Salt-resistant and high-temperature-resistant tea polyphenol-modified resin fluid loss reducer for drilling fluid, preparation method and application thereof

Through the preparation of tea polyphenol-modified resin fluid loss additives, the problem of insufficient salt resistance and high temperature resistance of existing drilling fluid fluid loss additives has been solved, and efficient drilling fluid performance improvement and environmental protection effects have been achieved, which is suitable for complex applications. drilling conditions.

CN113929845BActive Publication Date: 2024-10-15SINOPEC OILFIELD SERVICE CORPORATION +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010606762.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-06-29
Publication Date
2024-10-15
Estimated Expiration
2040-06-29

AI Technical Summary

Technical Problem

Existing drilling fluid fluid loss additives have deficiencies in salt resistance and high temperature resistance, especially in areas with high environmental protection requirements. They are difficult to meet the complex conditions of oil drilling, and their biodegradability is poor, which limits the scope of application.

Method used

Tea polyphenols, acetone and paraformaldehyde are used to polymerize under alkaline conditions to prepare a tea polyphenol-modified resin fluid loss reducer with fused ring groups, phenyl groups and sulfite groups, forming a branched chain structure. Resin products to improve their resistance to temperature and salt.

Benefits of technology

The tea polyphenol-modified resin fluid loss agent exhibits a thermal decomposition temperature higher than 310°C, has good salt resistance and high temperature fluid loss properties, reduces the occurrence of complex drilling accidents, improves drilling quality and efficiency, and has Good environmental performance, suitable for a wide range of salt-resistant fluid loss additive technical requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0002559460150000041
    Figure BDA0002559460150000041
  • Figure BDA0002559460150000051
    Figure BDA0002559460150000051
  • Figure BDA0002559460150000101
    Figure BDA0002559460150000101
Patent Text Reader

Abstract

The present invention belongs to the technical field of petroleum industry. The present invention provides a salt-resistant and high-temperature-resistant tea polyphenol-modified resin fluid loss reducer for drilling fluid, a preparation method and application thereof. The tea polyphenol-modified resin fluid loss reducer is prepared by polymerization reaction of tea polyphenol, acetone, sulfite and polyformaldehyde under alkaline conditions; the tea polyphenol-modified resin fluid loss reducer molecule includes a condensed ring group, a phenyl group and a sulfite group, and has a branched structure. The tea polyphenol-modified resin of the present invention has good degradability, does not pollute the environment, and produces a good environmental protection effect; the modified resin product provided by the present invention has good salt resistance and high-temperature resistance fluid loss reduction performance, can effectively avoid or reduce the occurrence of complex drilling accidents, thereby improving drilling quality and efficiency, and meets the technical requirements of salt-resistant and high-temperature-resistant fluid loss reducers with a wide range of use in the market, which is conducive to the application in drilling fluid.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of petroleum industry, and specifically relates to a salt-resistant and high-temperature-resistant tea polyphenol-modified resin fluid loss reducer for drilling fluid, and a preparation method and application thereof. Background Art

[0002] Drilling fluid is an important fluid in the drilling project of the oil industry. The quality of its performance is directly related to the quality of drilling, and it plays a vital role in the oil recovery efficiency of an oil field. Drilling fluid is mainly composed of base slurry and various treatment agents, and the treatment agents include fluid loss reducers, pH adjusters, etc. Among them, properly controlling the fluid loss through fluid loss reducers is one of the important properties of drilling fluid. In addition, as the exploitation of oil and natural gas resources gradually develops to deep and ultra-deep layers, the formations encountered are becoming more and more complex, and the difficulty of oil drilling is also increasing accordingly, which also puts higher requirements on the temperature resistance, salt resistance and other properties of drilling fluid.

