Method for manufacturing magnetic memory element using Ru and diamond-like carbon hard mask
By using Ru and diamond-like carbon hard masks, the problem of insufficient resistance to ion milling and chemical mechanical polishing in the prior art is solved, and the memory element column spacing is closer, the data density is higher and the absence of memory elements is achieved. The effect of parasitic resistance.
Patent Information
- Application Number
- CN202080030017.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-04-29
- Filing Date
- 2020-04-28
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2040-04-28
AI Technical Summary
During the manufacturing process of existing magnetic random access memory (MRAM), there is insufficient resistance to ion milling and chemical mechanical polishing of hard mask materials, resulting in large column spacing of memory components, low data density, and easy formation of hard mask materials. Electrically insulating oxides, increasing parasitic resistance.
Using Ru and diamond-like carbon hard masks, a Ru hard mask is formed and a diamond-like carbon layer is deposited on it. Reactive ion etching and chemical mechanical polishing technology are used to form a highly resistant Mask structure reduces the thickness of memory element columns and avoids the formation of electrically insulating oxides.
The memory element column spacing is achieved, increasing data density, and maintaining electrical conductivity, avoiding the emergence of parasitic resistance, and improving manufacturing efficiency and performance of memory elements.
Smart Images

Figure CN113826216B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to magnetic random access memory (MRAM), and more particularly, to a method of fabricating a magnetic memory element using Ru and a diamond-like carbon hard mask. Background Art
[0002] Magnetic random access memory (MRAM) is a non-volatile data storage technology that uses magnetoresistive cells, such as magnetoresistive tunnel junction (MTJ) cells, to store data. At its most basic level, such MTJ elements include first and second magnetic layers separated by a thin non-magnetic layer, such as a tunnel barrier layer, which may be constructed of a material such as Mg-O. The first magnetic layer, which may be referred to as the reference layer, has a magnetization that is fixed in a direction perpendicular to the plane of the layer. The second magnetic layer, which may be referred to as the magnetic free layer, has a magnetization that is free to move so that it can be oriented in either of two directions, both of which are substantially perpendicular to the plane of the magnetic free layer. Thus, the magnetization of the free layer may be parallel to the magnetization of the reference layer, or may be antiparallel to the direction of the reference layer (i.e., opposite to the direction of the reference layer).
[0003] The resistance through the MTJ element in the direction perpendicular to the plane of the layers varies with the relative orientation of the magnetizations of the magnetic reference layer and the magnetic free layer. When the magnetization of the magnetic free layer is oriented in the same direction as the magnetization of the magnetic reference layer, the resistance through the MTJ element is in its lowest resistance state. Conversely, when the magnetization of the magnetic free layer is oriented in the opposite direction to the magnetization of the magnetic reference layer, the resistance across the MTJ element is in its highest resistance state.
[0004] The switching of the MTJ element between the high resistance and low resistance states is caused by the electron spin transfer. Electrons have a spin orientation. Typically, electrons flowing through a conductive material have a random spin orientation without a net spin orientation. However, when electrons flow through a magnetized layer, the spin orientation of the electrons becomes aligned, so that there is a net alignment orientation of the electrons flowing through the magnetic layer, and the orientation of this alignment depends on the orientation of the magnetization of the magnetic layer through which the electrons pass. When the orientation of the magnetization of the free layer and the reference layer is oriented in the same direction, the orientation of most of the spins of the electrons in the free layer is the same as the orientation of most of the spins of the electrons in the reference layer. Since the directions of these electron spins are substantially the same, electrons can pass through the tunnel barrier layer relatively easily. However, if the magnetization orientations of the free layer and the reference layer are opposite to each other, then the spins of most of the electrons in the free layer are substantially opposite to the spins of most of the electrons in the reference layer. In this case, electrons cannot easily pass through the barrier layer, resulting in a higher resistance through the MTJ stack.
[0005] Because the MTJ element can be switched between low resistance and high resistance states, it can be used as a memory element to store a data bit. For example, the low resistance state can be read as "1" and the high resistance state can be read as "0". In addition, because the magnetic orientation of the magnetic free layer remains in its switched orientation in the absence of any power to the element, it provides a robust non-volatile data storage bit.
[0006] In order to write a data bit to the MTJ cell, the magnetic orientation of the magnetic free layer can be switched from a first direction to a second direction 180 degrees from the first direction. This can be achieved, for example, by applying a current through the MTJ element in a direction perpendicular to the plane of the layer of the MTJ element. The current applied in one direction will switch the magnetization of the free layer to the first direction, and switching the direction of the current so that it is applied in the second direction will switch the magnetization of the free layer to the second opposite direction. Once the magnetization of the free layer has been switched by the current, the state of the MTJ element can be read by reading the current across the MTJ element to determine whether the MTJ element is in a "1" bit state or a "0" bit state. Advantageously, once the switching current is removed, the magnetic state of the free layer will remain in the switched orientation until another current is applied to switch the MTJ element again. Therefore, the recorded data bit is non-volatile because it remains intact in the absence of any power. Summary of the invention
[0007] The present invention provides a method for manufacturing a magnetic memory element using Ru and a diamond-like carbon hard mask. The method comprises depositing a plurality of memory element layers, depositing a Ru layer on the plurality of memory element layers, and depositing a diamond-like carbon layer on the Ru layer. A photoresist mask is formed on the diamond-like carbon layer, and reactive ion etching is performed to transfer the image of the photoresist mask to the diamond-like carbon layer to form a diamond-like carbon mask. Ion milling is then performed to transfer the image of the diamond-like carbon mask to the Ru layer to form a Ru hard mask. The ion milling is continued to remove portions of the plurality of magnetic memory element layers that are not protected by the Ru hard mask.
