Semiconductor structure and method for forming semiconductor structure

By forming a barrier layer on the first open side wall during the formation of the semiconductor structure, the problem of complex process and poor performance of the local interconnect structure in the prior art is solved, and higher etching accuracy and semiconductor structure performance are achieved .

CN113903722BActive Publication Date: 2024-11-22SEMICON MFG INT (SHANGHAI) CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010641654.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-07-06
Publication Date
2024-11-22
Estimated Expiration
2040-07-06

AI Technical Summary

Technical Problem

The process of local interconnect structures in the manufacturing of existing semiconductor devices is complex and the performance needs to be improved, resulting in poor performance of the formed semiconductor structures.

Method used

During the formation of the semiconductor structure, a barrier layer is formed on the side wall of the first opening and the initial second mask layer continues to be etched until the surface of the dielectric structure is exposed, and the second mask layer is formed, and the barrier layer reduces etching The process erected the side walls of the initial second mask layer to ensure the accuracy of the second opening and the semiconductor structure performance after subsequent pattern transmission.

Benefits of technology

Through the use of the barrier layer, the etching accuracy is improved, the semiconductor structure formed is better, the inhomogeneity and shorting risks of metal layers are reduced, and the overall performance of semiconductor devices is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113903722B_ABST
    Figure CN113903722B_ABST
Patent Text Reader

Abstract

A semiconductor structure and a method for forming the semiconductor structure, the method comprising: providing a substrate; forming a dielectric structure on the substrate; forming a first mask layer on the dielectric structure; forming an initial second mask layer on the first mask layer; forming a first opening in the initial second mask layer, wherein the first opening exposes a portion of the surface of the first mask layer and the first opening spans the surface of the first mask layer; forming a barrier layer on the sidewall of the first opening; etching the initial second mask layer at the bottom of the first opening until the surface of the dielectric structure is exposed, forming a second mask layer, wherein the second mask layer has a second opening. The performance of the semiconductor structure formed by the method is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor manufacturing, and in particular to a semiconductor structure and a method for forming the semiconductor structure. Background Art

[0002] The metal interconnection structure is an indispensable structure in semiconductor devices, which is used to realize the interconnection between active areas, between transistors, or between metal lines of different layers, and complete the transmission and control of signals. Therefore, in the semiconductor manufacturing process, the formation of the metal interconnection structure has a great influence on the performance of semiconductor devices and the semiconductor manufacturing cost. In order to increase the density of devices, the size of semiconductor devices in integrated circuits has been continuously reduced. In order to realize the electrical connection of each semiconductor device, a multi-layer interconnection structure is usually required.

[0003] Generally, in the back-end interconnection process of the semiconductor device manufacturing process, the first metal layer (M1) needs to form an electrical connection with the active device structure (including the source and drain regions and the gate structure region) of the lower layer. Therefore, before forming the first metal layer, it is usually necessary to pre-form a local interconnection structure (Local Interconnect) of the semiconductor device. The local interconnection structure includes: a zeroth metal layer (M0) electrically connected to the source and drain regions of the lower layer, and a zeroth gate metal layer (M0G) electrically connected to the gate structure.

[0004] However, the manufacturing process of the semiconductor structure with the local interconnection structure in the prior art is complicated, and the performance of the formed semiconductor structure needs to be further improved. Summary of the invention

[0005] The technical problem solved by the present invention is to provide a semiconductor structure and a method for forming the semiconductor structure.

[0006] To solve the above technical problems, the technical solution of the present invention provides a semiconductor structure, including: a substrate; a dielectric structure located on the substrate; a first mask layer located on the dielectric structure; an initial second mask layer located on the first mask layer, the initial second mask layer having a first opening, the first opening exposing a portion of the surface of the first mask layer, and the first opening spanning the surface of the first mask layer; and a blocking layer located on the sidewall surface of the first opening.

[0007] Optionally, the material of the blocking layer and the material of the initial second mask layer have different etching selectivities.

[0008] Optionally, the material of the initial second mask layer includes an inorganic material, and the inorganic material includes amorphous carbon.

