Stable high-nickel NMC cathode materials for improved battery performance

By forming a stable coating on the particle surface of the high nickel NMC cathode material of the lithium-ion battery, the problem of high nickel NMC in the charging/discharge cycle is solved, and its performance and life in the lithium-ion battery is improved, especially Degradation caused by liquid-based electrolyte is inhibited by incorporating vanadium, tantalum and niobium into the high nickel NMC cathode material of lithium-ion batteries.

CN113875045BActive Publication Date: 2024-11-12NANO ONE MATERIALS
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202080038523.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-05-21
Filing Date
2020-05-07
Publication Date
2024-11-12
Estimated Expiration
2040-05-07

AI Technical Summary

Technical Problem

High nickel NMC is unstable during the charge/discharge cycle, resulting in limited use of its use in lithium-ion batteries, especially due to degradation problems caused by particle agglomeration and erosion of liquid electrolytes.

Method used

In the high nickel NMC cathode material of lithium-ion batteries, the coating contains metal oxide salts of vanadium, tantalum and niobium to inhibit degradation, especially by liquid-based, by incorporating a stable coating at the gap interface and surface of the particles. Electrolyte-induced degradation.

Benefits of technology

Improves the stability and life of the high nickel NMC cathode, ensures excellent performance during repeated discharge/charging cycles, reduces the impact of uncoated areas on particles, and enhances resistance to disturbances.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113875045B_ABST
    Figure CN113875045B_ABST
Patent Text Reader

Abstract

An improved cathode material is provided, which is particularly suitable for lithium ion batteries. The cathode material includes particles containing an oxide defined by the following formula: LiNi a Mn b X c G d O2, wherein G is an optional dopant; X is Co or Al; a ≥ 0.5; b + c + d ≤ 0.5; and d ≤ 0.1. Each particle includes a coating covering a surface of the particle, wherein the coating comprises a salt of an oxide of a metal selected from vanadium, tantalum and niobium. An agglomerate includes the particles, wherein the agglomerate includes an interstitial interface. The interstitial interface includes adjacent coatings on adjacent particles.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to co-pending U.S. Provisional Application No. 62 / 850,777, filed on May 21, 2020, which is incorporated herein by reference in its entirety. Background Art

[0003] The present invention relates to the formation of high nickel NMC having excellent stability resulting in the ability to undergo multiple charge / discharge cycles.

[0004] Cathode materials containing nickel, manganese and cobalt, known as NMC, have proven to be very suitable for many applications. High nickel NMC is particularly desirable due to its expected high charge capacity. Unfortunately, transition metal-based NMC containing more than 50 mol% nickel has proven to be unstable, so high nickel NMC has had limited success. Coatings of lithium niobate have mitigated the drawbacks of high nickel NMC, but the number of charge cycles is still insufficient.

[0005] Without being limited by theory, it is hypothesized that particles agglomerate during the formation of the high nickel NMC. Since this agglomeration occurs before the lithium niobate coating is formed, the agglomerates such as Figure 1 In the schematic illustration, it is coated. Figure 1 In the embodiment of the present invention, agglomerates 8 of particles 10 have coatings 12 formed on the surfaces of the agglomerates. In the interior regions of the agglomerates, at interstitial interfaces 14 between particles and at interstitial surfaces 15 of the particles, the particles have regions that are not coated with lithium niobate. If the agglomerates are not disturbed, the interior uncoated regions are inconsequential. Unfortunately, during the process of forming the cathode, the particles may at least partially deagglomerate, resulting in particles having uncoated surfaces 11, as shown in FIG. Figure 2 As shown, the uncoated surface may originate from uncoated interstitial interfaces or interstitial surfaces. Yet another perturbation is considered to be the charge cycle, assuming that it also causes some deagglomeration, or at least sufficient separation at the particle boundaries to effectively expose uncoated regions of the particles. Uncoated regions are considered to be a source of degradation for high nickel NMCs, especially when used with liquid electrolytes.

[0006] This article provides an improved high nickel NMC in which individual particles are coated and the coated individual particles form agglomerates. Therefore, during the normal process of cathode formation and charge / discharge, any deagglomerated particles are coated across the entire surface, thereby mitigating the impact of uncoated areas on the particles. Summary of the invention

[0007] It is an object of the present invention to provide an improved high nickel NMC cathode for lithium ion batteries.

[0008] A particular object of the present invention is to provide a high nickel NMC cathode for lithium ion batteries which is stable to perturbations such as repeated discharge / charge cycles, thereby providing a high nickel NMC with excellent performance and life in use.

[0009] One particular feature is the incorporation of a stable coating on the interstitial interfaces and surfaces of the particles of the cathode material, wherein the coating inhibits degradation, particularly when attacked by a liquid-based electrolyte.

[0010] One embodiment of the present invention provides an improved cathode material for a lithium ion battery, comprising:

[0011] Particles comprising an oxide defined by the formula:

[0012] LiNi a Mn b X c G d O2

[0013] wherein G is an optional dopant;

[0014] X is Co or Al;

[0015] a≥0.5;

[0016] b+c+d≤0.5; and

[0017] d ≤ 0.1; and

[0018] Each particle includes a coating covering a surface of the particle, wherein the coating comprises a salt of an oxide of a metal selected from vanadium, tantalum and niobium. The agglomerates include particles, wherein the agglomerates include interstitial interfaces. The interstitial interfaces include adjacent coatings on adjacent particles.

[0019] Another embodiment provides an agglomerate comprising particles comprising an oxide defined by the formula:

[0020] LiNi a Mn b X c G d O2

[0021] wherein G is an optional dopant;

[0022] X is Co or Al;

[0023] a≥0.5;

[0024] b+c+d≤0.5; and

[0025] d≤0.1;

[0026] wherein the particles agglomerate to form agglomerates; and

[0027] Coating material between adjacent particles in an agglomerate. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is a schematic diagram of the prior art.

[0029] Figure 2 It is a schematic diagram of the prior art.

[0030] Figure 3 is a schematic illustration of an embodiment of the present invention.

[0031] Figure 4 is a schematic representation of an isolated particle including a coating.

[0032] Figure 5 Graph illustration to illustrate advantages of embodiments of the present invention.

[0033] Figure 6 Graph illustration to illustrate advantages of embodiments of the present invention.

[0034] Figure 7 Graph illustration to illustrate advantages of embodiments of the present invention. DETAILED DESCRIPTION

[0035] The present invention relates specifically to an improved cathode for lithium ion batteries, in particular a high nickel NMC or NCA cathode for lithium ion batteries. More specifically, the present invention relates specifically to a high nickel cathode for lithium ion batteries, comprising a coating on the interstitial interfaces and interstitial surfaces of particles forming agglomerates, wherein the coating inhibits the formation of space charge regions and degradation at the surface.

[0036] In a preferred embodiment, the lithium metal compound of the present invention is defined by the following formula:

[0037] LiNi a Mn b X c G d O2

[0038] wherein G is an optional dopant;

[0039] X is Co or Al;

[0040] a≥0.5;

[0041] b+c+d≤0.5; and

[0042] d≤0.1.

[0043] A preferred embodiment is a high nickel NMC where X is Co, 0.5≤a≤0.9, more preferably 0.58≤a≤0.62, as represented by NMC 622, or 0.78≤a≤0.82, as represented by NMC 811.

