reaction time is greater than or equal to 12 hours, and the temperature is lowered to 25°C to 30°C.

[0017] According to another aspect of the present invention, there is also provided a use of the UV-curable high-fluorine-content anti-fingerprint resin in a UV anti-fingerprint liquid.

[0018] Furthermore, the UV anti-fingerprint liquid comprises the following components in parts by weight: 50-60 parts of UV-curable high-fluorine anti-fingerprint resin, 15-30 parts of fluorinated (meth)acrylate monomer, 1-5 parts of multifunctional acrylate, 3-7 parts of photoinitiator, 5-10 parts of (meth)acryloxysilane coupling agent, and 5-10 parts of solvent.

[0019] Further, the fluorinated (meth)acrylate monomer includes one or more of hexafluorobutyl acrylate, dodecafluoroheptyl methacrylate, octafluoro-1,6-hexanediol diacrylate, and heptadecafluorodecyl acrylate; the multifunctional acrylate includes 10-15-functional hyperbranched polyester acrylate or pentaerythritol hexaacrylate; the photoinitiator includes 2-hydroxy-2-methyl-1-phenyl-1-propanone or diphenyl-(2,4,6-trimethylbenzoyl)phosphine oxide (L); and the (meth)acryloxysilane coupling agent includes methacryloxytrimethoxysilane or acryloxytrimethoxysilane.

[0020] Furthermore, the UV anti-fingerprint liquid is spin-coated on the surface of the glass substrate and cured by UV to obtain an anti-fingerprint coating.

[0021] The present invention has the following beneficial effects:

[0022] The UV-curable high-fluorine-content anti-fingerprint resin of the present invention contains both UV-curable acryloxy groups and a large number of highly hydrophobic fluorocarbon groups. By adopting a rotary coating method and coordinating with UV curing, the problem of the spray-type AF solution currently commonly used in the market using a thermal curing method with high energy consumption, large VOC emissions, environmental pollution, and affecting the health of employees is solved. At the same time, the production efficiency is significantly improved by using UV curing. The above-mentioned UV-curable high-fluorine-content anti-fingerprint resin has a high fluorine content, which can reach more than 22%, and the resulting coating has lower surface tension, better hydrophobicity, and stronger anti-fingerprint ability.

[0023] In addition to the above-described objects, features and advantages, the present invention has other objects, features and advantages. The present invention is further described in detail. DETAILED DESCRIPTION

[0024] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.

[0025] A preferred embodiment of the present invention provides a UV-curable anti-fingerprint resin with a high fluorine content, which comprises the following components in parts by weight: 20 to 60 parts of fluorinated epoxy resin, 10 to 50 parts of perfluorocarboxylic acid, 5 to 30 parts of fluorinated acid anhydride, 8 to 35 parts of (meth) acrylic acid glycidyl ether, 0.05 to 0.5 parts of quaternary ammonium (phosphonium) salt, and 0.05 to 0.2 parts of inhibitor.

[0026] The UV-curable high-fluorine anti-fingerprint resin of the present invention contains both UV-curable acryloxy groups and a large number of strongly hydrophobic fluorocarbon groups. By adopting a spin coating method and coordinating with UV curing, the problem that the spray-type AF solution commonly used in the market adopts a thermal curing method with high energy consumption, large VOC emissions, environmental pollution, and affecting the health of employees is solved. At the same time, the production efficiency is significantly improved by using UV curing.

[0027] The above-mentioned fluorinated epoxy resin contains a large number of carbon-fluorine bonds and epoxy groups. The carbon-fluorine bonds make the resin have good hydrophobicity and ultra-low surface tension, which makes it have excellent anti-fingerprint effect. The epoxy group provides better reactivity and can be grafted with other substances. The carbon-fluorine bonds on the perfluorocarboxylic acid structure can provide hydrophobic properties, wherein the carboxyl group can react with the epoxy group on the fluorinated epoxy resin, so that the epoxy group opens the ring to produce a hydroxyl group. Fluorinated anhydride can increase the hydrophobicity of UV-cured high-fluorine content anti-fingerprint resin, wherein the anhydride can react with the hydroxyl group to generate a carboxyl group. (Meth) acrylic acid glycidyl ether reacts with the carboxyl group generated by the fluorinated anhydride, and finally the acryloxy group is grafted onto the main resin (fluorinated epoxy resin), so that the main resin has UV curing properties.