[0009] Optionally, the material of the barrier layer includes a dielectric material, and the dielectric material includes a combination of one or more of silicon oxide, silicon nitride, silicon carbide, silicon oxycarbide, silicon oxynitride, aluminum oxide, aluminum nitride, silicon carbide nitride and silicon carbon nitride oxynitride.

[0010] Optionally, the material of the first mask layer and the material of the initial second mask layer have different etching selectivities.

[0011] Optionally, the material of the first mask layer includes an inorganic material, and the inorganic material includes one or more combinations of silicon, silicon oxide, titanium nitride, carbon-doped tungsten, silicon nitride, silicon carbide, silicon carbide nitride, silicon oxynitride, silicon oxycarbide, and silicon oxycarbon nitride.

[0012] Optionally, it further includes: a graphic transfer structure located between the dielectric structure and the first mask layer, wherein the graphic transfer structure includes a first graphic transfer layer and a second graphic transfer layer located on the first graphic transfer layer.

[0013] Optionally, it also includes: a gate structure located on the substrate; source and drain doped regions located in the substrate on both sides of the gate structure; and the dielectric structure covers the top surface and side wall surfaces of the gate structure.

[0014] Optionally, part of the first opening is located on the surface of the source and drain doped regions.

[0015] Correspondingly, the technical solution of the present invention also provides a method for forming a semiconductor structure, including: providing a substrate; forming a dielectric structure on the substrate; forming a first mask layer on the dielectric structure; forming an initial second mask layer on the first mask layer; forming a first opening in the initial second mask layer, wherein the first opening exposes a portion of the surface of the first mask layer, and the first opening spans the surface of the first mask layer; and forming a blocking layer on the sidewall of the first opening.

[0016] Optionally, the method for forming the barrier layer includes: forming a barrier material layer on the side wall surface and the bottom surface of the first opening; and etching back the barrier material layer until an initial second mask layer at the bottom of the first opening is exposed to form the barrier layer.

[0017] Optionally, the gas used for etching back the barrier material layer includes a mixed gas of hydrogen, argon, helium, tetrafluoromethane and carbon monoxide.

[0018] Optionally, the material of the blocking layer and the material of the initial second mask layer have different etching selectivities.

[0019] Optionally, the material of the initial second mask layer includes an inorganic material, and the inorganic material includes amorphous carbon.

[0020] Optionally, the material of the barrier layer includes a dielectric material, and the dielectric material includes a combination of one or more of silicon oxide, silicon nitride, silicon carbide, silicon oxycarbide, silicon oxynitride, aluminum oxide, aluminum nitride, silicon carbide nitride and silicon carbon nitride oxynitride.

[0021] Optionally, the material of the first mask layer and the material of the initial second mask layer have different etching selectivities.

[0022] Optionally, the material of the first mask layer includes a dielectric material, and the dielectric material includes one or more combinations of silicon oxide, silicon nitride, silicon carbide, silicon oxycarbide, silicon oxynitride, aluminum oxide, aluminum nitride, silicon carbide nitride and silicon carbon nitride oxynitride.

[0023] Optionally, the method for forming the first opening includes: forming a patterned photoresist layer on an initial second mask layer; using the patterned photoresist layer as a mask, etching the initial second mask layer until a surface of the first mask layer is exposed to form the first opening.

[0024] Optionally, after forming the barrier layer, the method further includes: etching the initial second mask layer at the bottom of the first opening until the surface of the dielectric structure is exposed to form a second mask layer, wherein the second mask layer has a second opening.

[0025] Optionally, after forming the dielectric structure and before forming the first mask layer on the dielectric structure, it also includes: forming a graphic transfer structure on the dielectric structure, the graphic transfer structure including a first graphic transfer layer and a second graphic transfer layer located on the first graphic transfer layer; the second opening exposes the surface of the graphic transfer structure.

[0026] Optionally, before forming the first mask layer on the dielectric structure, the method further includes: forming a gate structure on the substrate, and forming source and drain doping regions in the substrate on both sides of the gate structure; the dielectric structure covers the top surface and side wall surfaces of the gate structure.