[0008] After performing the ion milling, a non-magnetic dielectric isolation layer may be deposited, followed by a layer of material resistant to chemical mechanical polishing (CMP stop layer). Chemical mechanical polishing may then be performed, and reactive ion etching may be performed to remove the CMP stop layer. Such reactive ion etching may also be used to remove the diamond-like carbon hard mask. The CMP stop layer may be diamond-like carbon, and the reactive ion etching process for removing the CMP stop layer and the diamond-like carbon hard mask may be performed using an atmosphere containing oxygen (O2).
[0009] The ion milling process may be performed to form a magnetic memory element pillar having an outer side. After performing the ion milling, a high angle (grazing angle) ion milling may be performed to remove any redeposited material (redep) from the outer side of the memory element pillar. After depositing the non-magnetic dielectric isolation layer, a post-pillar annealing process may be performed to repair damage to the outer side of the magnetic element pillar structure caused by the high angle ion milling process.
[0010] The use of diamond-like carbon in combination with Ru as a hard mask layer provides several decisive advantages. For example, the diamond-like carbon can be removed by reactive ion etching, which allows it to be easily patterned by reactive ion etching to form a mask for patterning the underlying Ru layer. In addition, diamond-like carbon is highly resistant to removal by chemical mechanical polishing (CMP). This makes diamond-like carbon (when present) a good CMP stop layer during the CMP planarization process described above. After performing the CMP, the diamond-like carbon mask can be easily removed by reactive ion etching, leaving only the Ru hard mask on the memory element structure.
[0011] On the other hand, Ru is a good hard mask during ion milling because of its resistance to ion milling removal. Once patterned by the diamond-like carbon hard mask above, the Ru hard mask can remain essentially intact during the entire ion milling process for defining the memory element column. Since the Ru hard mask has a high resistance to ion milling removal and chemical mechanical polishing, it can be much thinner than other hard mask materials. This advantageously reduces the thickness of the memory element column and the hard mask structure, which leads to a reduction in the shielding effect during the grazing, high-angle ion milling described above. As a result, adjacent memory cells can be spaced closer, resulting in an increase in data density in the memory element array. Another significant advantage of using Ru as a hard mask layer stems from the fact that Ru does not form an electrically insulating oxide like other hard mask layers (such as Ta). Because the Ru hard mask layer does not form an electrically insulating oxide, it remains highly conductive throughout the entire manufacturing process. Therefore, the Ru hard mask layer can be maintained in the finished memory element structure without applying any significant parasitic resistance to the memory element structure or the memory element array.
[0012] These and other features and advantages of the present invention will become apparent upon reading the following detailed description of the embodiments taken in conjunction with the accompanying drawings, wherein like reference numerals refer to like elements throughout. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] For a fuller understanding of the nature and advantages of the present invention, as well as the preferred mode of use, reference should be made to the following detailed description read in conjunction with the accompanying drawings, which are not drawn to scale.
[0014] Figure 1 is a schematic cross-sectional view of a perpendicular magnetic tunnel junction (pMTJ) element;
[0015] Figures 2 to 7 A magnetic memory element is shown at various stages of manufacture in order to illustrate a method of manufacturing a magnetic memory element according to an embodiment of the present invention;
[0016] Figures 8 to 15 A magnetic memory element is shown at various stages of fabrication to illustrate a method of fabricating a magnetic memory element according to an alternative embodiment;
[0017] Figures 16 to 24 A magnetic memory element is shown at various stages of manufacture to illustrate a method of manufacturing a magnetic memory element according to yet another embodiment; and
[0018] Fig.25a and 25b Illustrate the effect of post height on the minimum post spacing in high-angle ion milling process. DETAILED DESCRIPTION
[0019] The following description is of the best embodiment currently considered for carrying out the invention. This description is for the purpose of illustrating the general principles of the invention and is not meant to limit the inventive concept claimed herein.
[0020] Reference now Figure 1 , the magnetic memory element 100 may be in the form of a perpendicular magnetic tunnel junction (pMTJ) memory element. The magnetic memory element may include an MTJ 101, which may include a magnetic reference layer 102, a magnetic free layer 104, and a thin non-magnetic electrically insulating barrier layer 106 located between the magnetic reference layer 102 and the magnetic free layer 104. The barrier layer 106 may be an oxide such as MgO. The magnetic reference layer has a magnetization 108 that is fixed in a direction that is preferably perpendicular to the plane of the layer as indicated by arrow 108. The magnetic free layer 104 has a magnetization 110 that may be in either of two directions perpendicular to the plane of the layer 104. Although the magnetization 110 of the free layer 104 remains in either of the two directions perpendicular to the plane of the layer 104 in a stationary state, it can move between the two directions, as will be described in more detail below. When the magnetization 110 of the magnetically free layer 104 is in the same direction as the magnetization 108 of the reference layer 102, the resistance across the layers 102, 106, 104 is in a low resistance state. Conversely, when the magnetization 110 of the free layer 104 is opposite to the magnetization 108 of the reference layer 102, the resistance across the layers 102, 106, 104 is in a high resistance state.