[0003] At present, there are many types of fluid loss reducers on the market. For example, SMP is a very good resin-based high-temperature resistant fluid loss reducer. The raw materials of SMP are mainly formaldehyde and phenol, and its structure contains benzene rings. It has excellent long-term high-temperature stability and thermal stability (<180°C). It has always been the most widely used and irreplaceable product at home and abroad, and is suitable for almost all drilling fluid systems.

[0004] However, with the severe environmental situation, the product has problems such as poor biodegradability. Although the SMP product itself is non-toxic, its biodegradability is poor. In some areas with high environmental protection requirements, the application of SMP has been restricted. Therefore, it is of great significance to develop a fluid loss reducer that is both temperature-resistant and salt-resistant and environmentally friendly, and can ensure the high efficiency of drilling fluids. Summary of the invention

[0005] In view of this, the present application provides a salt-resistant and high-temperature-resistant tea polyphenol-modified resin fluid loss reducer for drilling fluid, a preparation method and application thereof. The modified resin product provided by the present invention has good salt-resistant and high-temperature-resistant fluid loss reduction performance, can effectively avoid or reduce the occurrence of complex drilling accidents, thereby improving drilling quality and efficiency. At the same time, it is more environmentally friendly and can meet the technical requirements of salt-resistant fluid loss reducers with a wide range of use on the market.

[0006] The present invention provides a salt-resistant and high-temperature-resistant tea polyphenol-modified resin fluid loss reducer for drilling fluid, which is prepared by polymerization reaction of tea polyphenol, acetone, sulfite and paraformaldehyde under alkaline conditions;

[0007] The tea polyphenol modified resin fluid loss reducer molecule comprises a condensed ring group, a phenyl group and a sulfite group, and has a branched chain structure.

[0008] Preferably, the thermal decomposition temperature of the tea polyphenol modified resin fluid loss reducer is higher than 310°C.

[0009] Preferably, the polymerization degree of the paraformaldehyde is 8-12.

[0010] Preferably, the mass ratio of the tea polyphenols, acetone, sulfite and paraformaldehyde is (20-30):(4-6):(1-2):(10-20).

[0011] The present invention provides a method for preparing the salt-resistant and high-temperature-resistant tea polyphenol-modified resin fluid loss reducer for drilling fluid as described above, comprising the following steps:

[0012] Tea polyphenols, paraformaldehyde, acetone and water are mixed, and sulfite is used to make the system alkaline, and the mixture is heated to carry out polymerization reaction to obtain a viscous liquid, which is then dried to obtain a tea polyphenol modified resin fluid loss reducer.

[0013] Preferably, specifically, under stirring, 20 to 30 parts by mass of tea polyphenols, 10 to 20 parts by mass of paraformaldehyde and 4 to 6 parts by mass of acetone are added to 100 to 120 parts by mass of water.

[0014] Preferably, the sulfite is anhydrous sodium sulfite, and the amount used is 1 to 2 parts by mass.

[0015] Preferably, the pH value of the system is 10-12, and the temperature of the polymerization reaction is 60-70°C.

[0016] Preferably, the stirring rate is 300-350 rpm; and the polymerization reaction time is 3-5 h.

[0017] The present invention also provides the use of the tea polyphenol modified resin fluid loss reducer as described above in drilling fluid.

[0018] Compared with the prior art, the embodiment of the present invention mainly uses tea polyphenols, acetone and polyformaldehyde to carry out polymerization reaction in the presence of sulfite to obtain a resin product with a branched structure and multiple groups such as condensed rings. The molecular chain of the product is mainly composed of benzene rings, has strong rigidity, and has good temperature resistance; at the same time, the density of the sulfite group is large, and it has a branched structure, which will be beneficial to the adsorption and hydration ability of the molecule at high temperature and improve its salt resistance. The tea polyphenol modified resin described in the present invention has good degradability, does not pollute the environment, and produces good environmental protection effects. It meets the technical requirements of salt-resistant and high-temperature resistant filtration reducers with a wide range of use in the market, and is conducive to its application in drilling fluids. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 This is the infrared spectrum of the modified resin product prepared in Example 1 of the present invention;

[0020] Figure 2 This is the DTA-TG curve of the modified resin product prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0021] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other examples improved or modified by ordinary technicians in this field belong to the scope of protection of the present invention.