[0027] Optionally, part of the second opening is located on the source and drain doped regions.

[0028] Optionally, after forming the second opening, the method further includes: etching the dielectric structure with the second opening until the surface of the source and drain doped regions is exposed, thereby forming a third opening in the dielectric structure; after forming the third opening, removing the second mask layer and the first mask layer; after removing the second mask layer and the first mask layer, forming a metal layer in the third opening, wherein the metal layer is electrically connected to the source and drain doped regions.

[0029] Optionally, the process of etching the initial second mask layer at the bottom of the first opening includes a dry etching process, and the gas of the dry etching process includes a combination of one or more of hydrogen, nitrogen, carbon monoxide, carbon dioxide, carbon oxysulfide, sulfur dioxide and oxygen.

[0030] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:

[0031] In the semiconductor structure of the technical solution of the present invention, the initial second mask layer has a first opening, and the side wall surface of the first opening has a barrier layer, so that in the process of continuing to etch the initial second mask layer, the barrier layer can reduce the lateral etching of the initial second mask layer side wall located on the surface of the first mask layer by the etching process, so that the size accuracy of the formed second opening is better, and the semiconductor structure formed after the pattern of the second mask layer is subsequently transferred has better performance.

[0032] The method for forming a semiconductor structure in the technical solution of the present invention forms a barrier layer on the sidewall of the first opening, and then continues to etch the initial second mask layer at the bottom of the first opening until the surface of the dielectric structure is exposed, thereby forming a second mask layer, wherein the second mask layer has a second opening. The barrier layer enables the etching process to reduce the lateral etching of the sidewall of the initial second mask layer located on the surface of the first mask layer during the process of continuing to etch the initial second mask layer, thereby making the size accuracy of the formed second opening better, and the semiconductor structure formed after the pattern of the second mask layer is subsequently transferred has better performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figures 1 to 3 is a schematic cross-sectional structural diagram of a semiconductor structure in one embodiment;

[0034] Figures 4 to 14 It is a schematic cross-sectional structure diagram of the semiconductor structure forming process in an embodiment of the present invention. DETAILED DESCRIPTION

[0035] As described in the background art, the manufacturing process of the semiconductor structure with the local interconnection structure in the prior art is complicated, and the performance of the formed semiconductor structure needs to be improved.

[0036] Figures 1 to 3 It is a schematic cross-sectional structure diagram of a semiconductor structure in one embodiment.

[0037] Please refer to Figure 1 , Figure 2 and Figure 3 , Figure 1 for Figure 2 and Figure 3A top view of Figure 2 for Figure 1 Schematic diagram of the cross-section structure along the section line AA'. Figure 3 for Figure 1 A schematic cross-sectional structure diagram along the section line BB' direction, providing a substrate 100; forming a gate structure 101 on the substrate 100; forming source and drain doping regions 102 in the substrate on both sides of the gate structure 101; forming a dielectric structure 103 on the substrate 100, the dielectric structure 103 being located on the top surface and sidewall surface of the gate structure 101; forming a first mask layer 104 on the dielectric structure 103; forming a second mask layer 105 on the first mask layer 104 and the dielectric structure 103, the second mask layer 105 having an opening 106, the opening 106 exposing a portion of the surface of the first mask layer 104 and the surface of the dielectric structure 103.

[0038] In the semiconductor structure, the first mask layer 104 is used to isolate the opening 106. Subsequently, the dielectric structure 103 is further etched with the second mask layer 105 until the source-drain doped region 102 is exposed, and a groove (not shown) is formed in the dielectric structure 103. When a metal layer (not shown) is continuously formed in the groove, the first mask layer 104 can isolate the formed metal layer, so that the connection of the formed metal layer has diversity.