[0028] The present invention adopts fluorinated epoxy resin and perfluorocarboxylic acid ring-opening grafting to significantly increase the fluorine content of fluorinated epoxy resin (main resin), so that the main resin has excellent surface hydrophobicity, extremely low surface tension, low surface friction coefficient and good wear resistance. Fluorinated acid anhydride is used to react with hydroxyl groups on the main resin to introduce carboxyl groups on the main resin, which can improve the hydrophobicity and wear resistance of the main resin compared with conventional fluorine-free acid anhydride. Then, the carboxyl group reacts with (meth) acrylic acid glycidyl ether, so that the synthesized main resin has both high fluorine content and UV curing properties.

[0029] Refer to the Ministry of Railways bridge protection coating standard TB / T1527-2004 and Japanese standards that stipulate a fluorine content standard of 15% or more for fluorocarbon paints, the HG / T3792 standard stipulates that the fluorine content of fluorocarbon paints is 18%, and the transportation industry standard JT / T695-2007 "Technical Conditions for Anticorrosion of Surface Coatings of Concrete Bridge Structures" stipulates that the fluorine content of fluorocarbon topcoats should be greater than or equal to 20%. The above-mentioned UV-cured high-fluorine anti-fingerprint resin has a high fluorine content, which can reach more than 22%, and the resulting coating has lower surface tension, better hydrophobicity, and stronger anti-fingerprint ability.

[0030] In this embodiment, the fluorinated epoxy resin is 25 to 56 parts, the perfluorocarboxylic acid is 12 to 48 parts, the fluorinated anhydride is 8 to 29 parts, the (meth) acrylic acid glycidyl ether is 11 to 30 parts, the quaternary ammonium (phosphonium) salt is 0.08 to 0.4 parts, and the polymerization inhibitor is 0.08 to 0.15 parts. Preferably, the fluorinated epoxy resin is 26 to 54 parts, the perfluorocarboxylic acid is 12 to 46 parts, the fluorinated anhydride is 9 to 28 parts, the (meth) acrylic acid glycidyl ether is 11 to 30 parts, the quaternary ammonium (phosphonium) salt is 0.1 to 0.3 parts, and the polymerization inhibitor is 0.08 to 0.15 parts.

[0031] In this embodiment, the epoxy value of the fluorinated epoxy resin is 0.20 to 0.60. The epoxy value of the fluorinated epoxy resin is lower than 0.2, so that the amount of perfluorocarboxylic acid connected is small, and the hydrophobicity and wear resistance of the resin are poor; the epoxy value of the fluorinated epoxy resin is higher than 0.6, the epoxy groups are close, the steric hindrance is large, and the perfluorocarboxylic acid, fluorinated anhydride, (meth) acrylic acid glycidyl ether are difficult to connect, which will lead to incomplete reaction of the epoxy group and affect the storage stability of the anti-fingerprint coating.

[0032] In this embodiment, the fluorinated epoxy resin includes: one or more of perfluorobisphenol A diglycidyl ether, 1,3-bis(3-glycidyl tetrafluorophenoxy)-2-hydroxypropane, 1,4-bis(hydroxyhexafluoroisopropyl)benzene diglycidyl ether, 1,3-bis(hydroxyhexafluoroisopropyl)benzene diglycidyl ether, 1,3-bis(hydroxyhexafluoroisopropyl)-5-perfluoropropylbenzene diglycidyl ether, 1,4-bis(hydroxyhexafluoroisopropyl)tetrafluorobenzene diglycidyl ether, 4,4′-dihydroxyoctafluorobiphenyl diglycidyl ether, and 4,4′-bis(hydroxyhexafluoroisopropyl)octafluorobiphenyl diglycidyl ether. Preferably, the fluorinated epoxy resin includes: one or more of 1,3-bis(3-glycidyltetrafluorophenoxy)-2-hydroxypropane, 1,3-bis(hydroxyhexafluoroisopropyl)-5-perfluoropropylbenzene diglycidyl ether, 1,4-bis(hydroxyhexafluoroisopropyl)tetrafluorobenzene diglycidyl ether, 4,4′-dihydroxyoctafluorobiphenyl diglycidyl ether, and 4,4′-bis(hydroxyhexafluoroisopropyl)octafluorobiphenyl diglycidyl ether.