[0044] In formulas throughout this specification, lithium is defined stoichiometrically to balance the charge, it being understood that lithium moves between the anode and cathode. Thus, at any given time, the cathode may be relatively lithium-rich, or relatively lithium-poor. In a lithium-poor cathode, the lithium will be below stoichiometric balance, and during charging, the lithium may be above stoichiometric balance. Likewise, in formulas listed throughout this specification, metals are expressed in charge balance, it being understood that the metals may be slightly enriched or slightly depleted, as determined by elemental analysis, since in practice it is impossible to formulate a perfectly balanced stoichiometry. Throughout this specification, specific listed formulas are intended to represent molar ratios of metals to within 10%. For example, for LiNi 0.6 Mn 0.2 Co 0.2 O2, each metal is within 10% of the stoichiometric amount, so Ni 0.6 Represents Ni 0.54 To you 0.66 .

[0045] Dopants may be added to enhance the properties of the oxide (e.g., electronic conductivity and stability). Dopants are preferably alternative dopants added with the initial nickel, manganese and cobalt or aluminum. Dopants are preferably present in an amount not exceeding 10 mol %, and preferably not exceeding 5 mol % in the oxide. Preferred dopants include Al, Gd, Ti, Zr, Mg, Ca, Sr, Ba, Mg, Cr, Cu, Fe, Zn, V, Bi, Nb and B, with Al and Gd being particularly preferred.

[0046] The cathode is formed from an oxide precursor comprising a salt of Li, Ni, Mn, Co, or Al, as described more fully herein. The oxide precursor is calcined to form a cathode material, such as a lithium metal oxide.

[0047] The particles of the cathode material are coated with a metal oxide of niobium, vanadium or tantalum, most preferably lithium niobate (LiNbO3). This coating then provides a passivation effect, especially when using a liquid-based electrolyte (e.g. ethylene carbonate (EC): diethylene carbonate (DEC) 1:1), which prevents degradation and reduces the space charge resistance when using a solid electrolyte.

[0048] refer to Figure 3 One embodiment of the present invention is described, which forms an integral, non-limiting part of the present invention. Figure 3In the embodiment of the invention, agglomerates 16 are schematically illustrated in cross-section. The agglomerates include particles 10, wherein the entire surface of the particles is coated with a protective coating 12. As a result of the entire surface being coated, the following advantages are brought about, namely, the gap interface 14 is an interface comprising a coating, and the gap surface 15 is a surface comprising a coating. If any disturbance disturbs the agglomerate, each particle has a completely coated surface, such as Figure 4 , where fully separated particles are shown with intact surface coatings. Figure 4 While complete separation of the particles is illustrated in the figure, it should be understood that most disturbances expose the surface of the particles or the coating on the particles as in the present invention, but do not necessarily cause complete separation of the particles. For the purposes of illustration and discussion, the coatings of adjacent particles are illustrated as distinct and distinguishable. In actual samples, the coatings may form a uniform layer between adjacent particles, and it is not necessary to distinguish the boundaries defined between the coatings of adjacent particles. In other words, the coatings can be distinguished as different coatings by visual and spectroscopic techniques, or the coatings can appear as a continuum of coating material.

[0049] For the purposes of the present invention, the interstitial interface of an agglomerate is defined as the contact point of adjacent particles, the contact point of the coating of adjacent particles, or the contact point of a particle with the coating of an adjacent particle. For the purposes of the present invention, the interstitial surface of an agglomerate is defined as the surface of a particle or the surface of a particle's coating that is not in contact with an adjacent particle or the coating of an adjacent particle.

[0050] The coating has a thickness of preferably 5 to 10 nanometers over the entire particle.

[0051] In the presence of counterions, the oxide precursor is formed by the reaction of salts, which form relatively insoluble salts. Relatively insoluble salts are believed to form suspended crystals, which are believed to be ripened by Ostwald and eventually precipitated into an ordered lattice. For the purposes of the present invention, preferred manganese and nickel, and optional cobalt or aluminum salts are mixed in a solution containing counterions, and manganese, nickel and cobalt or aluminum are precipitated at a rate sufficient to allow crystal growth. Soluble counterions of manganese, nickel, cobalt or aluminum refer to those having a solubility of at least 0.1 grams of salt per 100 grams of solvent at 20°C, including acetate, nitrate or bicarbonate. The metal is precipitated in the form of an insoluble salt (having a solubility of less than 0.05 grams of salt per 100 grams of solvent at 20°C), including carbonates and oxalates.

[0052] A particular advantage of the present invention is that the materials that form the precursors are added to the coating before the particles form agglomerates, thereby allowing a complete coating to form on the surface of the particles. After drying, the particles will still agglomerate, but the surface of the particles will be pre-coated with the coating, thereby eliminating the formation of uncoated gap interfaces and gap surfaces. In contrast, prior art methods incorporate coating precursors after agglomeration, resulting in the formation of uncoated gap interfaces and gap surfaces. Alternatively, the prior art may rely on the development of coating materials on the surface (bloom), which is not effective in forming a coating at least at the gap interface.

[0053] The entire reaction includes two secondary reactions in sequence. In the presence of excess polycarboxylic acid, the first reaction is the digestion of the carbonate feedstock, as shown in reaction A:

[0054]

[0055] Wherein X represents a metal suitable for cathode materials, preferably selected from Li2, Ni, Mn, Co or Al. In reaction A, the acid is released by the polycarboxylic acid, which is not separately represented in reaction A for simplicity. The result of reaction A is a metal salt in solution, wherein the salt is chelated by the deprotonated polycarboxylic acid, as shown in reaction B:

[0056] X 2+ + - OOCR1COO - →X(OOCR1COO) B

[0057] Where R 1 represents the alkyl chain comprising the polycarboxylate. As discussed elsewhere herein, the salt represented by X(OOCR1COO) precipitates in the form of an ordered crystalline lattice.

[0058] The metal carbonate of reaction A can be replaced by a metal acetate (such as Li(O2CCH3), Ni(O2CCH3)2 or Mn(O2CCH3)2), which can be added in the form of an aqueous solution or a solid material.

[0059] If necessary, the pH can be adjusted with ammonium hydroxide due to its simplicity and improved ability to precisely control the pH. In prior art methods, the use of ammonium hydroxide poses difficulties due to the tendency of NH3 to complex with nickel in aqueous solution, as shown in the reaction:

[0060]

[0061] The result is incomplete precipitation of nickel, which complicates the determination and control of the stoichiometry of the final oxide precursor. Polycarboxylic acids, especially oxalic acid, are preferred over NH4 +Effectively coordinates with nickel, thereby increasing the rate of precipitation and incorporation of nickel into the ordered oxide precursor. Preferential precipitation of the polycarboxylic acid drives the reaction toward nickel precipitation and avoids the use of ammonium hydroxide.

[0062] In the presence of a polycarboxylic acid, the carbonate digestion process comprises mixing a metal carbonate and oxalic acid into a reactor, preferably in the presence of water, followed by stirring. The slurry is then dried, preferably by spray drying, and subsequently calcined. The calcination temperature can vary between 400°C and 1000°C to form materials with different structural properties.

[0063] A particular feature of the carbonate digestion process is that it does not require grinding or blending of precursor powders, filtering of slurries, or decanting of supernatants, although these steps may be performed if desired.