[0022] The present invention provides a salt-resistant and high-temperature-resistant tea polyphenol-modified resin fluid loss reducer for drilling fluid, which is prepared by polymerization reaction of tea polyphenol, acetone, sulfite and paraformaldehyde under alkaline conditions;

[0023] The tea polyphenol modified resin fluid loss reducer molecule comprises a condensed ring group, a phenyl group and a sulfite group, and has a branched chain structure.

[0024] The tea polyphenol modified resin product for drilling fluid provided by the present invention has good salt resistance, high temperature resistance and fluid loss reduction performance, can effectively avoid or reduce the occurrence of complex drilling accidents, thereby improving drilling quality and efficiency, and is more environmentally friendly and can meet the technical requirements of salt resistance and fluid loss reducers with a wide range of use in the market.

[0025] The commonly used salt-resistant fluid loss reducers that meet environmental protection requirements have certain deficiencies in performance, and it is difficult to effectively resist salt and high temperature to reduce fluid loss, and it is difficult to ensure the high performance of drilling fluids. For example, the natural polymer fluid loss reducers currently used include natural polymer materials such as cellulose and their modified products.

[0026] Among them, commonly used natural polymers include cellulose, starch, humic acid, lignin, etc. Natural polymer materials have the advantages of wide sources, low prices, and easy biodegradation, but they usually cannot meet actual needs in terms of temperature resistance and salt resistance. Therefore, the natural polymer fluid loss reducers currently used are mostly modified products thereof.

[0027] There are two main ways to modify cellulose. One is to use the hydroxyl groups in the cellulose molecular chain to react with organic compounds for esterification and etherification to obtain modified cellulose-based fluid loss reducers. The other is to use functional monomers for grafting and copolymerization modification of cellulose. For example, modified cellulose grafted with AMPS and DMA has good fluid loss reduction properties in saturated salt water and 150°C.

[0028] The structure of starch is similar to that of cellulose, and the modification methods mainly include grafting, etherification, esterification, carboxylmethylation and cross-linking. The main drawback of this type of fluid loss reducer is that it is easily degraded at high temperatures and has poor temperature resistance. The current means to solve this problem include using 3-chloro-2-hydroxypropyl-trimethylammonium chloride for grafting modification, and the temperature resistance can reach 118°C. In addition, inorganic silicates are introduced into silicified carboxymethyl starch, and the temperature resistance can be increased to 150°C.

[0029] The above-mentioned prior art improves the environmental performance of the fluid loss reducer to a certain extent by modifying the natural polymer materials. However, it is limited by the molecular structure of polysaccharides such as cellulose and starch. It is a long-chain polymer compound composed of many cyclic glucose units, which is easy to break at high temperature and lose the function of the fluid loss reducer. It cannot have both temperature and salt resistance.

[0030] The present invention mainly uses tea polyphenols to prepare resin-based fluid loss additive products, and the tea polyphenol-modified resin product is mainly prepared from the following raw materials: tea polyphenols, paraformaldehyde, acetone and sulfite. The mass ratio of the tea polyphenols, acetone, sulfite and paraformaldehyde is preferably (20-30): (4-6): (1-2): (10-20); for example, the mass ratio can be 25:4:1.5:15, 30:4.5:2:10, 30:5.5:1.5:20. The present invention has no special restrictions on the source of each raw material, and commercially available products can be used.

[0031] Among them, the tea polyphenols (Green Tea Polyphenols, abbreviated as GTP), also known as antioxidant, vitamin polyphenol, and anti-haring, are usually polyphenols extracted from green tea and its by-products as raw materials. The main components are polyphenol complexes such as catechins, flavonoids, and phenolic acids; the content of tea polyphenols is greater than 95%, preferably greater than 97%.