[0021] The magnetic reference layer 102 may be part of an antiparallel magnetic pinning structure, such as a synthetic antiferromagnet (SAF) 112, which may include a magnetically balanced bottom layer 114 and a non-magnetic antiparallel coupling layer (e.g., Ru) 116 located between the bottom SAF layer 114 and the reference layer 102. The antiparallel coupling layer 116, which will be described in more detail below, may be constructed to have a composition and thickness such that it couples the layers 114, 102 in an antiparallel configuration. The antiparallel coupling between the layers 114, 102 ensures that the magnetization 108 of the reference layer 102 is in a direction opposite to the direction of the magnetization 118 of the bottom SAF layer 114.
[0022] A seed layer 120 may be provided near the bottom of the memory element 100 to initiate the desired crystal structure in the above-mentioned deposited layer. A capping layer 121 may be provided near the top of the memory element 100 to protect the bottom layer during manufacturing, such as during high temperature annealing, and to prevent it from being exposed to the ambient atmosphere. The capping layer 121 may be constructed of, for example, Ta. In addition, a Ru hard mask layer 122 is formed at the top of the memory element 100, on the capping layer 121. Optionally, the Ru layer 122 can be used as both a hard mask layer and a capping layer 121, thereby eliminating the need for a separate capping layer 122. The use of Ru provides several advantages compared to other hard mask material layer materials. For example, even after various processing steps that would oxidize other hard mask materials, the Ru hard mask layer 122 does not oxidize, and therefore remains a good conductor. Therefore, the Ru hard mask 122 can remain in the finished memory element 100 without applying any parasitic resistance. In addition, Ru has high resistance to removal by ion beam etching (also known as ion milling). This advantageously allows the hard mask layer to be thinner, which in turn allows the pitch of the memory element to be reduced and the data density to be increased.These advantages of such a Ru cap layer 122 will be more readily understood with respect to the various methods of fabricating magnetic memory elements described in more detail below.
[0023] Additionally, electrodes 124, 126 may be provided at the bottom and top of the memory element 100. The electrodes 124, 126 may be constructed of a non-magnetic conductive material, such as one or more of Ta, W, Cu, and Al, may provide electrical connections to circuitry 128, which may include a current source and may further include circuitry for reading the resistance across the memory element 100, such as CMOS circuitry.
[0024] The magnetic free layer 104 has a perpendicular magnetic anisotropy that causes the magnetization 110 of the free layer 104 to remain stable in one of two directions perpendicular to the plane of the free layer 104. In a write mode, the orientation of the magnetization 110 of the free layer 104 can be switched between these two directions by applying a current from the circuit system 128 through the memory element 100. A current in one direction will flip the memory element to a first orientation, while a current in the opposite direction will flip the magnetization to a second, opposite direction. For example, if the magnetization 110 is in a write mode, the magnetization 110 of the free layer 104 will be switched between these two directions. Figure 1 If the reference layer 102 is initially oriented in a downward direction, then applying a current through the element 100 in the downward direction will cause electrons to flow in the opposite direction, upward, through the element 100. The electrons traveling through the reference layer will become spin-polarized due to the magnetization 108 of the reference layer 102. These spin-polarized electrons produce a spin torque on the magnetization 110 of the free layer 104, which causes the magnetization to flip direction.
[0025] On the other hand, if the magnetization 110 of the free layer 104 is Figure 1 If the free layer 104 is initially in the upward direction, then applying a current through the element 100 in the upward direction will cause electrons to flow through the element 100 in the opposite direction, downward. However, because the magnetization 110 of the free layer 104 is opposite to the magnetization 108 of the reference layer 102, the electrons with the opposite spin will not be able to efficiently pass through the barrier layer 106 to the reference layer 102. As a result, the electrons with the opposite spin will be reflected at the barrier layer 106 and return to the free layer 104 with a spin polarization opposite to the reference layer 102. These spin-polarized electrons cause a spin torque that causes the magnetization 110 of the free layer 104 to flip from the upward direction to the downward direction.
[0026] Figures 2 to 7 A method for fabricating a magnetic memory element with a Ru capping layer according to an embodiment is described. A substrate 202 is provided, which may be a semiconductor substrate (e.g., a Si substrate). In addition, the substrate 202 may have various circuit systems incorporated therein, such as CMOS circuit systems (not shown), to facilitate writing and reading data to the magnetic memory element.
[0027] A series of magnetic memory element layers 206 are deposited on the seed layer 204. The magnetic memory element layers 206 may include layers for forming magnetic tunnel junction elements, and may include the seed layer 204, a synthetic antiferromagnetic (SAF) structure 208, a non-magnetic barrier layer 210 (e.g., MgO) deposited on the SAF structure 208, a magnetic free layer 212 deposited on the non-magnetic barrier layer 210, and a cap layer 214 deposited on the magnetic free layer 212. The SAF structure may include a first magnetic layer (reference layer) 216 formed adjacent to the barrier layer 210, a second magnetic layer 218 opposite the reference layer 216, and a non-magnetic antiparallel exchange coupling layer 220 located between the reference layer 216 and the second magnetic layer 218. The antiparallel exchange coupling layer 220 may be a material such as Ru, and have a thickness selected to exchange couple the magnetic layers 216, 218 in an antiparallel direction relative to each other. The magnetic layers 216, 218, 212 may include one or more magnetic materials such as CoFe, CoFeB, and / or Heusler alloys. The cap layer 214 may include a non-magnetic conductive material such as Ta. The seed layer 204 may be formed of a conductive material selected to initiate a desired crystal structure in the layers deposited thereon.