[0039] When forming the second mask layer 105 having the opening 106, the dry etching process for forming the second mask layer 105 does not expose the surface of the dielectric structure 103 when etching the material of the second mask layer 105 to the surface of the first mask layer 104, so it is necessary to continue etching until the surface of the dielectric structure 103 is exposed. The etching gas of the dry etching process causes less damage to the first mask layer 104. Therefore, in the process of continuing to etch the material of the second mask layer 105 until the surface of the dielectric structure 103 is exposed, the etching gas on the first mask layer 104 will laterally etch the material of the second mask layer 105, so that the size of the formed opening 106 at a position adjacent to the first mask layer 104 is larger (e.g., Figure 1 The CD2 described in the figure is larger than the size (CD1) of the opening 106 far away from the first mask layer 104. After the pattern of the second mask layer 105 is subsequently transferred to form a groove, when a metal layer electrically connected to the source and drain doping regions 102 is formed in the groove, the size of the metal layer is uneven, and the size of the metal layer adjacent to the first mask layer 104 is large, which is easy to short-circuit with the gate structure 101, thereby affecting the performance of the semiconductor structure.

[0040] In order to solve the above problems, the technical solution of the present invention provides a semiconductor structure and a method for forming the semiconductor structure, wherein a barrier layer is formed on the sidewall of the first opening, and then the initial second mask layer at the bottom of the first opening is continuously etched until the surface of the dielectric structure is exposed, thereby forming a second mask layer, wherein the second mask layer has a second opening. The barrier layer enables the etching process to reduce the lateral etching of the sidewall of the initial second mask layer located on the surface of the first mask layer during the process of continuing to etch the initial second mask layer, thereby making the size accuracy of the formed second opening better, and the semiconductor structure formed after the pattern of the second mask layer is subsequently transferred has better performance.

[0041] In order to make the above-mentioned objects, features and beneficial effects of the present invention more obvious and easy to understand, specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.

[0042] Figures 4 to 14 It is a schematic cross-sectional structure diagram of the semiconductor structure forming process in an embodiment of the present invention.

[0043] Please refer to Figure 4 , providing a substrate 200.

[0044] In this embodiment, the material of the substrate 200 is silicon.

[0045] In other embodiments, the substrate material includes silicon carbide, silicon germanium, a multinary semiconductor material composed of group III-V elements, silicon on insulator (SOI) or germanium on insulator (GOI). Among them, the multinary semiconductor material composed of group III-V elements includes InP, GaAs, GaP, InAs, InSb, InGaAs or InGaAsP.

[0046] Please refer to Figure 5 , a gate structure 201 is formed on the substrate, and source-drain doped regions 202 are formed in the substrate 200 on both sides of the gate structure 201 ; a dielectric structure 203 is formed on the substrate 200 , and the dielectric structure 203 covers the top surface and sidewall surface of the gate structure 201 .

[0047] The gate structure 201 includes: a gate dielectric layer (not shown) and a gate layer (not shown) located on the gate dielectric layer.

[0048] The source-drain doping region 202 has doping ions therein, and the doping ions include N-type ions or P-type ions. The N-type ions include phosphorus ions, arsenic ions, or antimony ions; and the P-type ions include boron ions, boron fluoride ions, or indium ions.

[0049] The material of the dielectric structure 203 includes a dielectric material, and the dielectric material includes one or more combinations of silicon oxide, silicon nitride, silicon carbide, silicon oxycarbide, silicon oxynitride, aluminum oxide, aluminum nitride, silicon carbide nitride, and silicon oxycarbon nitride. In this embodiment, the material of the dielectric structure 203 includes silicon oxide.

[0050] Please continue to refer to Figure 5 , forming a graphic transfer structure 204 on the medium structure.

[0051] In this embodiment, the graphic transfer structure 204 includes a first graphic transfer layer (not shown) and a second graphic transfer layer (not shown) located on the first graphic transfer layer.

[0052] The pattern transfer structure 204 is used to stably transfer the pattern of the second mask layer subsequently.

[0053] The material of the first pattern transfer layer includes an inorganic material; the material of the second pattern transfer layer includes an inorganic material.

[0054] In this embodiment, the material of the first pattern transfer layer includes titanium nitride, and the material of the second pattern transfer layer includes silicon oxide.

[0055] In other embodiments, the graphic transfer structure may not be formed.