[0032] For example, the tea polyphenols contain 98% phenols and are in brown-red powder form. The tea polyphenols contain 70% to 80% catechins, and the structural formula is shown in Formula 1 below. The chemical formula is C 15 H 14 O6, molecular weight 290.27, melting point 212~216℃.

[0033]

[0034] The molecular structure of catechin contains a large number of benzene rings and active phenolic hydroxyl groups. The benzene rings make it very resistant to high temperatures, and the phenolic hydroxyl groups make it very chemically reactive. Catechins and acetone can react as shown in Formula 2 and Formula 3:

[0035]

[0036] The above intermediate product is further reacted in the presence of paraformaldehyde and sulfite to obtain a product with a branched structure. Preferably, the polymerization degree of the paraformaldehyde is 8 to 12; and the sulfite is preferably anhydrous sodium sulfite.

[0037] This product is the tea polyphenol modified resin described in the present application. Compared with the SMP molecular structure (see Formula 4), its molecular chain is mainly composed of benzene rings, has strong rigidity, and has good temperature resistance. However, at the same time, the tea polyphenol modified resin described in the present application uses acetone as a cross-linking agent, has a high density of sulfite groups, and has a branched structure, which will be beneficial to the adsorption and hydration ability of the molecule at high temperature and improve its salt resistance.

[0038] In the specific examples of the present application, infrared spectroscopy was used to analyze the product structure; the results included: 3421cm -1 It is the absorption peak of the condensed ring contraction vibration; 1650cm -1 It is the stretching vibration absorption peak of CC and CO; 1455cm -1 It is the vibration absorption peak of the benzene ring skeleton; 1170cm -1 and 1141cm -1 is the vibration absorption peak of -SO3-. That is, the tea polyphenol modified resin fluid loss agent molecule includes a condensed ring group, a phenyl group and a sulfite group (also called a sulfonic acid group), and has a branched structure.

[0039] In addition, the tea polyphenol modified resin fluid loss reducer of the present invention has good thermal stability, and its thermal decomposition temperature is higher than 310°C.

[0040] Accordingly, the embodiment of the present invention provides a method for preparing the salt-resistant and high-temperature-resistant tea polyphenol-modified resin fluid loss reducer for drilling fluid as described above, comprising the following steps:

[0041] Tea polyphenols, paraformaldehyde, acetone and water are mixed, and sulfite is used to make the system alkaline, and the mixture is heated to carry out polymerization reaction to obtain a viscous liquid, which is then dried to obtain a tea polyphenol modified resin fluid loss reducer.

[0042] In the reaction kettle, the embodiment of the present invention first adds clean water, then adds tea polyphenols, paraformaldehyde and acetone in a certain mass ratio in sequence, and stirs to dissolve, and then preferably adds sulfite in batches to adjust the pH value of the system to alkaline, and slowly heats to carry out the polymerization reaction.

[0043] Preferably, in the embodiment of the present invention, 20 to 30 parts by mass of tea polyphenols, 10 to 20 parts by mass of paraformaldehyde and 4 to 6 parts by mass of acetone are added to 100 to 120 parts by mass of water under stirring. In addition, the sulfite is preferably anhydrous sodium sulfite, and the amount used can be 1 to 2 parts by mass. The pH value of the system is preferably 10 to 12, for example, 10.5 / 11 / 11.5; the temperature of the polymerization reaction is preferably 60 to 70°C, specifically 60°C, 65°C, 70°C.