[0028] A new hard mask layer 222 is deposited on the memory element layer. The hard mask layer 222 includes a Ru layer 224 and may also include an optional RIEable layer 226 formed of a material that can be removed by reactive ion etching and deposited on the Ru layer 224. A photoresist mask layer 228 is deposited on the hard mask layer 222. Ru as a hard mask layer 224 provides several advantages. For example, Ru is highly resistant to ion etching (ion milling) removal, which allows the Ru layer to be deposited thinner than other hard mask layers. For reasons that will be more clearly described below, this reduced thickness allows higher data density by allowing the memory element array to be spaced closer together. In addition, Ru provides the advantage that it does not form oxides. This allows the Ru in the finished magnetic memory element to remain highly conductive, thereby not applying harmful parasitic resistance. The RIEable layer 226 can be a material such as tantalum (Ta), tantalum nitride (TaN), or silicon oxide (SiOx). The photoresist layer 228 may include a layer of photoresist material, and may also include other layers, such as a bottom anti-reflective coating and / or an image transfer layer.
[0029] Reference now Figure 3, the photoresist layer 228 is photolithographically patterned to form a photoresist mask 228. When viewed from above, the photoresist mask 228 may have a circular configuration designed to form a cylindrical pillar structure, as will be seen. However, this is not required and other configurations are possible. Reactive ion etching may then be performed to transfer the image of the photoresist mask 228 to the underlying RIEable mask layer 226, as shown. Figure 3 . The reactive ion etching may be performed using a chemistry selected to preferentially remove layer 226. For example, if layer 226 is Ta or TaN, the reactive ion etching may be performed using a fluorine (F2) or chlorine chemistry. If layer 226 is SiOx, the reactive ion etching may be performed using a chemistry including fluorine.
[0030] Then, refer to Figure 4 , ion etching (also referred to as ion milling) is performed to transfer the image of the RIEable mask 226 onto the underlying Ru hard mask layer 224. The ion etching is further continued to remove portions of the memory element material layer 206 that are not protected by the masks 224, 226. The ion etching process can be performed at one or more angles relative to the normal in order to achieve the desired substantially vertical sidewalls on the sides of the resulting memory element pillars. Ion milling can remove all of the photoresist 228, and can also remove some or all of the RIEable mask 226. As described below, any remaining RIEable mask 226 can be removed later by reactive ion etching.
[0031] The process of ion etching used to form the memory element pillars inevitably results in redeposition of removed material (also referred to as "redep") 402 at the sides of the memory element pillars. Such redep on the sides of the memory element pillars 206 is undesirable because it can result in current shunting and reduced performance of the finished memory element. Therefore, the redep 402 should be removed before further processing is performed. This redep 402 can be effectively removed by performing the ion etching at a high angle relative to the normal, thereby producing a redep 402 such as Figure 5 The structure shown in FIG. 1 does not have redep. This ion etching (which may be referred to as grazing angle ion etching or ion milling) may be performed at an angle of 50 to 80 degrees relative to the normal.
[0032] As will be appreciated by those skilled in the art, the memory element pillars are formed into an array of many memory element pillars, and the closer these memory element pillars are spaced relative to one another, the higher the data density will be. Therefore, it is desirable to space adjacent memory element pillars as close to one another as possible while avoiding magnetic and electrical interference between adjacent memory element pillars. However, as previously described, this spacing reduction is limited by the need to perform high angle milling to remove redep 402. This is because when the memory element pillars are spaced too closely, shadowing from adjacent pillars can prevent the high angle ion milling process from reaching the bottom of the pillars. The taller the pillar structure, the greater the shadowing effect. This reference Fig.25a and 25b To explain. Fig.25a shows ion milling performed at an angle θ on an array of pillars 2502 having a first height H1, and Fig.25b Ion milling is shown performed at the same angle θ on a second array of pillars 2504 having a height H2 less than height H1. Fig.25a , in order for ion milling to reach the bottom of adjacent pillars, the pillars 2502 must be spaced apart by a certain minimum distance L1. Fig.25b In the case where the pillars 2504 are shorter, the pillars 2504 may be spaced apart by a second minimum distance L2 that is significantly less than the first minimum distance L1. Thus, reducing the height of the pillars being ion milled reduces the minimum allowable spacing between the pillars.
[0033] Reference again Figure 4 and 5 , the effective height of the pillars on which high angle ion milling will be performed includes the thickness of the Ru hard mask 224. However, since Ru is very resistant to removal by ion milling, it can be made much thinner than is possible using other hard mask layers. This effectively reduces the height of the pillars being ion milled, and therefore advantageously allows arrays of memory element pillars to be spaced significantly closer together to increase data density.
[0034] Continue to refer Figure 5 The ion milling process described above causes a certain amount of damage to the material layer outside the memory element pillar 206. Figure 5, this results in a damaged region 502 at the outer edge of the non-magnetic electrically insulating barrier layer 210. Although it is desirable that the barrier layer 210 be constructed of a material having a desired crystalline structure, such as magnesium oxide (MgO), the damage caused by ion milling may result in the damaged portion 502 having, for example, an amorphous structure or may result in segregation of Mg and O, such that the damaged portion 502 may include Mg rather than crystalline MgO. This may result in undesirable electrical shunting through the damaged portion 502 during use. However, a post-pillar annealing process, which will be described in more detail below, may overcome this problem by repairing the damaged portion 502, thereby producing a desired crystalline MgO structure for the entire barrier layer 210.