[0033] In this embodiment, the perfluorocarboxylic acid includes one or more of trifluoroacetic acid, perfluoropropionic acid, perfluorobutyric acid, perfluoropentanoic acid, perfluorohexanoic acid, perfluoroheptanoic acid, perfluorooctanoic acid, perfluorononanoic acid, perfluorodecanoic acid, perfluoroundecanoic acid, perfluorododecanoic acid, perfluorotridecanoic acid, and perfluorotetradecanoic acid. Preferably, the perfluorocarboxylic acid includes one or more of trifluoroacetic acid, perfluoropropionic acid, perfluorobutyric acid, perfluoropentanoic acid, perfluorohexanoic acid, and perfluoroheptanoic acid.

[0034] In this embodiment, the fluorinated acid anhydride includes one or more of monofluorobenzoic anhydride, difluorobenzoic anhydride, tetrafluorobenzoic anhydride, and difluoromaleic anhydride. Preferably, the fluorinated acid anhydride includes one or more of difluorobenzoic anhydride, tetrafluorobenzoic anhydride, and difluoromaleic anhydride.

[0035] In this embodiment, the (meth) acrylic acid glycidyl ether includes: one or more of acrylic acid glycidyl ether, methacrylic acid glycidyl ether, hydroxyethyl acrylate glycidyl ether, hydroxyethyl methacrylate glycidyl ether, hydroxypropyl acrylate glycidyl ether, and hydroxypropyl methacrylate glycidyl ether. Preferably, the (meth) acrylic acid glycidyl ether includes: one or more of acrylic acid glycidyl ether, hydroxyethyl acrylate glycidyl ether, and hydroxypropyl acrylate glycidyl ether.

[0036] In the present embodiment, the quaternary ammonium (phosphonium) salt includes: one or more of benzyltrimethylammonium chloride, benzyltriethylammonium chloride, benzyltrimethylammonium bromide, benzyltriethylammonium bromide, pyridine hydrochloride and butyltriphenylphosphonium chloride, benzyltriphenylphosphonium chloride, benzyltriphenylphosphonium bromide. Preferably, the quaternary ammonium (phosphonium) salt includes: benzyltriethylammonium chloride, benzyltriethylammonium bromide, pyridine hydrochloride and butyltriphenylphosphonium chloride, benzyltriphenylphosphonium chloride, benzyltriphenylphosphonium bromide. The quaternary ammonium (phosphonium) salt has a catalytic effect, increases the reaction rate, and reduces the reaction temperature.

[0037] In this embodiment, the polymerization inhibitor includes: p-tert-butylcatechol, p-hydroxyanisole, 2,6-di-tert-butyl-p-cresol, tris(N-nitroso-N-phenylhydroxylamine)aluminum. The carboxyl group generated by (methyl) acrylic acid glycidyl ether and fluorinated acid anhydride reacts to obtain acryloyloxy groups. The polymerization inhibitor effectively prevents the acryloyloxy groups from self-polymerization, and further promotes the grafting of acryloyloxy groups onto the main resin.

[0038] According to another aspect of the present invention, there is also provided a method for preparing the above-mentioned UV-curable high-fluorine-content anti-fingerprint resin, comprising the following steps:

[0039] S1, mixing the fluorinated epoxy resin, the perfluorocarboxylic acid and part of the quaternary ammonium (phosphonium) salt uniformly, heating to react, measuring the acid value until the acid value is less than or equal to 20, then heating to react until the acid value is less than or equal to 0.5, cooling to obtain a mixture A;

[0040] S2, adding fluorinated anhydride to mixture A, controlling the temperature to react, measuring the acid value until the acid value is 70-120, adding part of the polymerization inhibitor and stirring evenly to obtain mixture B;

[0041] S3, the remaining polymerization inhibitor, the remaining quaternary ammonium (phosphonium) salt and the (meth) acrylic acid glycidyl ether are mixed uniformly to obtain a mixture C, the mixture C is slowly added dropwise to the mixture B, the temperature is controlled to react, the acid value is measured until the acid value is less than or equal to 0.5, and the temperature is lowered to obtain a UV-curable anti-fingerprint resin with a high fluorine content.