[0044] The embodiment of the present invention can obtain a viscous liquid after a certain period of reaction under stirring, and finally the viscous liquid is dried and crushed to obtain a salt-resistant and high-temperature-resistant tea polyphenol resin filtration reducer. The stirring rate can be 300-350rpm; the polymerization reaction time is preferably 3h-5h. In some embodiments of the present application, anhydrous sodium sulfite is added in batches to adjust the pH value to 10.5, slowly heated to 60°C for reaction, and the reaction time is 5h to obtain a viscous liquid. In other embodiments, anhydrous sodium sulfite is added in batches to adjust the pH value to 11.5, slowly heated to 65°C for reaction, and the reaction time is 4h; or, anhydrous sodium sulfite is added in batches to adjust the pH value to 11, slowly heated to 70°C for reaction, and the reaction time is 3h to obtain a viscous liquid.

[0045] In addition, the drying is preferably carried out at 75-80° C.; the obtained powder is the target product, salt-resistant and high-temperature-resistant tea polyphenol resin fluid loss reducer for drilling fluid.

[0046] The present invention also provides the use of the tea polyphenol modified resin fluid loss reducer as described above in drilling fluid. The present invention has no special restrictions on components such as base slurry in the drilling fluid.

[0047] The salt-resistant and high-temperature-resistant tea polyphenol resin fluid loss reducer prepared by the present invention has good performance, see Table 1 at the end of this specification. The performance of the fluid loss reducer product in the embodiment of the present invention is: the water content is ≤10%, the fluid loss at 150℃ high temperature and high pressure after aging of 25% brine at 150℃ is ≤25mL, BOD5 / COD Cr ≥0.25. The tea polyphenol modified resin product of the present invention has good performance, good salt resistance and fluid loss reduction performance, and still shows good temperature resistance and salt resistance after aging at 150°C, which can effectively avoid or reduce the occurrence of complex accidents under high-temperature well conditions, ensure safe drilling, and has good biodegradability and environmental protection function.

[0048] In addition, the process steps of the present invention are relatively simplified, easy to operate, easy to control and implement, and suitable for industrial large-scale production. At the same time, the raw materials of the present invention are easily degradable and will not cause environmental pollution to the land.

[0049] Compared with the prior art, the beneficial effects of the present invention include:

[0050] (1) The salt-resistant and high-temperature-resistant tea polyphenol resin filtrate reducer for drilling fluid of the present invention has good performance, temperature resistance of 150°C, resistance to salt saturation, good compatibility with drilling fluid, good reservoir protection effect, especially in deep well and ultra-deep well drilling operations, has outstanding effects.

[0051] (2) The raw materials for synthesizing the salt-resistant and high-temperature-resistant tea polyphenol resin fluid loss reducer for drilling fluid of the present invention are green, widely available, and cost-effective. The product has good biodegradability and excellent environmental performance.

[0052] (3) The salt-resistant and high-temperature-resistant tea polyphenol resin filtrate reducer for drilling fluid provided by the present invention has mild preparation conditions, simple process, and no secondary pollution.

[0053] In order to further understand the present invention, the salt-resistant and high-temperature-resistant tea polyphenol-modified resin fluid loss reducer for drilling fluid provided by the present application, its preparation method and application are specifically described below in combination with the examples. However, it should be understood that these examples are implemented on the premise of the technical solution of the present invention, and detailed implementation methods and specific operation processes are given only to further illustrate the features and advantages of the present invention, rather than to limit the claims of the present invention, and the protection scope of the present invention is not limited to the following examples.

[0054] The raw materials in the following examples are all commercially available products, among which tea polyphenols were purchased from Xi'an Tianxiang Bioengineering Co., Ltd. The main components are polyphenol complexes such as catechins, flavonoids, and phenolic acids, with a polyphenol content of 98%, catechins accounting for 70% to 80%, and brown-red powder;

[0055] Paraformaldehyde was purchased from Shandong Aldehyde Industry Co., Ltd., CAS No.: 30525-89-4, degree of polymerization 8-12;

[0056] Acetone was purchased from Beijing Yanshan Chemical Co., Ltd. of Sinopec Group, CAS No. 67-64-1;

[0057] Anhydrous sodium sulfite was purchased from Shouguang Boyu Chemical Co., Ltd., with a content of 98% and a CAS number of 7757-83-7.