[0035] Reference now Figure 6 , a non-magnetic dielectric material (separation layer) (e.g., SiNx) 602 can be deposited by a process such as sputtering deposition or chemical vapor deposition to a height of about the height of the memory element pillar structure 206. A layer of material that is resistant to chemical mechanical polishing and can also be removed by reactive ion etching (CMP stop layer) 604 can be deposited on the separation layer 602. The CMP stop layer 604 can be, for example, diamond-like carbon or some other suitable material. In addition, Ru is advantageously very resistant to chemical mechanical polishing removal. Therefore, the Ru hard mask 224 can also be used as an effective CMP stop layer in the area on the pillar structure.
[0036] Then, chemical mechanical polishing (CMP) is performed to planarize the structure, and then reactive ion etching may be performed to remove the CMP stop layer 604. A reactive ion etching process may be performed to remove any remaining RIEable mask layer 226, leaving behind the structure. Figure 7 At this point, a post-column annealing process may be performed to repair any damage to the barrier layer 210 (e.g., repair Figure 5 The damaged portion 502 in the column structure) and the layers of the column structure are appropriately crystallized. This post-column annealing process may include heating the entire structure (e.g., a wafer) to a desired temperature and for a desired duration to allow the damaged portion 502 ( Figure 6 ) and other layers of the pillar structure as needed. Although this annealing process may include separate annealing steps (one for repairing the damaged portion 502 and another for recrystallizing the other pillar layers), the annealing may be performed as a single annealing step to achieve both purposes. This annealing process may include raising the wafer and associated magnetic memory element layer 206 to a temperature of 350 to 400° C. for a duration of 3 minutes to 3 hours.
[0037] Figures 8 to 14 Magnetic memory elements are shown at various intermediate fabrication stages in order to illustrate methods of fabricating magnetic memory elements according to alternative embodiments of the present invention. Figure 8, a plurality of layers 206 configured to define a magnetic memory element structure are deposited on a substrate 202. Layers 206 may include a seed layer or bottom layer 204, a synthetic antiferromagnetic structure 208, a nonmagnetic electrically insulating barrier layer 210, a magnetically free layer 212, and a cap layer 214. The magnetically free layer may include one or more of Co, CoFe, a Heusler alloy, or some other suitable material or combination of materials. Barrier layer 210 may be formed of an oxide, and is preferably constructed of magnesium oxide MgO. Cap layer 214 may be a material such as Ta and / or some other layer or combination of layers that is selected to promote the desired magnetic properties in the underlying layers and may protect the underlying layers from damage during fabrication.
[0038] The synthetic antiferromagnetic structure 208 may include a first magnetic layer 218, a second magnetic layer as a reference layer 216, and an antiparallel exchange coupling layer 220 located between the first magnetic layer 218 and the reference layer 216. The first magnetic layer 218 and the reference layer 216 may each be constructed of one or more of CoFe, CoFeB, a Heusler alloy, or some other suitable magnetic material. The antiparallel exchange coupling layer 220 may be formed of a material such as Ru, the thickness of which is selected to strongly antiparallel exchange couple the first magnetic layer 218 and the reference layer 216 so that they have magnetizations pinned in opposite directions perpendicular to the planes of the layers 218, 216.
[0039] A novel hard mask structure 802 is deposited on the memory element layer 206, and a photoresist material layer 228 is deposited on the novel hard mask structure 802. The novel hard mask structure 802 includes a Ru layer 804 and a carbon layer, preferably diamond-like carbon (DLC) 806, deposited on the Ru layer 804. The hard mask structure 802 may also include other layers, such as one or more of Ta, TaN, or SiOx (not shown) deposited on the Ru layer. As discussed above, the use of Ru as a hard mask layer provides several advantages over the use of other hard mask layers. For example, Ru does not form an electrically insulating oxide, and therefore provides a good conductive hard mask / capping layer that can be left in the finished memory element without imparting undesirable parasitic resistance to the memory element structure. In addition, as discussed above, Ru has good resistance to ion etching (ion milling) removal, so it can be deposited thinner than other hard mask materials. As discussed above, this results in less shadowing effects, which allows memory element pillars to be spaced closer together to improve data density.
[0040] In addition, the use of diamond-like carbon 228 provides additional benefits compared to other hard mask materials. Diamond-like carbon can be removed by reactive ion etching, and can therefore be patterned by reactive ion etching to form an effective hard mask for patterning the underlying Ru layer 804, as will be seen. This ability to remove diamond-like carbon by reactive ion etching also allows for efficient removal of the diamond-like carbon after the pillars are formed by reactive ion etching, thereby providing good conductivity. Another significant advantage of diamond-like carbon is that it has excellent resistance to chemical mechanical polishing (CMP), making it a good CMP stop layer, as will be seen.