[0064] Taking oxalate as an example, the carbonate digestion process or digestion (hydrolysis)-precipitation reaction can be described by the following reaction equation, which preferably occurs in the presence of water:

[0065] H2C2O 4(aq) +XCO 3(s) →CO 2(g) +H2O (l) +XC2O 4(s,aq) (X = transition metal, Li2)

[0066] Without being bound by theory, it is hypothesized that oxalic acid hydrolyzes carbonate to form CO 2(g) 、H2O (l) and metal ions. The transition metal ions are then precipitated in the form of metal oxalates. The lithium oxalate may precipitate or remain dissolved in the water, depending on the water content. It is contemplated that the soluble lithium oxalate will be coated on the transition metal oxalate particles during the spray-drying process. It is not necessary to achieve complete dissolution of the metal carbonate or oxalic acid, as water is only a medium that digests the metal carbonate and precipitates the metal oxalate in a controlled manner, thereby allowing nucleation and crystal growth. The rate of the digestion (hydrolysis)-precipitation reaction depends on the temperature, water content, pH, gas introduction, crystal structure and morphology of the raw materials.

[0067] The reaction can be carried out at a temperature in the range of 10-100°C, and in one embodiment water reflux temperature is preferred because the digestion reaction rate is increased.

[0068] The water content can vary from about 1 to about 400 mL per 1 g of oxalic acid, with lower water content being preferred because the reaction rate is increased and less water must subsequently be removed.

[0069] The pH of the solution can vary between 0 and 12. A particular advantage of the carbonate digestion process is that the reaction can be carried out without additional pH control, thereby simplifying the process and eliminating the need for additional process controls or additives.

[0070] Although the reaction can be carried out under an untreated atmosphere, other gases (e.g., CO2, N2, Ar, other inert gases, or O2) may be used in some embodiments. In some embodiments, bubbling N2 and CO2 into the solution is preferred because they can slightly increase the crystallinity of the precipitated metal oxalate.

[0071] The crystallinity and morphology of the precursor (eg, amorphous versus crystalline carbonate feedstock) can affect digestion rates due to differences in solubility and particle size and particle size range.

[0072] The carbonate digestion process proceeds via a cascade of equilibria from solid carbonate feedstock to solid oxalate precursor material. For the purposes of discussion but not limitation, the process can be defined by several different processes based on the following reactions:

[0073] (1)H2C2O 4(s) →H2C2O 4(aq) (Dissolution of oxalic acid)

[0074] (2)H2C2O 4(aq) ←→H + (aq) +HC2O4 - (aq) (Oxalic acid dissociation step 1, pK a =1.25)

[0075] (3) HC2O4 - (aq) ←→H + (aq) +C2O4 2- (aq) (Oxalic acid dissociation step 2, pK a =4.19)

[0076] (4)XCO 3(s,aq) +2H + (aq) →X 2+ +H2O (l) +CO 2(g) (Carbonate Hydrolysis)

[0077] (5)X 2+ (aq) +C2O4 2- (aq) →XC2O 4(s) (Precipitation of Metal Oxalates)

[0078] The reactions are written out step by step for the purpose of discussion and explanation, it being understood that under the operating reaction conditions, the reactions may occur simultaneously. By varying various reaction parameters (e.g., water content / ionic strength, excess oxalic acid content, batch size, temperature, atmosphere, reflux reaction mixture, pH control, etc.), the rate of each step can be controlled, and other desired parameters (e.g., solid content) can be optimized.

[0079] The carbonate digestion process can be described as a cascade equilibrium in which CO 2(g) Release from solution, as described above in reaction 4, and precipitation of highly insoluble metal oxalates, as described above in reaction 5. Both CO2 release and precipitation drive the reactions to completion.

[0080] The rate of carbonate hydrolysis is related to the K of metal carbonates sp Related, the following are provided for convenience:

[0081] Lithium carbonate, Li2CO3, 8.15×10 -4 , very fast (seconds to minutes);

[0082] Nickel(II) carbonate, NiCO3, 1.42×10 -7 , fast (a few minutes);

[0083] Manganese(II) carbonate, MnCO3, 2.24×10 -11 , slower (hours to days); and

[0084] Aluminum hydroxide, Al(OH)3, 3×10 -34 , very slowly.

[0085] The uniformity of the coprecipitation may depend on the rate of carbonate hydrolysis. For example, if nickel(II) carbonate is completely hydrolyzed before manganese(II) carbonate, it may subsequently precipitate as NiC2O4 and MnC2O4, respectively.

[0086] Temperature can be controlled because it affects the rate of oxalic acid dissolution, carbonate hydrolysis, and metal oxalate precipitation. In particular, it is useful to conduct the reaction at the reflux temperature of the water. The reaction produces CO 2(g) , increasing temperature will increase CO 2(g) The removal rate of CO 2(g) The water solubility of carbonates is low, and increasing the temperature may increase the rate of carbonate hydrolysis.

[0087] Bubbling can also be an effective method to control the rate of the reaction by changing the rate of CO2 release. 2(g) , O 2(g) , CO 2(g)Bubbling of the atmosphere and / or air may be beneficial as these gases can displace dissolved CO 2(g) Or improve the mixing of reactants.

[0088] If carbonates are first present as metastable bicarbonates, they can be digested more quickly. For example, Li2CO3 undergoes the following reaction:

[0089] Li2CO 3(s) +CO 2(g) +H2O (l) ←→2LiHCO 3(aq)

[0090] Metastable lithium bicarbonate is far more soluble than Li2CO3, and subsequent hydrolysis can proceed stoichiometrically with a single proton as follows:

[0091] LiHCO 3(aq) +H + (aq) →H2O (l) +CO 2(g) +Li + (aq)l

[0092] Rather than proceeding as in reaction 4 above.

[0093] Divalent metal oxalates (e.g., NiC2O4, MnC2O4, CoC2O4, ZnC2O4, etc.) are highly insoluble, however, monovalent metal oxalates (e.g., Li2C2O4) are soluble to some extent, with a solubility of 8 g / 100 mL in water at 25° C. If it is desired to have lithium oxalate in solution and evenly dispersed in the mixed metal oxalate precipitate, it may be advantageous to maintain the water volume above the solubility limit of the lithium oxalate.

[0094] The rate of carbonate hydrolysis, metal oxalate precipitation, and the crystal structure and particle size of the metal oxalate precipitate are affected by pH and water content or ionic strength. In some embodiments, it may be beneficial to work at higher ionic strength or lower water content because this increases the proton activity of oxalic acid and the precipitation rate of metal oxalate. The water content can be normalized to the carbonate feed content, and the preferred ratio of the number of moles of carbonate to the volume (L) of water is in the range of about 0.05 to about 20. A water content of about 1.64 L per 1.25 moles of carbonate provides a ratio of the number of moles of carbonate to the volume (L) of water of 1.79, which is suitable for demonstration of the present invention.

[0095] A stoichiometric amount of oxalate to carbonate is sufficient to achieve complete precipitation. However, adding excess oxalic acid can increase the reaction rate because the second proton on oxalic acid is much less acidic and participates in the hydrolysis. About 5% excess oxalic acid on a molar basis to carbonate is sufficient to ensure complete hydrolysis of the carbonate. Inductively coupled plasma mass spectrometry (ICP) analysis showed that a 10% excess of oxalic acid leaves a similar number of Mn / Ni ions in solution as a 0% stoichiometric excess by the time the reaction is complete. A small stoichiometric excess of oxalic acid should be effective to achieve complete precipitation, however, a lower stoichiometric excess may affect the rate of carbonate hydrolysis.