[0042] In this embodiment, in step S1, the heating temperature is 80°C to 90°C, the heating reaction time is greater than or equal to 4 hours, the temperature is raised to 100°C to 130°C for reaction, and the temperature is lowered to 80°C to 95°C; and / or, in step S2, the temperature is controlled to 80°C to 97°C, and the reaction time is greater than or equal to 4 hours; and / or, in step S3, the mixture C is slowly added dropwise within 4 hours, the temperature is controlled to 95°C to 97°C, the heating reaction time is greater than or equal to 12 hours, and the temperature is lowered to 25°C to 30°C.

[0043] According to another aspect of the present invention, there is also provided a use of the UV-curable high-fluorine-content anti-fingerprint resin in UV anti-fingerprint liquid. The UV-curable high-fluorine-content anti-fingerprint resin is used to prepare UV anti-fingerprint liquid, and its high fluorine content makes the final coating have lower surface tension, easier to spin-coat on a substrate, and has higher adhesion, better hydrophobicity, and stronger anti-fingerprint ability.

[0044] In this embodiment, the UV anti-fingerprint liquid comprises the following components in parts by weight: 50-60 parts of UV-curable high-fluorine anti-fingerprint resin, 15-30 parts of fluorinated (meth)acrylate monomer, 1-5 parts of multifunctional acrylate, 3-7 parts of (meth)acryloxysilane coupling agent, 5-10 parts of (meth)acryloxysilane coupling agent, and 5-10 parts of solvent.

[0045] In this embodiment, the fluorinated (meth)acrylate monomer includes one or more of hexafluorobutyl acrylate, dodecafluoroheptyl methacrylate, octafluoro-1,6-hexanediol diacrylate, and heptadecafluorodecyl acrylate; the multifunctional acrylate includes 10-15-functional hyperbranched polyester acrylate or pentaerythritol hexaacrylate; the photoinitiator includes 2-hydroxy-2-methyl-1-phenyl-1-propanone or diphenyl-(2,4,6-trimethylbenzoyl)phosphine oxide (L); and the (meth)acryloxysilane coupling agent includes methacryloxytrimethoxysilane or acryloxytrimethoxysilane.

[0046] The preparation method of the above-mentioned UV anti-fingerprint liquid comprises: UV curing high fluorine content anti-fingerprint resin, fluorinated (meth) acrylate monomer, multifunctional acrylate, photoinitiator at a rotation speed of 500 to 1000 rpm, stirring evenly, adding solvent, stirring evenly, and then adding (meth) acryloyloxy silane coupling agent to disperse evenly to obtain UV anti-fingerprint liquid. The UV anti-fingerprint liquid is filtered through an 800 mesh screen, spin-coated on the surface of a glass substrate, and illuminated with a mixed LEDUV lamp at 365nm, 395nm and 405nm, with an intensity of 50 to 500mW / cm 2 , energy 300~1200mj / cm 2 UV curing.

[0047] In this embodiment, the UV anti-fingerprint liquid is spin-coated on the surface of the glass substrate and UV cured to obtain an anti-fingerprint coating. In the above embodiment, an anti-fingerprint coating is formed on the glass substrate by UV curing, with a light transmittance of more than 99%, an adhesion of 5B, water boiling resistance, high insulation performance, and better hydrophobicity.