[0041] Reference now Fig. 9 , the photoresist layer 228 is photolithographically patterned to have a shape configured to define a magnetic memory element pillar. As discussed above, the photoresist mask 228 can be patterned to have a generally circular shape when viewed from above so as to define a cylindrical pillar thereunder. However, this is not required. Then, with reference to Fig.10 , a reactive ion etch is performed to transfer the image of the photoresist mask 228 to the underlying DLC layer 806, leaving a patterned DLC hard mask 806, as shown. Fig.10 . Reactive ion etching is performed using an atmosphere selected to preferably remove carbon (DLC). Therefore, this reactive ion etching can be performed in an oxygen (O2) atmosphere, which easily removes carbon. In addition, as mentioned above, in addition to the DLC layer 806, other mask layers such as Ta, TaN or SiOx (not shown) may also be included. The use of these additional mask layers may involve additional reactive ion etching steps configured to remove such additional layers. For example, if a Ta or TaN layer is deposited on the DLC layer 806, a first reactive ion etching can be performed using an atmosphere containing fluorine (F2) or chlorine. This first reactive ion etching in a fluorine or chlorine atmosphere can be used to transfer the image of the photoresist mask to the underlying Ta or TaN mask layer. Then, a second reactive ion etching can be performed in an atmosphere containing O2 to transfer the image of the patterned Ta or TaN mask to the DLC layer 806. On the other hand, if a SiOx layer is formed on the DLC layer, a fluorine atmosphere can be used to remove this material. Reactive ion etching using an O2 atmosphere can then be used to transfer the image of the hard mask onto the underlying DLC layer.
[0042] Then, refer to Fig.11, ion etching (also referred to as ion milling) is performed to transfer the image of the patterned DLC mask 806 (and other mask layers, if present) onto the underlying Ru hard mask layer 804. This ion milling can continue to remove the memory element material 206 to define the memory element pillar structure, as shown. In addition, the DLC mask layer 806, which is also resistant to removal by ion milling, can remain substantially intact after ion milling. This advantageously allows the Ru hard mask 804 to be deposited thinner than would otherwise be possible, while also allowing the remaining DLC mask 806 to be removed later by reactive ion etching.
[0043] This ion milling process causes redeposition of material (redep) 402 on the sides of the memory element pillar 206. As previously discussed, this redeposited material can cause current shunting in the finished memory element structure. Therefore, a high angle (e.g., grazing angle) ion milling process may be performed to remove the redeposited material 402 from the sides of the memory element pillar 206, leaving behind a portion of the memory element pillar 206. Fig.12 The structure shown in FIG. 1 is a schematic diagram of a structure shown in FIG. 1. This high angle or grazing angle ion milling can be performed at an angle of 50 to 80 degrees relative to the normal. The Ru hard mask layer 804 and the DLC hard mask 806 protect the upper portion of the memory element pillar 20. Fig.12 As can be seen in , this high angle ion milling can result in damage to the material at the outer edge of the memory element pillar. More specifically, the high angle ion milling can result in damage at the outer edge of the barrier layer 210 (represented as the shaded area 502). As a result, the damaged outer portion 502 of the barrier layer 210 can have an amorphous structure rather than the desired crystalline structure. This can cause the outer portion to be conductive and not act as an effective tunnel barrier, and therefore can result in current shunting through the damaged outer portion 502. A post-pillar annealing process, which will be described in more detail below, can correct this by reordering the damaged portion 502 to the desired crystalline state. This anneal can include raising the wafer and the memory element layer 206 formed thereon to a temperature of 350 to 400° C. and continuing for a duration of 3 minutes to 3 hours.
[0044] Reference now Fig.13 , a non-magnetic dielectric isolation layer such as SiNx 1302 is deposited to a height at least as high as the top of the memory element structure. A CMP stop layer 1304 such as diamond-like carbon (DLC) may then be deposited on the dielectric isolation layer 1302. A chemical mechanical polishing is then performed to planarize the surface. A reactive ion etch may then be performed to remove any remaining CMP stop layer 1304 and any remaining DLC hard mask layer 806, leaving a Fig.14 The structure shown in Fig.14, only the Ru hard mask 804 remains on the memory element structure 206. Advantageously, because the Ru hard mask 804 does not oxidize, it can remain in the finished structure without adding any parasitic resistance to the memory element layer. A conductive top contact can be added on the Ru layer 804.
[0045] Figures 15 to 24 A method for manufacturing a magnetic memory element according to another embodiment is described. This method is a self-aligned partial milling process that results in improved properties of the memory element layer, especially with respect to the tunnel barrier layer. This method can be implemented with any of the novel hard mask structures described above. Fig.15 , a substrate 202 is provided, which may be a silicon wafer substrate and may include circuitry (e.g., CMOS circuitry) formed therein. A series of memory element layers 206 are deposited on the substrate 202. The memory element layers 206 may include a seed layer 204, a synthetic antiferromagnetic structure (SAF) 208, a nonmagnetic barrier layer 220, a magnetic free layer 212, and a cap layer 214. The synthetic antiferromagnetic structure 208 may include first and second magnetic layers 218, 216, and a nonmagnetic antiparallel exchange coupling layer 220 located between the first and second magnetic layers 218, 216. Each memory element layer 206 may include, for example, the above-mentioned Figures 2 to 7 8 to 15 discussed above. The memory element layer 206 may also include other additional layers, such as, but not limited to, a spin current structure (not shown). A hard mask structure 222 may be deposited on the memory element layer 206. The hard mask structure 222 may be any of the hard mask structures described above. For example, the hard mask structure 222 may include a Ru layer 224 and a RIEable layer 226, which may be one or more of Ta, TaN, SiOx, or diamond-like carbon (DLC) deposited on the Ru hard mask 224. Alternatively, the hard mask structure 222 may include only the Ru layer 224 without the RIEable layer 226 deposited thereon. A photoresist layer 228 is then formed on the hard mask structure 222. The photoresist layer 228 may be spin-coated onto the hard mask layer 222 by techniques familiar to those skilled in the art.