[0096] A particular advantage of the carbonate digestion process is the ability to carry out the entire reaction to completion in a single reactor. Since the lithium source is ideally in solution prior to the spray drying and calcination steps, it may be useful and / or possible to precipitate the transition metal separately and add the lithium source in the form of an aqueous lithium salt solution (e.g., oxalate) after co-precipitation.

[0097] A coating metal precursor salt (wherein the metal will not be incorporated into the crystal lattice) can be added after digestion to ultimately form a metal oxide coating comprising vanadium, tantalum or niobium. A particularly preferred metal is niobium, and a particularly preferred niobium precursor as a coating metal precursor salt is a dicarboxylate, most preferably an oxalate. The preferred niobium oxalate can be formed in situ from niobium carbonate, or the niobium oxalate can be prepared separately and added to the cathode metal precursor. Preferably, the coating comprises primarily a lithium salt (e.g., lithium niobate) coating material, wherein at least 95 mole percent of the coating is a lithium salt of the coating metal oxide or less than 5 mole percent of the metal ions in the coating are lithium salts of the active cathode material. In a particularly preferred embodiment, the metal in the coating is at least 95 mole percent lithium niobate.

[0098] The present invention is applicable to the use of transition metal acetates and mixed carbonate feedstocks to more closely match the solubility of the metal complexes. Consider using a mixed carbonate feedstock (e.g. Ni 0.25 Mn 0.75 CO3+Li2CO3) to produce LiNi 0.5 Mn 1.5 O4 material. Raw material impurities may be critical to the properties of the final material. In particular, MnCO3 samples may contain small amounts of unknown impurities that are not hydrolyzed during the reflux process.

[0099] Polycarboxylic acid comprises at least two carboxyl groups. Particularly preferred polycarboxylic acid is oxalic acid, partly because the carbon that must be removed in the calcination process is minimum. Other low molecular weight dicarboxylic acids can be used, such as malonic acid, succinic acid, glutaric acid and adipic acid. Higher molecular weight dicarboxylic acids can be used, particularly those with an even number of carbons of higher solubility, but the necessity of removing extra carbon and the solubility of reduction make them less ideal. Other acids can be used, such as citric acid, lactic acid, oxaloacetic acid, fumaric acid, maleic acid and other polycarboxylic acids, provided that they have enough solubility to realize at least a small amount of stoichiometric excess and have enough chelating properties. It is preferred not to use the acid with hydroxyl, because of the hygroscopicity they improve.

[0100] To complete the reaction to form the oxide precursor, a solution of the starting salt is prepared. An additive solution is preferably prepared jointly, individually or in some combination, preferably comprising a solution of nickel, manganese and cobalt or aluminum, and a bulk solution preferably comprising lithium. The additive solution comprising the metals is then added to the bulk solution as described elsewhere herein. The order of the solutions may be reversed, however, it is preferred to add the transition metals in the desired stoichiometry, and therefore it is advantageous to add a single solution comprising all transition metals to the bulk solution comprising lithium.

[0101] Each solution is prepared by dissolving the solid in a selected solvent, preferably a polar solvent (e.g., water), but not limited thereto. The choice of solvent depends on the solubility of the solid reactant in the solvent and the temperature of dissolution. It is preferred to dissolve at ambient temperature and at a fast rate so that dissolution is not energy-intensive. Dissolution can be carried out at a slightly higher temperature, but preferably below 100°C. Other dissolution aids may be acid or base additives.

[0102] During mixing, it is preferred to bubble the gas into the bulk solution. For the purpose of discussion, a gas is defined as inert, which does not contribute to the chemical reaction; or a gas is defined as reactive, which either adjusts the pH or contributes to the chemical reaction. Preferred gases include air, CO2, NH3, SF6, HF, HCl, N2, helium, argon, methane, ethane, propane, or mixtures thereof. Particularly preferred gases include ambient air unless the reactant solution is sensitive to air. If a reducing atmosphere is required, carbon dioxide is particularly preferred, and if carbonates are formed, carbon dioxide can also be used as a solvent, pH regulator, or reactant. Ammonia can also be introduced as a gas for adjusting pH. Ammonia can form ammonia complexes with transition metals and help dissolve such solids. As an example, a gas mixture (e.g., 10% O2 in argon) can be used.

[0103] For forming the oxide precursor, the pH is preferably at least about 1 and no more than about 9.6, but is not limited thereto. Ammonia or ammonium hydroxide is suitable for raising the pH, as is any soluble base for adjustment (LiOH is particularly preferred). Acids, particularly formic acid, are suitable for lowering the pH, as is desired. In one embodiment, lithium may be added prior to drying, for example by adding lithium acetate to obtain a sufficient solids content, typically about 20 to 30 wt%.

[0104] A particular advantage of the present invention is the ability to form a gradient of transition metal concentration throughout the oxide body, wherein each region (e.g., the center) may have a ratio of one transition metal, and the ratio may vary through the oxide body in a continuous or step-wise manner. Considering NMC for purposes of discussion and clarity, but not limited thereto, the concentrations of Ni, Mn, and Co may vary radially from the core of the particle to the surface. In an exemplary embodiment provided for clarity, the Ni content may be gradient, such that there is a relatively low nickel concentration on or near the surface of the oxide particle and a relatively high nickel concentration in the core of the oxide particle. Based on a neutral stoichiometry, the ratio of lithium to transition metal will remain constant throughout the oxide particle. For example, for NMC 622 and NMC 811, the overall composition of Ni:Mn:Co may be 6:2:2 and 8:1:1, respectively, wherein the core is relatively enriched in one transition metal and the shell is relatively depleted in the same transition metal. Even more specifically, the core may be enriched in one transition metal, such as nickel, with the ratio of the transition metal decreasing radially relative to the other transition metals. As a non-limiting stepwise example, a core of NMC 8:1:1 may have a shell of NMC 6:2:2 on the outside and a shell of NMC 1:1:1 on the outside. These reactions may be performed in a stepwise addition or in a continuous gradient by varying the pump rate of the transition metal. The ratio of each transition metal addition and the number of additions may be varied to obtain the desired gradient profile.

[0105] A particular feature of the present invention is the ability to preferentially incorporate dopants and other materials into the interior of the oxide or toward or even on the surface. In the case of the prior art, the dopant is, for example, uniformly dispersed in the oxide. In addition, any surface treatment (such as aluminum) is as a surface reactant on the formed oxide, and not necessarily incorporated as atoms into the oxide lattice. The present invention allows the dopant to be systematically dispersed in the core, as is the case when the dopant is incorporated into the initial transition metal slurry, dispersed in radial bands, as is the case when the dopant is incorporated into the subsequent transition metal slurry, or dispersed in the shell, as is the case when the dopant is incorporated into the final transition metal slurry.