[0048] Example

[0049] Example 1

[0050] The preparation method of UV-curable high-fluorine content anti-fingerprint resin comprises the following steps:

[0051] S1. Add 100 g of 1,3-bis(3-glycidyltetrafluorophenoxy)-2-hydroxypropane resin (epoxy value 0.40) into a four-necked bottle, stir with a glass stirrer, add 125.6 g of perfluorohexanoic acid, add 0.45 g of benzyltriethylammonium chloride, heat and control the temperature to react at 80°C, react for 4 hours, measure the acid value, and then measure the acid value every 2 hours. When the acid value is less than 20, heat to 120°C for reaction, until the acid value is less than 0.5, cool to 95°C, and obtain mixture A;

[0052] S2, add 88 g of tetrafluorophthalic anhydride, control the temperature at 95° C. to react for 4 h, measure the acid value until the acid value drops to 71, add 0.32 g of p-hydroxyanisole, stir and dissolve completely, and obtain a mixture B;

[0053] S3. Evenly mix 0.16 g of p-hydroxyanisole, 0.32 g of benzyltriethylammonium chloride and 56.8 g of glycidyl acrylate to obtain a mixture C. Slowly drop the mixture C into the mixture B within 4 h. Control the temperature at 95 ° C for 12 h. Measure the acid value until the acid value is less than or equal to 0.5. Cool the temperature to 25 ° C to obtain a UV-curable anti-fingerprint resin with a high fluorine content, referred to as anti-fingerprint resin A.

[0054] Application of UV-curable high-fluorine anti-fingerprint resin in UV anti-fingerprint liquid.

[0055] UV anti-fingerprint liquid, the weight proportions of each component are shown in Table 1.

[0056] Table 1 Weight percentage of each component of UV anti-fingerprint liquid

[0057]

[0058] Anti-fingerprint resin A, hexafluorobutyl methacrylate, 10-15-functional hyperbranched polyester acrylate, 2-hydroxy-2-methyl-1-phenyl-1-propanone and diphenyl-(2,4,6-trimethylbenzoyl)phosphine oxide (L) were stirred at a speed of 800 rpm, methanol was added, stirred evenly, and then methacryloxytrimethoxysilane was added and dispersed evenly to obtain a UV anti-fingerprint liquid.

[0059] The UV anti-fingerprint liquid was filtered through an 800-mesh screen and applied on the surface of the glass substrate by spin coating under a mixed LED UV lamp at 365nm, 395nm and 405nm with an intensity of 200mW / cm 2 , energy 500mj / cm 2 UV curing is performed to obtain an anti-fingerprint coating.

[0060] Example 2

[0061] The preparation method of UV-curable high-fluorine content anti-fingerprint resin comprises the following steps:

[0062] S1. Add 100 g of 1,3-bis(hydroxyhexafluoroisopropyl)-5-perfluoropropylbenzene diglycidyl ether resin (epoxy value 0.29) into a four-necked bottle, stir with a glass stirrer, add 62.06 g of perfluorobutyric acid, add 0.32 g of pyridine hydrochloride and butyltriphenylphosphonium chloride, heat and control the temperature to react at 85°C, react for 4 hours, measure the acid value, and then measure the acid value every 2 hours. When the acid value is less than 20, heat to 110°C for reaction, until the acid value is less than 0.5, cool to 95°C, and obtain mixture A;

[0063] S2, add 63.8 g of tetrafluorophthalic anhydride, control the temperature at 96° C. to react for 4 h, measure the acid value until the acid value drops to 73, add 0.23 g of p-hydroxyanisole, stir and dissolve completely, and obtain a mixture B;

[0064] S3. 0.12 g of p-hydroxyanisole, 0.23 g of pyridine hydrochloride, and 53.36 g of hydroxyethyl acrylate glycidyl ether were uniformly mixed to obtain a mixture C, and the mixture C was slowly added dropwise to the mixture B within 4 h. The temperature was controlled to react at 97 ° C for 12 h, and the acid value was measured until the acid value was less than or equal to 0.5. The temperature was lowered to 26 ° C to obtain a UV-curable anti-fingerprint resin with a high fluorine content, referred to as anti-fingerprint resin B.

[0065] Application of UV-curable high-fluorine anti-fingerprint resin in UV anti-fingerprint liquid.

[0066] UV anti-fingerprint liquid, the weight proportions of each component are shown in Table 2.