[0046] Reference now Fig.16 , the photoresist layer 228 is photolithographically patterned and developed to form a photoresist mask, as shown, which is configured to define the upper portion of the memory element pillar structure. As described above, the patterned photoresist mask 228 can be configured to have a circular shape when viewed from above. Fig.17, a reactive ion etching process is performed to transfer the image of the photoresist mask onto the underlying RIEable hard mask layer 226. This reactive ion etching is performed in an atmosphere selected to effectively remove the material constituting the RIEable hard mask layer 226. For example, if the RIEable hard mask 226 is Ta or TaN, the reactive ion etching can be performed using a fluorine or chlorine atmosphere. If the mask layer 226 is SiOx or diamond-like carbon (DLC), the reactive ion etching can be performed in a fluorine atmosphere.
[0047] Then, refer to Fig.18 , a first ion beam etch (also referred to as ion milling) is performed. This first ion milling is performed so as to extend only partially through the plurality of memory element layers 206. More preferably, the first ion milling is performed until the barrier layer 210 has been removed or shortly thereafter (which will remove material slightly into the reference layer 216). This ion milling results in a certain amount of redeposited material 1802 on the sides of the ion milled portions of the memory element layers 206, such as Fig.18 Advantageously, however, because the first ion milling removes only a portion of the layers of memory element 1802, the amount of redeposited material 1802 is greatly reduced compared to the amount of redeposited material that would be present if a full ion milling process that would remove all layers of memory element 206 were performed.
[0048] High angle ion milling (a high angle relative to the normal, or a "grazing" angle) is then performed to remove redeposited material 1802 from the sides of the ion milled portion of the memory element, leaving behind Fig.19 . This high angle ion milling can be performed at an angle of 50 to 80 degrees or more relative to the normal. As indicated by the shaded area 1902, the high angle ion milling also causes a small amount of damage to the outer edge of the nonmagnetic barrier layer. The partial first ion milling described above provides a number of advantages. First, because the amount of redeposited material is significantly less than that present using full ion milling, a less aggressive high angle ion milling is required to remove the redeposited material 1802. This results in less damage to the sides of the memory element, and more specifically, less damage 1902 to the outer edge of the nonmagnetic barrier layer 210. In addition, as described above with reference to Fig.25a and 25b As discussed, the amount by which the spacing between adjacent memory element pillars can be reduced during high angle ion milling is limited by the height of the memory element pillars. However, in the case of the first portion of ion milling described above, the height of the pillars is greatly reduced during high angle ion milling. This advantageously allows the memory element pillars in the array to be spaced closer to each other while being less limited by shadowing effects from adjacent memory element pillars. Therefore, this allows for greater data density in the memory element array.
[0049] Reference now Fig. 20 , deposit a non-magnetic electrically insulating material layer (insulating layer) 2002. The insulating layer may be SiOx or some other suitable material, and may be deposited by sputtering deposition, atomic layer deposition (ALD) or chemical vapor deposition (CVD). Then, refer to Fig.21 , a second ion milling is performed to remove the remaining portion of the memory element layer 206. This ion milling can terminate at the substrate 202 or at a non-conductive bottom layer to avoid current shunting between adjacent memory element pillars. As can be seen, during this second ion milling, the insulating layer 2002 protects the previously defined portion of the memory element 206, and more specifically protects the previously defined barrier layer 212.
[0050] Reference now Fig. 22 , a non-magnetic dielectric isolation layer 2202 is deposited, preferably to a height substantially flush with the top of the memory element layer 206. A CMP stop layer 2204 is then deposited on the non-magnetic dielectric isolation layer 2202. The non-magnetic dielectric isolation layer 2202 may be, for example, an oxide (e.g., silicon oxide SiOx) that may be deposited by sputtering deposition. The CMP stop layer 2204 is a material layer that is resistant to removal by chemical mechanical polishing. The CMP stop layer is preferably diamond-like carbon (DLC), which may be deposited by sputtering deposition, atomic layer deposition (ALD), or chemical vapor deposition (CVD).
[0051] Chemical mechanical polishing may then be performed to planarize the structure, and reactive ion etching may be performed to remove the CMP stop layer 2204. Reactive ion etching may also be performed to remove the RIEable mask layer 224. This leaves a Fig.23 . If the CMP stop layer 2204 is diamond-like carbon (DLC), a reactive ion etch may be performed using an atmosphere (O2) containing oxygen. If the RIEable mask layer 226 is SiOx or diamond-like carbon (DLC), a reactive ion etch using an oxygen chemistry may also be used to remove the mask layer 226. If the mask layer 226 is Ta or TaN, a reactive ion etch using a fluorine or chlorine chemistry may be used to remove the mask layer 226. If the mask 226 is SiOx, a fluorine chemistry may be used, and if the mask 226 is DLC, an oxygen chemistry may be used. As can be seen, the above process results in a structure in which the Ru cap layer 224 remains exposed at the top above the top of the memory element pillar 206. As previously discussed, since the Ru cap layer does not form an electrically insulating oxide and is highly conductive, it may remain in the finished structure without applying any parasitic resistance to the memory cell structure.