[0106] For the purposes of the present invention, each radial portion of the oxide particle will be defined based on the percentage of transition metal used to form that portion. For example, if the initial slurry has a first proportion of transition metal, and the initial slurry includes 10 mol% of the total transition metal used to form the oxide, the core will be considered to be 10% of the volume of the oxide, and the composition of the core will be defined as having the same proportion as the first proportion of transition metal. Similarly, each shell surrounding the core will be defined by the percentage of transition metal therein. As a non-limiting example, an oxide precursor formed with three slurries, each slurry having an equimolar transition metal, wherein the first slurry has a Ni:Mn:Co ratio of 8:1:1, the second slurry has a Ni:Mn:Co ratio of 6:2:2, and the third slurry has a Ni:Mn:Co ratio of 1:1:1, it will be considered that the oxide precursor forms an oxide in which 1 / 3 of the volume of the oxide particles represents a core with a transition metal ratio of 8:1:1, the first shell on the core represents 1 / 3 of the volume of the oxide particles with a transition metal ratio of 6:2:2, and the outer shell on the first shell represents 1 / 3 of the volume of the oxide particles with a transition metal ratio of 1:1:1, without considering transition metal migration that may occur during sintering of the precursor to the oxide.

[0107] In a particularly preferred embodiment, the dopant is incorporated into a shell within the coating, the particular dopant being aluminum. More preferably, the shell comprising the dopant is less than 10% of the volume of the oxide particles, even more preferably less than 5% of the volume of the oxide particles, and most preferably not more than 1% of the volume of the oxide particles. For the purposes of the present invention, the dopant is defined as a material that is precipitated with at least one transition metal selected from Ni, Mn, Co, Al and Fe during the formation of a precursor for the oxide. More preferably, the precursor for the oxide comprises Ni and Mn and optionally Co or Al. In this context, materials that are added after the precipitation of at least one transition metal is complete are defined as surface treatments, with niobium, in particular lithium niobate, being preferred.

[0108] After the reaction to form the oxide precursor is completed, the resulting slurry mixture is dried to remove the solvent and obtain a dried precursor powder. Any type of drying method and equipment can be used, including spray dryers, tray dryers, freeze dryers, etc., selected according to the preferred final product. The drying temperature is determined and limited by the equipment used, and this type of drying is preferably below 350°C, more preferably 200-325°C. An evaporator can be used for drying so that the slurry mixture is placed in a tray and the solvent is released as the temperature increases. Any evaporator used in industrial applications can be used. A particularly preferred drying method is a spray dryer with a fluidizing nozzle or a rotary atomizer. These nozzles preferably have a minimum size diameter suitable for the size of the oxide precursor in the slurry mixture. For cost considerations, the drying medium is preferably air.

[0109] The particle size of the oxide precursor is nanometer-sized primary and secondary particles and up to smaller micrometer-sized secondary particles or agglomerates, which range less than 50 microns, and these agglomerates are very easy to crush to smaller sizes. It should be understood that the composition of the final powder will also affect the morphology. The particle size of the oxide precursor is preferably about 1-5 μm. If a spray dryer, freeze dryer or the like is used, the resulting mixture is continuously stirred as it is pumped into the spray dryer head. For a disk dryer, the liquid evaporates from the surface of the solution.

[0110] The dried powder is transferred to the calcining system in batches or by conveyor belt. In large-scale production, this transfer can be continuous or batch. The calcining system can be a box furnace using a ceramic tray or sagger as a container, a rotary calcining furnace, a fluidized bed (which can be co-current or countercurrent), a rotary tube furnace and other similar equipment, but is not limited thereto.

[0111] The heating and cooling rates during calcination depend on the type of end product desired. Generally, a heating rate of about 5°C per minute is preferred, but typical industrial heating rates are also suitable.

[0112] The final powder obtained after the calcination step is a fine powder, ultrafine powder or nano-sized powder, which may not require additional crushing, grinding or milling as currently done in conventional processing. The particles are relatively soft and do not sinter as in conventional processing.

[0113] The final calcined oxide powder is preferably characterized by surface area, particle size (by electron microscopy), porosity, elemental chemical analysis, and preferably property testing as required for a specific application.

[0114] The spray dried oxide precursor is preferably very fine and nano-sized.

[0115] The spray dryer collector can be modified so that the outlet valve opens and closes as the spray powder is transferred to the calciner. The spray dried powder in the collector can be transferred in batches to trays or saggers and then moved to the calciner. A rotary calciner or a fluidized bed calciner can be used to illustrate the present invention. The calcination temperature is determined by the composition of the powder and the desired final phase purity. For most oxide type powders, the calcination temperature ranges from as low as 400°C to slightly above 1000°C. After calcination, the powder is screened because these powders are soft and unsintered. The calcined oxide does not require long grinding or classification to obtain a narrow particle size distribution.

[0116] The preferred crystallite size of the LiMO2 forming agglomerates is about 50-250 nm, more preferably about 150-200 nm.

[0117] A particular advantage of the present invention is the formation of metal chelates of polycarboxylic acids rather than acetates. Acetates act as combustion fuel during the subsequent calcination of the oxide precursor and require additional oxygen for complete combustion. Lower molecular weight polycarboxylic acids, particularly lower molecular weight dicarboxylic acids, and more particularly oxalic acid, decompose at lower temperatures without the introduction of additional oxygen. For example, oxalates decompose at about 300°C without the need for additional oxygen, thereby enabling more accurate control of the calcination temperature.

[0118] This method of forming an oxide precursor is referred to herein as the complex precursor formulation (CPF) method, which is suitable for large-scale industrial production of high-performance fine, ultrafine and nano-sized powders that require defined unique chemical and physical properties that are essential to meet the performance specifications of specialized applications. The CPF method provides an oxide precursor in which the metal is precipitated as an ordered lattice in the form of a salt. The oxide precursor is then calcined to form the oxide. Although not limited to theory, it is hypothesized that the formation of an ordered lattice, as opposed to an amorphous solid, promotes oxide formation during calcination.

[0119] The CPF process provides controlled formation of specialized micro- or nanostructures, and a final product with particle size, surface area, porosity, phase purity, chemical purity, and other necessary properties tailored to meet performance specifications. Powders produced by the CPF process are obtained with a reduced number of processing steps relative to currently used technologies and can utilize currently available industrial equipment.

[0120] The CPF method is applicable to any inorganic powder and organometallic powder with electrophilic or nucleophilic ligands. The CPF method can use low-cost raw materials as starting materials, and additional purification or separation can be performed in situ if necessary. The inert or oxidizing atmosphere conditions required for powder synthesis can be easily achieved using equipment for this method. The reaction temperature can be ambient temperature or slightly warm, but preferably does not exceed 100°C.

[0121] The CPF method produces fine, ultrafine and nanosized powders of precursor oxides in a simple and efficient manner by integrating the chemical principles of crystallization, solubility, transition complex formation, phase chemistry, acid-base, aqueous chemistry, thermodynamics and surface chemistry.

[0122] When crystallization begins, especially when the nucleation step begins, it is the most critical stage to form nano-sized powders. A special advantage that CPF provides is that nano-sized particles can be prepared at the beginning of this nucleation step. The solute molecules from the starting reactants are dispersed in a given solvent and are in solution. In this case, it is believed that under suitable temperature, supersaturation and other conditions, clusters begin to form on a nanoscale. These clusters constitute the core, in which atoms begin to arrange themselves in a limited and periodic manner, which subsequently limits the microstructure of the crystal. The size and shape of the crystal are the macroscopic properties of the crystal derived from the internal lattice structure.