[0067] Table 2 Weight percentage of each component of UV anti-fingerprint liquid

[0068]

[0069] Anti-fingerprint resin B, dodecafluoroheptyl methacrylate, pentaerythritol hexaacrylate, 2-hydroxy-2-methyl-1-phenyl-1-propanone and diphenyl-(2,4,6-trimethylbenzoyl)phosphine oxide (L) were stirred at a rotation speed of 1000 rpm, isopropanol was added, stirred evenly, and then acryloxytrimethoxysilane was added and dispersed evenly to obtain a UV anti-fingerprint liquid.

[0070] The UV anti-fingerprint liquid was filtered through an 800-mesh screen and applied on the surface of the glass substrate by spin coating under a mixed LED UV lamp at 365nm, 395nm and 405nm with an intensity of 200mW / cm 2 , energy 500mj / cm 2 UV curing is performed to obtain an anti-fingerprint coating.

[0071] Example 3

[0072] The preparation method of UV-curable high-fluorine content anti-fingerprint resin comprises the following steps:

[0073] S1. Add 100 g of 4,4′-dihydroxyoctafluorobiphenyl diglycidyl ether resin (epoxy value 0.29) into a four-necked bottle, stir with a glass stirrer, add 46.74 g of trifluoroacetic acid, add 0.29 g of benzyltriphenylphosphonium chloride, heat and control the temperature to react at 88°C, react for 4 hours, measure the acid value, and then measure the acid value every 2 hours. When the acid value is less than 20, heat to 115°C for reaction, until the acid value is less than 0.5, cool to 80°C, and obtain mixture A;

[0074] S2, add 54.94 g of difluoromaleic anhydride, control the temperature at 82° C. to react for 6 h, measure the acid value until the acid value drops to 114, add 0.2 g of tris(N-nitroso-N-phenylhydroxylamine)aluminum, stir and dissolve completely, and obtain mixture B;

[0075] S3. Evenly mix 0.1 g of tri(N-nitroso-N-phenylhydroxylamine)aluminum, 0.2 g of benzyltriphenylphosphonium chloride, and 81.18 g of hydroxypropyl acrylate glycidyl ether to obtain a mixture C. Slowly drop the mixture C into the mixture B within 4 hours. Control the temperature at 97° C. to react for 16 hours. Measure the acid value until the acid value is less than or equal to 0.5. Cool the temperature to 25° C. to obtain a UV-curable anti-fingerprint resin with a high fluorine content, referred to as anti-fingerprint resin C.

[0076] Application of UV-curable high-fluorine anti-fingerprint resin in UV anti-fingerprint liquid.

[0077] UV anti-fingerprint liquid, the weight proportions of each component are shown in Table 3.

[0078] Table 3 Weight percentage of each component of UV anti-fingerprint liquid

[0079]

[0080] Anti-fingerprint resin C, octafluoro-1,6-hexanediol diacrylate, heptadecafluorodecyl acrylate, pentaerythritol hexaacrylate, 2-hydroxy-2-methyl-1-phenyl-1-propanone and diphenyl-(2,4,6-trimethylbenzoyl)phosphine oxide (L) were stirred at a speed of 900 rpm, ethanol was added, stirred evenly, and then methacryloxytrimethoxysilane was added and dispersed evenly to obtain a UV anti-fingerprint liquid.

[0081] The UV anti-fingerprint liquid was filtered through an 800-mesh screen and applied on the surface of the glass substrate by spin coating under a mixed LED UV lamp at 365nm, 395nm and 405nm with an intensity of 200mW / cm2 , energy 500mj / cm 2 UV curing is performed to obtain an anti-fingerprint coating.

[0082] Comparative Example 1

[0083] The anti-fingerprint liquid A of Japan's Daikin is sold on the market.

[0084] The fingerprint liquid A is sprayed on the surface of the glass substrate and heated and cured to obtain an anti-fingerprint coating.

[0085] Comparative Example 2

[0086] Anti-fingerprint liquid B from Asahi Glass of Japan is sold on the market.

[0087] The fingerprint liquid B is sprayed on the surface of the glass substrate and heated and cured to obtain an anti-fingerprint coating.