[0058] In the following examples, the stirring rate (stirrer drilling speed) is 300-350 rpm.

[0059] Embodiment 1:

[0060] The salt-resistant and high-temperature-resistant tea polyphenol resin fluid loss reducer for drilling fluid of the present invention is prepared from the following raw materials in parts by mass: 100 parts of clean water, 25 parts of tea polyphenols, 15 parts of paraformaldehyde, 4.0 parts of acetone and 1.5 parts of anhydrous sodium sulfite.

[0061] The preparation method comprises the following process steps:

[0062] Add 100 parts of clean water into the reactor, and under stirring (the drilling speed of the stirrer is 300-350rpm), add tea polyphenols, paraformaldehyde and acetone in the above-mentioned mass ratio in sequence, add anhydrous sodium sulfite in batches to adjust the pH value to 10.5, slowly heat to 60°C for reaction, the reaction time is 5h, and a viscous liquid is obtained. Finally, the viscous liquid is dried and crushed at a drying temperature of 75°C to obtain a powder, which is a salt-resistant and high-temperature-resistant tea polyphenol resin filtrate reducer for drilling fluid.

[0063] The obtained product was pressed into a tablet with potassium bromide using a Nicolet 6700 infrared spectrometer, and finally analyzed using an infrared spectrometer to obtain an infrared spectrum. Figure 1 shown.

[0064] From the infrared spectrum:

[0065] 3421cm -1 It is the absorption peak of condensed ring contraction vibration;

[0066] 1650cm -1 It is the stretching vibration absorption peak of CC and CO;

[0067] 1455cm -1 It is the vibration absorption peak of the benzene ring skeleton;

[0068] 1170cm -1 and 1141cm -1 It is the vibration absorption peak of -SO3-.

[0069] Obviously, from the infrared spectrum of the product, it can be seen that there are initial molecular designed groups on the product molecular chain, and the four monomers also participate in the reaction, and the synthesized product is the target product.

[0070] The thermal stability of the product was studied using a STA-449F3 differential thermal thermogravimetric analyzer with a heating rate of 10°C / min. Figure 2 .

[0071] Depend on Figure 2 It can be seen that the thermal decomposition of the synthetic product can be divided into three stages:

[0072] The first stage is before 310℃, when the bound water of the product decomposes under heat, and the curve in this temperature range is relatively flat; the second stage is 310℃~340℃, when the epoxy bonds in the product begin to decompose, and the decomposition rate gradually accelerates with the increase of temperature. In this temperature range, the thermal decomposition curve shows a trend close to a vertical decline, and a sharp endothermic valley appears. When it reaches 340℃, the thermal weight loss curve tends to be flat again, indicating that the epoxy bonds have been basically decomposed completely at this time; the third stage is 340℃~550℃, during this stage, the sulfonic acid groups in the product decompose, and the main chain and side chain of the product also begin to break.

[0073] It can be seen from the analysis of the thermogravimetric data that when the temperature reaches 550°C, the mass retention rate of the product is about 41%, that is, the total thermogravimetric loss of the product in the entire test temperature range is about 60%, and the product does not undergo obvious thermal degradation before 310°C. In summary, the product obtained by the present invention has good thermal stability.

[0074] Embodiment 2:

[0075] The salt-resistant and high-temperature-resistant tea polyphenol resin fluid loss reducer for drilling fluid of the present invention is prepared from the following raw materials in parts by mass: 110 parts of clean water, 30 parts of tea polyphenols, 10 parts of paraformaldehyde, 4.5 parts of acetone and 2.0 parts of anhydrous sodium sulfite.