[0123] After nucleation begins, crystal growth also begins, and as long as supersaturation exists, nucleation and crystal growth can occur simultaneously. The rates of nucleation and growth are determined by the existing supersaturation in the solution, and the occurrence of nucleation or growth depends on the supersaturation state. In order to adjust the crystal size and shape, it is crucial to define the concentration of the reactants required accordingly. If nucleation is dominant over growth, smaller crystal sizes will be obtained. The nucleation step is a very critical step, and the reaction conditions of this initial step determine the crystals obtained. By definition, nucleation is an initial phase transition in a small area, such as the formation of crystals from a liquid solution. It is the result of rapid local fluctuations on a molecular scale in a homogeneous phase in a metastable equilibrium state. Total nucleation is the sum of two types of nucleation - primary and secondary. In primary nucleation, crystals are formed in the absence of a crystal as an initiator. Secondary nucleation occurs when a crystal is present to initiate the nucleation process. It is this consideration of the importance of the initial nucleation step that forms the basis of the CPF method.

[0124] In the CPF process, the reactants are preferably dissolved in solution at ambient temperature, or if necessary at a slightly elevated temperature but preferably not exceeding 100°C. The selection of inexpensive raw materials and suitable solvents is an important aspect of the present invention. The purity of the starting materials is also important because this will affect the purity of the final product, which may require a specified purity level required for its performance specifications. In this regard, low-cost starting materials that can be purified during the preparation process without significantly increasing processing costs must be considered.

[0125] The CPF uses conventional equipment to intimately mix the reactants, and preferably involves a highly agitated mixture, preferably with gas sparging, particularly where reactant gases are advantageous.

[0126] Preferably, the gas is directly introduced into the solution, and there is no restriction on the method for introducing. Gas can be introduced into the solution in the reactor by arranging a plurality of gas diffusers (e.g., pipes) on the side of the reactor, wherein the pipe has a hole for gas outlet. Another configuration is to have a double-walled reactor so that the gas passes through the inner wall of the reactor. The bottom of the reactor may also have a gas inlet. The gas may also be introduced by a stirring shaft to produce bubbles when leaving. Several other configurations are possible, and the description of these arrangements provided herein is not limited thereto.

[0127] In one embodiment, an aerator can be used as a gas diffuser. The gas diffusion aerator can be incorporated into the reactor. Tubular or dome-shaped ceramic diffusion aerators are particularly suitable for demonstrating the present invention. The pore structure of the ceramic bubble diffuser can produce relatively fine small bubbles, resulting in an extremely high gas-liquid interface per cubic foot per minute (cfm) of supplied gas. The high gas-liquid interface ratio plus the increased contact time due to the slow fine bubble rate can provide a higher transfer rate. The porosity of the ceramic is a key factor in the formation of bubbles and contributes significantly to the nucleation process. Although not limited to this for most configurations, a gas flow rate of at least one liter of gas per liter of solution per minute is suitable for demonstrating the present invention.

[0128] Ceramic tube gas diffusers on the side of the reactor wall are particularly suitable for demonstrating the present invention. Several of these tubes can be placed in different locations, preferably equidistant from each other, to more evenly distribute the gas throughout the reactor. The gas is preferably introduced into the diffuser inside the reactor through a fitting connected to a header assembly (which slightly pressurizes the chamber of the tube). As the gas permeates through the ceramic diffuser body, fine bubbles may begin to form due to the porous structure of the material and the surface tension of the liquid outside the ceramic tube. Once the surface tension is overcome, tiny bubbles are formed. The small bubbles then rise through the liquid, forming an interface for transfer between the gas and the liquid before reaching the surface of the liquid.

[0129] The dome-shaped diffuser can be placed at the bottom of the reactor or at the side of the reactor. With a dome-shaped diffuser, a plume of bubbles is usually produced that continuously rises from the bottom to the surface, providing a large reactive surface.

[0130] A membrane diffuser that closes when the airflow is insufficient to overcome the surface tension is suitable for demonstrating the present invention. This is useful to prevent any product powder from being lost into the diffuser.

[0131] In order to have higher gas efficiency and utilization, it is preferred to reduce gas flow and pressure and consume less pumping energy. The diffuser can be configured to form smaller bubbles with higher surface area for the same volume of gas compared to forming fewer larger bubbles. A larger surface area means that the gas dissolves faster in the liquid. This is advantageous in solutions where the gas also serves to solubilize the reactants by increasing their solubility in the solution.

[0132] Nozzles, preferably one-way nozzles, can be used to introduce gas into the solution reactor. A pump can be used to deliver the gas, and the flow rate should be controlled to achieve the desired bubbles and bubble rate. Nozzle diffusers (preferably on at least one side or bottom of the reactor) are suitable for demonstrating the present invention.

[0133] The rate at which the gas is introduced is preferably sufficient to increase the volume of the solution by at least 5%, excluding the effect of the agitator. In most cases, at least about one liter of gas per liter of solution per minute is sufficient to demonstrate the present invention. The gas is preferably recycled back to the reactor.

[0134] The additive solution is preferably transferred to the main solution using a pipe connected to a pump, which connects the solution to be transferred to the reactor. The pipe entering the reactor is preferably a single orifice or multiple orifices with a selected predetermined internal diameter, so that the diameter size can deliver the stream of the additive solution at a given rate. An atomizer with a fine nozzle is suitable for delivering the additive solution to the reactor. The end of this transfer pipe can include a nozzle, thereby providing a plurality of streams of additive solutions simultaneously. In large-scale production, the speed of transfer is a time factor, so the transfer rate should be fast enough to produce the required correct size.

[0135] The agitator can be equipped with a plurality of propellers of different configurations, each group including one or more propellers placed at an angle to each other or in the same plane. In addition, the mixer can have one or more groups of these propellers. The goal is to create enough turbulence for sufficient solution turnover. Straight or oblique propellers are applicable. The size and design of these propellers determine the type of solution flow and the direction of flow. Speeds of at least about 100 revolutions per minute (rpm) are suitable for demonstrating the present invention.

[0136] The rate of transfer of the added solution to the main solution has a kinetic effect on the rate of nucleation. The preferred method is to have a fine transfer flow to control the local concentration of reactants that affect nucleation and the rate of nucleation exceeds the crystal growth rate. For smaller sized powders, slower transfer rates will produce finer powders. The appropriate conditions for competitive nucleation and growth must be determined by the desired final powder properties. The temperature of the reaction is preferably ambient temperature, or at a mild temperature if necessary.

[0137] Specific nanostructures are preformed to bring these structures into the final product, thereby enhancing the performance of the material in the desired application. For the purposes of this invention, nanostructures are defined as structures with primary particles having an average size of 100 to 300 nm.

[0138] Neither surfactants nor emulsifiers are necessary. In fact, it is preferred that surfactants and emulsifiers are not used because they inhibit drying.

[0139] Size control can be achieved by the concentration of the solution, the flow rate of the gas, or the transfer rate of the additive solution into the bulk solution.

[0140] No repetitive and tedious grinding and sorting steps are used.

[0141] Reduced calcination times can be achieved, and repeated calcinations are generally not necessary.

[0142] The reaction temperature is ambient temperature. If solubilization is required, the temperature is increased, but preferably does not exceed 100°C.

[0143] The tailored physical properties of the powders (eg, surface area, porosity, tap density, and particle size) can be carefully controlled by selecting reaction conditions and starting materials.