[0052] At this point, a post-pillar formation annealing process may be performed to repair the damaged outer portion 1902 of the barrier layer 210 caused by the previous high-angle ion milling operation, leaving behind Fig.24 , where the damaged portion 1902 is repaired. As described above, the self-aligned process results in significantly less damage 1902 to the outer portion of the barrier layer 210. As a result, the amount of annealing required to repair the outer edge of the barrier layer to its desired crystalline state can be advantageously reduced. It should be noted that the post-pillar annealing process can also be performed after the deposition of the dielectric isolation layer 2202 and before performing the chemical mechanical polishing and reactive ion etching processes.
[0053] Although various embodiments have been described above, it should be understood that they are presented by way of example only and not limitation. Other embodiments falling within the scope of the present invention may also become apparent to those skilled in the art. Therefore, the breadth and scope of the present invention should not be limited by any of the exemplary embodiments described above, but should only be defined in accordance with the appended claims and their equivalents.
Claims
1. A method for manufacturing a magnetic memory element, the method comprising: include: depositing a plurality of memory element layers on the wafer; depositing a Ru layer on the plurality of memory element layers; depositing a diamond-like carbon layer on the Ru layer; forming a photoresist mask on the diamond-like carbon layer; performing a first reactive ion etching to transfer the image of the photoresist mask to the diamond-like carbon layer to form a diamond-like carbon mask; performing ion milling to transfer the image of the diamond-like carbon mask onto the Ru layer to form a Ru hard mask and continuing the ion milling to remove portions of the plurality of memory element layers not protected by the Ru hard mask; After performing said ion milling, depositing a non-magnetic dielectric spacer layer; depositing a layer of material resistant to chemical mechanical polishing; Perform chemical mechanical polishing; and A second reactive ion etching is performed to remove the diamond-like carbon mask and the chemical mechanical polishing resistant material layer. 2 . The method according to claim 1 , wherein the chemical mechanical polishing resistant material layer comprises diamond-like carbon, and the first reactive ion etching and the second reactive ion etching are performed using an atmosphere containing oxygen.
3. The method of claim 1 , wherein the ion milling is a first ion milling configured to form a magnetic memory element pillar having an outer side, the method further comprising performing a second ion milling configured to remove redeposited material from the outer side of the magnetic memory element pillar. The method of claim 3 , wherein the second ion milling is performed at a high angle relative to a normal to the wafer. 5 . The method of claim 3 , wherein the second ion milling is performed at an angle of 50 to 80 degrees relative to a normal to the wafer. 6 . The method of claim 3 , further comprising depositing a non-magnetic dielectric material after performing the second ion milling.
7. A method for manufacturing a magnetic memory array, the method include: depositing a plurality of memory element layers on the wafer; depositing a Ru layer on the plurality of memory element layers; depositing a diamond-like carbon layer on the Ru layer; depositing a photoresist material on the diamond-like carbon layer; photolithographically patterning the photoresist material to form a plurality of photoresist masks configured to define a plurality of memory element pillars; performing a first reactive ion etch to transfer the images of the plurality of photoresist masks to the diamond-like carbon layer; performing ion milling to transfer an image of the diamond-like carbon layer onto the Ru layer to form a plurality of Ru hard mask structures configured to define a plurality of memory element pillars; continuing to perform the ion milling to remove portions of the plurality of memory element layers not covered by the plurality of Ru hard mask structures to form a plurality of magnetic memory element pillars; and After performing the ion milling, high angle ion milling is performed to remove re-deposited material from one side of the magnetic memory element pillar.
8. The method of claim 7, wherein the high angle ion milling is performed at an angle of 70 degrees relative to a normal to the wafer.
9. The method of claim 7, further comprising depositing a non-magnetic dielectric isolation material after forming the plurality of magnetic memory element pillars, and then performing chemical mechanical polishing. 10 . The method according to claim 9 , further comprising performing an annealing process after performing the chemical mechanical polishing.
11. The method of claim 7, wherein the high angle ion milling is performed at an angle of 50 to 80 degrees relative to a normal to the wafer. 12 . The method of claim 7 , further comprising, after performing the ion milling, performing reactive ion etching to remove the diamond-like carbon mask structure.
13. A method for manufacturing a magnetic memory element array, the method include: forming a first conductive contact structure on the substrate; Depositing a plurality of memory element layers on the first conductive contact structure, the plurality of memory element layers comprising a magnetic reference layer, a magnetic free layer, and a non-magnetic barrier layer located between the magnetic reference layer and the magnetic free layer; depositing a Ru layer on the plurality of memory element layers; depositing a diamond-like carbon layer on the Ru layer; forming a photoresist mask on the diamond-like carbon layer; performing reactive ion etching to transfer the image of the photoresist mask to the diamond-like carbon layer to form a diamond-like carbon mask; performing ion milling to transfer the image of the diamond-like carbon mask onto the Ru layer and onto at least a portion of the plurality of memory element layers; and After the ion milling is performed, a non-magnetic dielectric spacer layer is deposited, a CMP stop layer is deposited on the non-magnetic dielectric spacer layer, and chemical mechanical polishing is performed. 14 . The method of claim 13 , further comprising performing reactive ion etching to remove the diamond-like carbon layer and the CMP stop layer after performing the chemical mechanical polishing process.
15. The method of claim 14, wherein the CMP stop layer comprises diamond-like carbon.
16. The method of claim 14, wherein the CMP stop layer comprises diamond-like carbon, and the reactive ion etch performed to remove the CMP stop layer and diamond-like carbon layer is performed using an oxygen chemistry.