[0076] The preparation method comprises the following process steps:

[0077] Add 110 parts of clean water into the reactor, and under stirring (the drilling speed of the stirrer is 300-350rpm), add tea polyphenols, paraformaldehyde and acetone in the above-mentioned mass ratio in sequence, add anhydrous sodium sulfite in batches to adjust the pH value to 11.5, slowly heat to 65°C for reaction, the reaction time is 4h, and a viscous liquid is obtained. Finally, the viscous liquid is dried and crushed at a drying temperature of 75°C to obtain a powder, which is a salt-resistant and high-temperature-resistant tea polyphenol resin filtrate reducer for drilling fluid.

[0078] Embodiment 3:

[0079] The salt-resistant and high-temperature-resistant tea polyphenol resin fluid loss reducer for drilling fluid of the present invention is prepared from the following raw materials in parts by mass: 120 parts of clean water, 30 parts of tea polyphenols, 20 parts of paraformaldehyde, 5.5 parts of acetone and 1.5 parts of anhydrous sodium sulfite.

[0080] The preparation method comprises the following process steps:

[0081] Add 120 parts of clean water into the reactor, and under stirring (the drilling speed of the stirrer is 300-350rpm), add tea polyphenols, paraformaldehyde and acetone in the above-mentioned mass ratio in sequence, add anhydrous sodium sulfite in batches to adjust the pH value to 11, slowly heat to 70°C for reaction, the reaction time is 3h, and a viscous liquid is obtained. Finally, the viscous liquid is dried and crushed at a drying temperature of 80°C to obtain a powder, which is a salt-resistant and high-temperature-resistant tea polyphenol resin filtrate reducer for drilling fluid.

[0082] Example 4: Drilling Fluid Properties

[0083] The following is the performance test part of the present invention:

[0084] Moisture determination: Use a weighing bottle with known mass that has been dried at 105℃±2℃ for 2h, weigh about 1g~1.5g of filtrate reducer product with an accuracy of 0.0001g, put it in a 105℃±2℃ oven for 4h, take it out, immediately put it in a dryer to cool for 30min, weigh it, and the moisture content is calculated as follows:

[0085] W = (m2-m3) × 100 / (m2-m1);

[0086] Where:

[0087] W——water content, %;

[0088] m1——weight of weighing bottle, g;

[0089] m2——mass of sample and weighing bottle, g;

[0090] m3——Mass of the sample and weighing bottle after drying, g.

[0091] Preparation of base slurry: Measure 350 mL of distilled water and place it in a cup, add 14 g of sodium bentonite for drilling fluid testing and 14 g of evaluation soil, and 0.75 g of anhydrous sodium carbonate, stir at high speed for 20 minutes, stopping at least twice during the process to scrape off the clay adhering to the container wall, and cure in a closed container for 24 hours as the base slurry.

[0092] 25% sodium chloride brine slurry drilling fluid performance test (normal temperature):

[0093] Add 10.5g, 14g and 17.5g of sample to three cups of base slurry respectively and stir at high speed for 20min. Stop at least twice during the process to scrape off the sample adhering to the container wall. Then add 105g of sodium chloride to the three cups respectively and stir at high speed for 10min. Add 8.75g of anhydrous sodium carbonate solution to adjust the pH value of the system. At room temperature, use a medium pressure filter loss meter to measure the water loss.

[0094] 25% sodium chloride brine slurry drilling fluid performance test (150℃ / 16h aging):

[0095] Add 10.5g, 14g and 17.5g of sample to three cups of base slurry respectively, stir at high speed for 20min, stop at least twice during the process to scrape off the sample adhering to the container wall, then add 105g of sodium chloride to the above three cups respectively, stir at high speed for 10min, and add 8.75g of anhydrous sodium carbonate solution to adjust the pH value of the system, transfer the drilling fluid to a high-temperature tank, heat-roll at 150℃ for 16h, take out the high-temperature tank, open it after cooling, stir evenly, and use a high-temperature and high-pressure filter loss instrument to measure the water loss at 150℃.