[0144] The method is readily scalable for large-scale manufacturing using currently available equipment and / or retrofitting of existing industrial equipment.

[0145] It is generally believed that in the prior art, the morphology of cathode materials includes dense polycrystalline spheres with diameters between 3 and 30 μm, and these spheres are compressed into cathode layers on aluminum foil to make electrodes for lithium-ion batteries with additional carbon and a binder (such as PVDF). The electrode layer is typically calendered to a porosity of about 30% to allow the electrolyte (such as 1M LiPF6 in EC / DEC 30 / 70) to form an interface with the surface of the cathode material. Generally, it is necessary to (i) coat these spheres to prevent side reactions such as electrolyte oxidation and transition metal dissolution, and (ii) reduce the surface area by optimizing the size of the spheres. Packing these spheres into the electrode layer requires optimizing the surface area to improve performance and durability.

[0146] The methods described herein produce cathode materials with different morphologies that can be optimized for improved performance and durability. The cathode materials include cathode material nanocrystals containing lithium transition metal oxides of the general formula LiMO2 or LiM2O4, wherein each individual nanocrystal is doped and coated with a protective layer comprising a second metal oxide that prevents undesirable side reactions while not interfering with the Li +The coated nanocrystals form agglomerates of similar average size to the prior art but porous in the process, which allows a larger interface between the electrode and the electrolyte while being protected from side reactions by the second oxide coating described above. This difference in morphology means that electrodes calendered to similar porosity or pore volume will have different pore size distributions (PSDs), with a significant proportion of the pore volume comprising micropores.

[0147] When prior art materials, including hard, dense, polycrystalline, coated spheres, are rolled in the formation of electrodes, it is feared that these spheres may break, exposing unprotected cathode materials. This may also occur in the process of volume changes during the battery charge / discharge cycle in normal use. Both of these effects will have an adverse effect on the durability of battery performance. In the technology described herein, the agglomerate secondary particles can be compressed and even broken during rolling without exposing unprotected cathode materials, because each individual nanocrystal is coated. In addition, the microporosity produced by the described morphology increases the electrode / electrolyte interface, which can achieve high charge and discharge rates without adversely affecting durability. The coating of the individual nanocrystals means that there is no need to reduce the active surface of the electrode to impart sufficient durability, and the overall performance of the battery will be significantly improved.

[0148] Example

[0149] Electrode preparation:

[0150] The composite electrode was prepared by mixing the active material with 10 wt% conductive carbon black (as a conductive additive), 5 wt% polyvinylidene fluoride (PVDF, as a binder) and dissolving in N-methyl-2-pyrrolidone (NMP) solvent. The slurry was cast on graphite-coated aluminum foil and dried in vacuum at 60 °C overnight. -2 The typical loading area on the electrode sheet is 1.54cm 2 The electrode disk.

[0151] Button battery assembly:

[0152] The coin cells were assembled in an argon-filled glove box. Lithium foil (340 μm) was used as the counter electrode and reference electrode in the half-cell, and commercial Li4Ti5O 12 The (LTO) composite electrode was used as the counter electrode and reference electrode in the full cell. 1M LiPF6 was used as the electrolyte in ethylene carbonate (EC): diethylene carbonate (DEC) 7:3 (vol%). The electrode in the half cell consisted of one or two 25 μm thick The cells are separated by a Celgard membrane in the full cell.

[0153] Cycling protocol:

[0154] Using an Arbin Instrument battery tester (model BT 2000), the battery was tested at 25°C in the voltage range of 3.5-4.9 V at different C-rates (1 C rate is equivalent to 146 mA g -1 ) constant current cycled cathode cells. At the end of the constant current charging step at 1C or higher rate, a constant voltage charging step of 4.9V was applied to the cells for 10 minutes. The rock salt NMC cells were cycled at 25°C at different C-rates (1C rate is equivalent to 200mAg -1 ) Constant current cycling. At the end of the constant current charging step at 1C or higher rate, a constant voltage charging step of 4.35V was applied to the battery for 10 minutes.

[0155] Comparative Example 1

[0156] With the formula LiNi 0.8 Mn 0.1 Co 0.1 The precursor of NMC 811 of O2 was prepared from 39 g Li2CO3, 95 g NiCO3, 12 g MnCO3 and 12 g CoCO3 dispersed in 200 mL deionized water in a beaker. The mixture was pumped into a separate beaker containing 201 g H2C2O4·2H2O in 400 mL deionized water at a rate of 0.38 mol carbonate per hour. The reaction mixture was then stirred for 1 h. The final mixture with a solid content of about 20% was spray dried to obtain a LiNi 0.8 Mn 0.1 Co 0.1 (C2O4) 1.5 The precursor was heated at 600°C for 5 h in air in a box furnace, heated at 125°C for 1 h under an oxygen flow, and calcined at 830°C for 15 h in a tube furnace under an oxygen flow to obtain NMC 811. NMC 811 was heated at 125°C for 1 h and calcined at 830°C for 15 h in a tube furnace under an oxygen flow to form re-fired NMC811, referred to herein as "original NMC 811".

[0157] Invention Example 1:

[0158] With the formula LiNi 0.8 Mn 0.1 Co 0.1The precursor of NMC 811 for O2 was prepared by adding 0.267 mol of nickel (II) carbonate hydrate (Alfa Aesar, 99.5% metal basis), 0.1 mol of cobalt (II) carbonate (Alfa Aesar, 99% metal basis) and 0.1 mol of manganese (II) carbonate (Sigma Aldrich ≥ 99.9% metal basis) and 0.525 mol of lithium carbonate (Alfa Aesar, 99%) to 200 mL of deionized water and stirring for 30 minutes to prepare a carbonate slurry. In a separate beaker, 1.617 mol of oxalic acid dihydrate was added to 400 mL of deionized water and stirred for 30 minutes. The carbonate slurry was added dropwise to the oxalic acid dihydrate mixture over 5 hours and stirred for another 18 hours to prepare an oxalate slurry.

[0159] The coating solution was prepared by adding 0.005 moles of niobium (V) oxalate hydrate (Alfa Aeser) and stirring overnight. The coating solution was added to the oxalate slurry and then stirred for another 2 hours before spray drying. The resulting powder was fired at 830°C in a tube furnace under an oxygen flow for 15 hours. The powder was ground to a sieve particle size of ≤45 μm and vacuum sealed in an aluminum bag. The resulting powder is referred to herein as 1-pot coated NMC811.

[0160] The electrical properties of Inventive Example 1 and Comparative Example 1 were characterized. Inventive Example 1 showed improved discharge capacity after repeated cycles, as shown in the representative Figure 5 As shown in the figure, the expected normalized discharge capacity is Figure 6 The expected improvement in rate performance of the embodiments of the present invention is shown in the representative Figure 7 In the description.

[0161] Comparative Example 2

[0162] With the formula LiNi 0.6 Mn 0.2 Co 0.2 The precursor of NMC 622 of O2 was prepared from 39g Li2CO3, 71g NiCO3, 23g MnCO3 and 24g CoCO3 dispersed in 200mL deionized water in a beaker. The mixture was pumped into a separate beaker containing 201g H2C2O4·2H2O in 400mL deionized water at a rate of 0.38 mol carbonate per hour. The reaction mixture was then stirred for 1h. The final mixture with a solid content of about 20% was spray dried to obtain a LiNi 0.6 Mn 0.2 Co 0.2 (C2O4) 1.5The precursor was heated at 110°C for 1 h and calcined in a box furnace at 800°C for 7.5 h in air to obtain NMC 622.