[0056] Please refer to Figure 6 and Figure 7 , Figure 6 for Figure 7 Schematic diagram of the structure along the section line CC'. Figure 7 for Figure 6 A first mask layer 205 is formed on the pattern transfer structure 204, as shown in FIG.

[0057] The first mask layer 205 is used to cut off the pattern of the subsequent second mask layer, and then the patterns of the second mask layer and the first mask layer 205 are transferred to the dielectric structure 204 to form a third opening, and then a metal layer is formed in the third opening. The metal layer can be isolated at the position of the first mask layer 205, thereby realizing different connections of the metal layer.

[0058] The material of the first mask layer 205 includes an inorganic material, and the inorganic material includes one or more combinations of silicon, silicon oxide, titanium nitride, carbon-doped tungsten, silicon nitride, silicon carbide, silicon carbide nitride, silicon oxynitride, silicon oxycarbide, and silicon oxycarbon nitride.

[0059] The material of the first mask layer 205 and the material on the surface of the pattern transfer structure 204 have different etching selectivities, so that when the first mask layer 205 is formed on the surface of the pattern transfer structure 204 , the surface of the pattern transfer structure 204 is less damaged.

[0060] In this embodiment, the material of the first mask layer 205 includes silicon nitride.

[0061] In other embodiments, the material of the first mask layer and the material of the dielectric structure have different etching selectivities.

[0062] Please refer to Figure 8 and Fig. 9 , Figure 8 for Fig. 9 Schematic diagram of the structure along the section line DD'. Fig. 9 for Figure 8 An initial second mask layer 206 is formed on the first mask layer 205, as shown in FIG.

[0063] The material of the initial second mask layer 206 includes an inorganic material, and the inorganic material includes amorphous carbon.

[0064] The material of the first mask layer 205 has a different etching selectivity ratio from that of the initial second mask layer 206 , so that the first mask layer 205 is less damaged during the subsequent etching of the initial second mask layer 206 .

[0065] Please continue to refer to Figure 8 and Fig. 9 , a first opening 207 is formed in the initial second mask layer 206 , wherein the first opening 207 exposes a portion of the surface of the first mask layer 205 , and the first opening 207 spans across the surface of the first mask layer 205 .

[0066] The method for forming the first opening 207 includes: forming a patterned photoresist layer (not shown) on the initial second mask layer 206; using the patterned photoresist layer as a mask, etching the initial second mask layer 206 until the surface of the first mask layer 205 is exposed to form the first opening 207.

[0067] Please refer to Fig.10 , Fig.10 For Figure 8 Based on the structural diagram of FIG. 1 , a barrier layer 208 is formed on the side wall of the first opening 207 .

[0068] The barrier layer 208 enables the barrier layer 208 to reduce the lateral etching of the side walls of the initial second mask layer 206 located on the surface of the first mask layer 205 during the subsequent etching of the initial second mask layer 206, thereby making the second opening size formed more accurate and the semiconductor structure formed after the pattern of the second mask layer is subsequently transferred to have better performance.

[0069] The method for forming the barrier layer 208 includes: forming a barrier material layer (not shown) on the sidewall surface and the bottom surface of the first opening 207; and etching back the barrier material layer until the initial second mask layer 206 at the bottom of the first opening 207 is exposed to form the barrier layer 208.

[0070] In this embodiment, the gas used for etching back the barrier material layer includes a mixed gas of hydrogen, argon, helium, tetrafluoromethane and carbon monoxide.

[0071] The material of the blocking layer 208 is different from the material of the initial second mask layer 206 , so that during the process of etching back the blocking material layer, the etching back process causes less damage to the morphology of the initial second mask layer 206 .

[0072] The material of the barrier layer 208 includes a dielectric material, and the dielectric material includes one or more combinations of silicon oxide, silicon nitride, silicon carbide, silicon oxycarbide, silicon oxynitride, aluminum oxide, aluminum nitride, silicon nitride carbonitride, and silicon oxycarbonitride. The process of forming the barrier material layer includes a deposition process, and the deposition process includes a chemical vapor deposition process or an atomic layer deposition process.