[0088] The anti-fingerprint coatings obtained in Examples 1, 2 and 3 and the anti-fingerprint coatings in Comparative Examples 1 and 2 were subjected to performance tests, specifically referring to the following indicators:

[0089] GB / T 9286-1998 Cross-cut test for paint and varnish films

[0090] GB / T 30693-2014 Measurement of contact angle between plastic film and water

[0091] GB / T 3048.5-2007 Electrical performance test methods for wires and cables Part 5: Insulation resistance test

[0092] QB / T 2702-2005 Test method for friction resistance of coated eyeglass lenses

[0093] GB5237-2008 boiling water test method

[0094] GB T 5433-1985 Determination of transmittance of daily-use glass

[0095] The test results are shown in Table 4.

[0096] Table 4 Performance test results

[0097]

[0098] It can be seen from Table 4 that the comprehensive performance of the anti-fingerprint coatings prepared in Examples 1 to 3 is the best. Compared with the results obtained by the commercially available anti-fingerprint liquids A and B in the comparative example, the UV anti-fingerprint liquid prepared by the present invention has better performance indicators.

[0099] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A UV-curable high-fluorine content anti-fingerprint resin, characterized in that: The composition includes the following components by weight: 20 to 60 parts of fluorinated epoxy resin, 10 to 50 parts of perfluorocarboxylic acid, 5 to 30 parts of fluorinated acid anhydride, 8 to 35 parts of (meth) acrylic acid glycidyl ether, 0.05 to 0.5 parts of quaternary ammonium salt or quaternary phosphonium salt, 0.05 to 0.2 parts of polymerization inhibitor, The preparation method of the UV-curable high-fluorine-content anti-fingerprint resin comprises the following steps: S1, mixing the fluorinated epoxy resin, the perfluorocarboxylic acid and part of the quaternary ammonium salt or quaternary phosphonium salt uniformly, heating to react, measuring the acid value until the acid value is less than or equal to 20, then heating to react until the acid value is less than or equal to 0.5, cooling to obtain a mixture A; S2, adding fluorinated anhydride to mixture A, controlling the temperature to react, measuring the acid value until the acid value is 70-120, adding part of the polymerization inhibitor and stirring evenly to obtain mixture B; S3, the remaining polymerization inhibitor, the remaining quaternary ammonium salt or quaternary phosphonium salt and (meth) acrylic acid glycidyl ether are mixed uniformly to obtain a mixture C, the mixture C is slowly added dropwise to the mixture B, the temperature is controlled to react, the acid value is measured until the acid value is less than or equal to 0.5, and the temperature is lowered to obtain a UV-curable high-fluorine content anti-fingerprint resin.

2. The UV-curable high-fluorine anti-fingerprint resin according to claim 1, characterized in that: The fluorinated epoxy resin is 25 to 56 parts, the perfluorocarboxylic acid is 12 to 48 parts, the fluorinated acid anhydride is 8 to 29 parts, the (meth) acrylic acid glycidyl ether is 11 to 30 parts, the quaternary ammonium salt or quaternary phosphonium salt is 0.08 to 0.4 parts, and the polymerization inhibitor is 0.08 to 0.15 parts.

3. The UV-curable high-fluorine anti-fingerprint resin according to claim 1 or 2, characterized in that: The fluorinated epoxy resin has an epoxy value of 0.20 to 0.60, and includes one or more of perfluorobisphenol A diglycidyl ether, 1,3-bis(3-glycidyl tetrafluorophenoxy)-2-hydroxypropane, 1,4-bis(hydroxyhexafluoroisopropyl)benzene diglycidyl ether, 1,3-bis(hydroxyhexafluoroisopropyl)benzene diglycidyl ether, 1,3-bis(hydroxyhexafluoroisopropyl)-5-perfluoropropylbenzene diglycidyl ether, 1,4-bis(hydroxyhexafluoroisopropyl)tetrafluorobenzene diglycidyl ether, 4,4΄-dihydroxyoctafluorobiphenyl diglycidyl ether, and 4,4΄-bis(hydroxyhexafluoroisopropyl)octafluorobiphenyl diglycidyl ether.

4. The UV-curable high-fluorine anti-fingerprint resin according to claim 1 or 2, characterized in that: The perfluorocarboxylic acid includes one or more of trifluoroacetic acid, perfluoropropionic acid, perfluorobutyric acid, perfluoropentanoic acid, perfluorohexanoic acid, perfluoroheptanoic acid, perfluorooctanoic acid, perfluorononanoic acid, perfluorodecanoic acid, perfluoroundecanoic acid, perfluorododecanoic acid, perfluorotridecanoic acid, and perfluorotetradecanoic acid.