[0163] Invention Example 2:

[0164] With the formula LiNi 0.6 Mn 0.2 Co 0.2 The precursor of NMC 622 of O2 was prepared from 39 g Li2CO3, 71 g NiCO3, 23 g MnCO3 and 24 g CoCO3 dispersed in 200 mL deionized water in a beaker. The mixture was pumped into a separate beaker containing 201 g H2C2O4·2H2O in 400 mL deionized water at a rate of 0.38 mol carbonate per hour. The reaction mixture was then stirred for 1 h.

[0165] The coating was prepared by adding 3.2 g of niobium (V) oxalate hydrate to the reaction mixture and stirring for another 2 hours. The final mixture with a solid content of about 20% was spray dried to obtain a precursor. The precursor was heated at 110°C for 1 h and calcined at 800°C in air for 7.5 h in a box furnace to obtain one-pot coated NMC 622.

[0166] Comparative Example 3:

[0167] With the formula LiNi 0.8 Co 0.15 Al 0.05 The precursor of NCA of O2 was prepared by dispersing 39g Li2CO3, 95g NiCO3, 8g Al(OH)(CH3COO)2 and 18g CoCO3 in 200mL deionized water in a beaker. The mixture was pumped into a separate beaker containing 201g of oxalic acid hydrate in 400mL deionized water at a rate of 0.38 mol carbonate per hour. The reaction mixture was stirred for 1h. The precursor was heated at 125°C for 1h and then calcined at 830°C for 15h in a tube furnace under an oxygen flow to obtain NCA.

[0168] Invention Example 3:

[0169] With the formula LiNi 0.8 Co 0.15 Al 0.05The precursor of NCA of O2 was prepared from 39 g Li2CO3, 95 g NiCO3, 8 g Al(OH)(CH3COO)2 and 18 g CoCO3 dispersed in 200 mL deionized water in a beaker. The mixture was pumped into a separate beaker containing 201 g oxalic acid hydrate in 400 mL deionized water at a rate of 0.38 mol carbonate per hour and then stirred for 1 h.

[0170] The coating was prepared by adding 3.2 g of niobium (V) oxalate hydrate to the reaction mixture and stirring for another 2 hours. The final mixture with a solid content of about 20% was spray dried to obtain a precursor. The precursor was heated at 125°C for 1 h and then calcined at 830°C for 15 h in a tube furnace under an oxygen flow to obtain a pot-coated NCA.

[0171] The present invention has been described with reference to preferred embodiments, but the present invention is not limited thereto. Those skilled in the art will recognize additional embodiments and modifications not specifically described herein but within the scope of the present invention as more particularly described in the appended claims.

Claims

1. An improved cathode material for a lithium-ion battery, comprising: Particles comprising an oxide defined by the formula: LiNi a Mn b X c G d O2 wherein G is an optional dopant; X is Co or Al; a≥0.5; b+c+d≤0.5; and d ≤ 0.1; and Each particle of the particles comprises a surface and a coating covering the entire surface, wherein the coating comprises a salt of an oxide of a metal selected from the group consisting of vanadium, tantalum, and niobium; an agglomerate comprising said particles, wherein said agglomerate comprises interstitial interfaces between adjacent said particles, wherein said interstitial interfaces comprise adjacent coatings on said adjacent said particles; The improved cathode material is calcined from an oxide precursor containing a salt of Li, Ni, Mn, Co or Al; and Before the particles form the agglomerates, a salt of Li, Ni, Mn, Co or Al forming an oxide precursor is added to the coating.

2. The improved cathode material for a lithium ion battery of claim 1, wherein said agglomerates further comprise interstitial surfaces, wherein said interstitial surfaces comprise said coating on each of said particles.

3. The improved cathode material for lithium ion batteries according to claim 1, wherein each of the coating layers has a thickness of 5 to 10 nanometers.

4. The improved cathode material for a lithium ion battery according to claim 1, wherein each of said coatings comprises LiNbO3.

5. The improved cathode material for lithium ion batteries according to claim 1, wherein the subscript a is defined by the equation 0.5≤a≤0.

9.

6. The improved cathode material for lithium ion batteries according to claim 5, wherein the subscript a is defined by the equation 0.58≤a≤0.62 or by the equation 0.78≤a≤0.

82.

7. The improved cathode material for lithium ion batteries according to claim 1, wherein the subscript d is 0.

8. The improved cathode material for lithium ion batteries according to claim 1, wherein said X is Co.

9. The improved cathode material for a lithium ion battery according to claim 1, wherein the G is selected from the group consisting of Al, Gd, Ti, Zr, Mg, Ca, Sr, Ba, Mg, Cr, Cu, Fe, Zn, V, Bi, Nb and B.

10. The improved cathode material for lithium ion batteries according to claim 1, wherein the G is selected from Al and Gd.

11. A battery half-cell comprising the improved cathode material for lithium-ion batteries according to claim 1.

12. A battery comprising the improved cathode material for lithium ion battery according to claim 1.

13. An agglomerate comprising: Particles comprising an oxide defined by the formula: LiNi a Mn b X c G d O2 wherein G is an optional dopant; X is Co or Al; a≥0.5; b+c+d≤0.5; and d≤0.1; wherein the particles agglomerate to form the agglomerates and wherein each particle of the particles comprises a surface; a coating material covering the entire surface, wherein the coating material is between adjacent particles in the agglomerate, wherein the coating material comprises niobium; and Before the particles agglomerate to form the agglomerates, a salt of Li, Ni, Mn, Co or Al forming an oxide precursor is added to the coating material.

14. The agglomerate of claim 13, wherein the agglomerate further comprises interstitial surfaces, wherein the interstitial surfaces comprise the coating material on each surface of each of the particles.

15. The agglomerate of claim 13, wherein each of the coating materials has a thickness of 5 to 10 nanometers.

16. The agglomerate of claim 13, wherein each of said coating materials comprises LiNbO3.

17. The agglomerate of claim 13, wherein subscript a is defined by the equation 0.5≤a≤0.

9.

18. The agglomerate of claim 17, wherein the subscript a is defined by the equation 0.58≤a≤0.62 or by the equation 0.78≤a≤0.

82.

19. The agglomerate of claim 13, wherein subscript d is 0.

20. The agglomerate of claim 13, wherein the X is Co.

21. The agglomerate of claim 13, wherein the G is selected from the group consisting of Al, Gd, Ti, Zr, Mg, Ca, Sr, Ba, Mg, Cr, Cu, Fe, Zn, V, Bi, Nb, and B.

22. The agglomerate of claim 13, wherein the G is selected from Al and Gd.

23. A battery half-cell comprising the agglomerate of claim 13.

24. A battery comprising the agglomerate according to claim 13.

Citation Information

Patent Citations

  • A cathode material of an all-solid state battery comprising a coating layer for preventing diffusion and a method for preparing thereof

    CN108878798A

  • Positive electrode active material for non-aqueous electrolyte secondary cell and method for manufacturing same, and non-aqueous electrolyte secondary cell

    WO2018123951A1

  • Positive electrode active material, method for producing same, positive electrode, and lithium ion battery

    WO2019065254A1