[0073] In this embodiment, the material of the barrier layer 208 includes silicon oxide; and the process of forming the barrier material layer includes a chemical vapor deposition process.

[0074] In this embodiment, the process of forming the first opening 207 and the process of forming the barrier material layer are performed in the same vacuum reaction chamber, thereby saving process flow.

[0075] In other embodiments, the process of forming the first opening and the process of forming the barrier material layer can be performed in different vacuum reaction chambers.

[0076] Please refer to Fig.11 and Fig.12 , Fig.11 for Fig.12 Schematic diagram of the cross-sectional structure along the section line FF'. Fig.12 for Fig.11 The top view of the first opening 207 is etched to form the initial second mask layer 206 at the bottom of the first opening 207 until the surface of the pattern transfer structure 204 is exposed to form a second mask layer 209, wherein the second mask layer 209 has a second opening 210, and part of the second opening 210 is located on the source and drain doping region 202.

[0077] In this embodiment, the process of etching the initial second mask layer 206 at the bottom of the first opening 207 includes a dry etching process, and the gas of the dry etching process includes a combination of one or more of hydrogen, nitrogen, carbon monoxide, carbon dioxide, carbon oxysulfide, sulfur dioxide and oxygen.

[0078] Since the barrier layer 208 is formed on the side wall of the first opening 207, the barrier layer 208 can reduce the lateral etching of the side wall of the initial second mask layer 206 located on the surface of the first mask layer 205 during the process of continuing to etch the initial second mask layer 206, thereby making the second opening 210 formed have better dimensional accuracy, and the semiconductor structure formed after the pattern of the second mask layer 209 is subsequently transferred has better performance.

[0079] Please refer to Fig.13 and Fig.14 , Fig.13 for Fig.14 Schematic diagram of the cross-sectional structure along the section line GG'. Fig.14 for Fig.13 , after forming the second opening 210, the pattern transfer structure 204 and the dielectric structure 203 are etched through the second opening 210 until the surface of the source-drain doped region 202 is exposed, and a third opening (not shown) is formed in the dielectric structure 203; after forming the third opening, the second mask layer 209 and the first mask layer 205 are removed; after removing the second mask layer 209 and the first mask layer 205, a metal layer 211 is formed in the third opening, and the metal layer 211 is electrically connected to the source-drain doped region 202.

[0080] The method and process for forming the third opening and the metal layer 211 are common technical means in the art and will not be described in detail here.

[0081] The material of the metal layer 211 includes metal, and the metal includes one or more combinations of copper, aluminum, tungsten, cobalt, and titanium nitride.

[0082] Since the barrier layer 208 is formed on the side wall of the first opening 207, the barrier layer 208 can reduce the lateral etching of the initial second mask layer 206 side wall on the surface of the first mask layer 205 by the etching process during the continuous etching of the initial second mask layer 206, so that the second opening 210 formed has better dimensional accuracy. Subsequently, the third opening is formed in the dielectric structure 203 by transferring the pattern of the second mask layer 209, and a metal layer 211 is formed in the third opening. The metal layer 211 has better dimensional uniformity, which reduces the situation where the local size of the metal layer 211 is large and is easily short-circuited with the gate structure 201, thereby improving the performance of the semiconductor structure.

[0083] Accordingly, the embodiment of the present invention further provides a semiconductor structure, please continue to refer to Fig.10 ,include:

[0084] Substrate 200;

[0085] A dielectric structure 203 located on the substrate 200;

[0086] A first mask layer 205 located on the dielectric structure 203;

[0087] An initial second mask layer 206 located on the first mask layer 205, wherein the initial second mask layer 206 has a first opening 207, wherein the first opening 207 exposes a portion of the surface of the first mask layer 205, and the first opening 207 spans across the surface of the first mask layer 205;

[0088] A barrier layer 208 is located on the sidewall surface of the first opening 207 .

[0089] In this embodiment, the material of the blocking layer 208 and the material of the initial second mask layer 206 have different etching selectivities.

[0090] In this embodiment, the material of the initial second mask layer 206 includes an inorganic material, and the inorganic material includes amorphous carbon.