5. The UV-curable high-fluorine anti-fingerprint resin according to claim 1 or 2, characterized in that: The fluorinated anhydride includes: one or more of monofluorobenzoic anhydride, difluorobenzoic anhydride, tetrafluorobenzoic anhydride, and difluoromaleic anhydride; and / or The (meth) acrylic acid glycidyl ether includes one or more of acrylic acid glycidyl ether, methacrylic acid glycidyl ether, hydroxyethyl acrylate glycidyl ether, hydroxyethyl methacrylate glycidyl ether, hydroxypropyl acrylate glycidyl ether, and hydroxypropyl methacrylate glycidyl ether.

6. The UV-curable high-fluorine anti-fingerprint resin according to claim 1 or 2, characterized in that: The quaternary ammonium salt or quaternary phosphonium salt includes: one or more of benzyltrimethylammonium chloride, benzyltriethylammonium chloride, benzyltrimethylammonium bromide, benzyltriethylammonium bromide, pyridine hydrochloride and butyltriphenylphosphonium chloride, benzyltriphenylphosphonium chloride, benzyltriphenylphosphonium bromide; and / or The polymerization inhibitor includes: p-tert-butylcatechol, p-hydroxyanisole, 2,6-di-tert-butyl-p-cresol, and tris(N-nitroso-N-phenylhydroxylamine)aluminum.

7. The UV-curable high-fluorine anti-fingerprint resin according to claim 1, characterized in that: In step S1, the heating temperature is 80°C to 90°C, the heating reaction time is greater than or equal to 4 hours, the temperature is raised to 100°C to 130°C for reaction, and the temperature is lowered to 80°C to 95°C; and / or In step S2, the temperature is controlled to be 80°C to 97°C, and the reaction time is greater than or equal to 4 hours; and / or In step S3, the mixture C is slowly added dropwise within 4 hours, the temperature is controlled at 95°C to 97°C, the heating reaction time is greater than or equal to 12 hours, and the temperature is lowered to 25°C to 30°C.

8. Use of the UV-curable high-fluorine anti-fingerprint resin according to any one of claims 1 to 6 in UV anti-fingerprint liquid.

9. The use according to claim 8, characterized in that: UV anti-fingerprint liquid includes the following components by weight: The UV-curable high-fluorine anti-fingerprint resin is 50-60 parts, the fluorinated (meth) acrylate monomer is 15-30 parts, the multifunctional acrylate is 1-5 parts, the photoinitiator is 3-7 parts, the (meth) acryloxy silane coupling agent is 5-10 parts, and the solvent is 5-10 parts.

10. The use according to claim 9, characterized in that: The fluorinated (meth) acrylate monomer includes one or more of hexafluorobutyl acrylate, dodecafluoroheptyl methacrylate, octafluoro-1,6-hexanediol diacrylate, and heptadecafluorodecyl acrylate; The multifunctional acrylate includes 10-15-functional hyperbranched polyester acrylate or pentaerythritol hexaacrylate; The photoinitiator includes 2-hydroxy-2-methyl-1-phenyl-1-propanone or diphenyl-(2,4,6-trimethylbenzoyl)phosphine oxide; The (meth)acryloxysilane coupling agent includes methacryloxytrimethoxysilane or acryloxytrimethoxysilane.

11. The use according to claim 9 or 10, characterized in that: The UV anti-fingerprint liquid is spin-coated on the surface of a glass substrate and cured by UV to obtain an anti-fingerprint coating.

Citation Information

Patent Citations

  • Fluorine-modified epoxy acrylate resin, ultraviolet curable gloss oil and preparation method thereof, and method for coating gloss oil on substrate

    CN103289058A

  • Application and preparation method of photosensitive resin with low dielectric constant / dielectric loss

    CN109824867A

  • Modified fluororesin as well as preparation method and application thereof

    CN112341560A

  • Hydrophobic coating compositions, articles coated with said compositions, and processes for manufacturing same