[0091] In the present embodiment, the material of the blocking layer 208 includes a dielectric material, and the dielectric material includes one or more combinations of silicon oxide, silicon nitride, silicon carbide, silicon oxycarbide, silicon oxynitride, aluminum oxide, aluminum nitride, silicon carbide nitride, and silicon oxycarbon nitride.

[0092] In this embodiment, the material of the first mask layer 205 and the material of the initial second mask layer 206 have different etching selectivities.

[0093] In this embodiment, the material of the first mask layer 205 includes an inorganic material, and the inorganic material includes one or more combinations of silicon, silicon oxide, titanium nitride, carbon-doped tungsten, silicon nitride, silicon carbide, silicon carbide nitride, silicon oxynitride, silicon oxycarbide, and silicon oxycarbon nitride.

[0094] In this embodiment, it also includes: a graphic transfer structure 204 located between the medium structure 203 and the partition structure, and the graphic transfer structure 204 includes a first graphic transfer layer (not shown) and a second graphic transfer layer (not shown) located on the first graphic transfer layer.

[0095] In this embodiment, it also includes: a gate structure 201 located on the substrate 200 ; source and drain doped regions 202 located in the substrate on both sides of the gate structure 201 ; and the dielectric structure 203 covering the top surface and sidewall surfaces of the gate structure 201 .

[0096] In this embodiment, a portion of the first opening 207 is located on the surface of the source / drain doped region 202 .

[0097] The semiconductor structure has a first opening 207 in the initial second mask layer 206, and the side wall surface of the first opening 207 has a barrier layer 208, so that in the process of continuing to etch the initial second mask layer 206, the barrier layer 208 can reduce the lateral etching of the side wall of the initial second mask layer 206 located on the surface of the first mask layer 205 by the etching process, so that the size accuracy of the second opening formed subsequently is better, and the semiconductor structure formed subsequently after transferring the pattern of the second mask layer has better performance.

[0098] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.

Claims

1. A semiconductor structure, characterized in that: include: substrate; a dielectric structure disposed on a substrate; a first mask layer located on the dielectric structure; an initial second mask layer located on the first mask layer, wherein the initial second mask layer has a first opening, wherein the first opening exposes a portion of the surface of the first mask layer, and the first opening spans across the surface of the first mask layer; A barrier layer is located on the side wall surface of the first opening, wherein the material of the barrier layer has a different etching selectivity from the material of the initial second mask layer, and the barrier layer is used to reduce lateral etching of the side wall of the initial second mask layer when etching the initial second mask layer at the bottom of the first opening.

2. The semiconductor structure according to claim 1, wherein: The material of the initial second mask layer includes an inorganic material, and the inorganic material includes amorphous carbon.

3. The semiconductor structure according to claim 1, wherein: The material of the barrier layer includes a dielectric material, and the dielectric material includes one or more combinations of silicon oxide, silicon nitride, silicon carbide, silicon oxycarbide, silicon oxynitride, aluminum oxide, aluminum nitride, silicon nitride carbide, and silicon oxycarbide nitride.

4. The semiconductor structure according to claim 1, wherein: The material of the first mask layer has a different etching selectivity from the material of the initial second mask layer.

5. The semiconductor structure according to claim 4, characterized in that The material of the first mask layer includes a dielectric material, and the dielectric material includes one or more combinations of silicon oxide, silicon nitride, silicon carbide, silicon oxycarbide, silicon oxynitride, aluminum oxide, aluminum nitride, silicon carbide nitride, and silicon oxycarbide nitride.

6. The semiconductor structure according to claim 1, wherein: Also includes: A pattern transfer structure is located between the dielectric structure and the first mask layer, and the pattern transfer structure includes a first pattern transfer layer and a second pattern transfer layer located on the first pattern transfer layer.

7. The semiconductor structure according to claim 1, wherein: Also includes: a gate structure located on the substrate; Source and drain doping regions located in the substrate on both sides of the gate structure; The dielectric structure covers the top surface and sidewall surfaces of the gate structure.

8. The semiconductor structure according to claim 7, wherein: Part of the first opening is located on the surface of the source and drain doped regions.

9. A method for forming a semiconductor structure, characterized in that: include: providing a substrate; forming a dielectric structure on a substrate; forming a first mask layer on the dielectric structure; forming an initial second mask layer on the first mask layer; forming a first opening in the initial second mask layer, wherein the first opening exposes a portion of the surface of the first mask layer and the first opening spans across the surface of the first mask layer; forming a barrier layer on the sidewall of the first opening, wherein the material of the barrier layer has a different etching selectivity from the material of the initial second mask layer; The initial second mask layer at the bottom of the first opening is etched until the surface of the dielectric structure is exposed to form a second mask layer, wherein the second mask layer has a second opening.

10. The method for forming a semiconductor structure according to claim 9, wherein: The method for forming the barrier layer comprises: forming a barrier material layer on the sidewall surface and the bottom surface of the first opening; etching back the barrier material layer until an initial second mask layer at the bottom of the first opening is exposed to form the barrier layer.

11. The method for forming a semiconductor structure according to claim 10, wherein: The gas used for etching back the barrier material layer includes a mixed gas of hydrogen, argon, helium, tetrafluoromethane and carbon monoxide.

12. The method for forming a semiconductor structure according to claim 9, wherein: The material of the initial second mask layer includes an inorganic material, and the inorganic material includes amorphous carbon.

13. The method for forming a semiconductor structure according to claim 9, wherein: The material of the barrier layer includes a dielectric material, and the dielectric material includes one or more combinations of silicon oxide, silicon nitride, silicon carbide, silicon oxycarbide, silicon oxynitride, aluminum oxide, aluminum nitride, silicon nitride carbide, and silicon oxycarbide nitride.

14. The method for forming a semiconductor structure according to claim 9, wherein: The material of the first mask layer has a different etching selectivity from the material of the initial second mask layer.

15. The method for forming a semiconductor structure according to claim 14, wherein: The material of the first mask layer includes an inorganic material, and the inorganic material includes one or more combinations of silicon, silicon oxide, titanium nitride, carbon-doped tungsten, silicon nitride, silicon carbide, silicon carbide nitride, silicon oxynitride, silicon oxycarbide, and silicon oxycarbon nitride.

16. The method for forming a semiconductor structure according to claim 9, wherein: The method for forming the first opening includes: forming a patterned photoresist layer on an initial second mask layer; using the patterned photoresist layer as a mask, etching the initial second mask layer until the surface of the first mask layer is exposed to form the first opening.

17. The method for forming a semiconductor structure according to claim 9, wherein: After forming the dielectric structure and before forming the first mask layer on the dielectric structure, the method further includes: forming a graphic transfer structure on the dielectric structure, the graphic transfer structure including a first graphic transfer layer and a second graphic transfer layer located on the first graphic transfer layer; the second opening exposes the surface of the graphic transfer structure.

18. The method for forming a semiconductor structure according to claim 9, wherein: Before forming the first mask layer on the dielectric structure, the method further includes: forming a gate structure on the substrate, and forming source and drain doping regions in the substrate on both sides of the gate structure; the dielectric structure covers the top surface and side wall surface of the gate structure.

19. The method for forming a semiconductor structure according to claim 18, wherein: Part of the second opening is located on the source-drain doped region.

20. The method for forming a semiconductor structure according to claim 19, wherein: After forming the second opening, the method further includes: etching the dielectric structure with the second opening until the surface of the source-drain doped region is exposed, thereby forming a third opening in the dielectric structure; after forming the third opening, removing the second mask layer and the first mask layer; after removing the second mask layer and the first mask layer, forming a metal layer in the third opening, wherein the metal layer is electrically connected to the source-drain doped region.

21. The method for forming a semiconductor structure according to claim 9, wherein: The process of etching the initial second mask layer at the bottom of the first opening includes a dry etching process, and the gas of the dry etching process includes a combination of one or more of hydrogen, nitrogen, carbon monoxide, carbon dioxide, carbon oxysulfide, sulfur dioxide and oxygen.