[0096] BOD5 / COD Cr :Measured in accordance with SY / T6788-2010 "Technical Evaluation Method for Environmental Protection of Water-soluble Oilfield Chemicals" and determined in accordance with SY / T6787-2010 "Technical Requirements for Environmental Protection of Water-soluble Oilfield Chemicals", BOD5 / COD Cr ≥0.05 is readily biodegradable.

[0097] The drilling fluid properties are as follows:

[0098] Table 1 Performance test results of salt-resistant and high-temperature-resistant tea polyphenol resin fluid loss reducer for drilling fluid prepared in each embodiment

[0099]

[0100]

[0101] It can be seen from Table 1 that the amount (weight percentage) of the fluid loss reducer product of the present invention in the 25% salt water base slurry is 3% to 5%; the performance of the product of the present invention is: the water content is ≤10.0%, the medium pressure filtration loss of the 25% salt water base slurry at room temperature is ≤10mL, the high temperature and high pressure filtration loss of 25% salt water after aging at 150℃ is ≤25mL, BOD5 / COD Cr ≥0.25. The salt-resistant and high-temperature-resistant tea polyphenol resin fluid loss reducer for drilling fluid prepared in each embodiment of the present invention can achieve good performance effects, and has both use performance and environmental protection performance for biomass oligophenols, and can meet the use requirements of 150°C well conditions.

[0102] Moreover, the preparation process of the present invention is simplified, easy to operate, and easy to control and implement. At the same time, the raw materials of the present invention are easily degradable and will not cause environmental pollution to the land.

[0103] In summary, the above embodiments of the present invention have good performance. It can effectively resist salt and high temperature and reduce fluid loss, effectively avoid or reduce the occurrence of complex drilling accidents, and improve the quality and efficiency of drilling. After high-temperature aging at 150°C, it still shows good salt resistance, can adapt to complex drilling conditions, and has good temperature resistance and salt resistance. At the same time, it has good degradability, does not pollute the environment, and produces good environmental protection effects, meeting the technical requirements of salt and high temperature resistance fluid loss reducers with a wide range of use in the market.

[0104] The above descriptions are only preferred embodiments of the present invention. It should be pointed out that professionals in this technical field can implement various modifications to these embodiments without departing from the technical principles of the present invention, and these modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A salt-resistant and high-temperature-resistant tea polyphenol-modified resin fluid loss reducer for drilling fluid, characterized in that: It is prepared by polymerization reaction of tea polyphenols, acetone, sulfite and paraformaldehyde under alkaline conditions; The tea polyphenol modified resin fluid loss reducer molecule comprises a condensed ring group, a phenyl group and a sulfite group, and has a branched chain structure.

2. The tea polyphenol modified resin fluid loss reducer according to claim 1, characterized in that: The thermal decomposition temperature of the tea polyphenol modified resin fluid loss reducer is higher than 310°C.

3. The tea polyphenol modified resin fluid loss reducer according to claim 1, characterized in that: The polymerization degree of the paraformaldehyde is 8-12.

4. The tea polyphenol modified resin fluid loss reducer according to any one of claims 1 to 3, characterized in that: The mass ratio of the tea polyphenols, acetone, sulfite and paraformaldehyde is (20-30):(4-6):(1-2):(10-20).

5. The method for preparing the salt-resistant and high-temperature-resistant tea polyphenol-modified resin fluid loss reducer for drilling fluid according to any one of claims 1 to 4, comprising the following steps: Tea polyphenols, paraformaldehyde, acetone and water are mixed, and sulfite is used to make the system alkaline, and the mixture is heated to carry out polymerization reaction to obtain a viscous liquid, which is then dried to obtain a tea polyphenol modified resin fluid loss reducer.

6. The preparation method according to claim 5, characterized in that: Specifically, 20 to 30 parts by mass of tea polyphenols, 10 to 20 parts by mass of paraformaldehyde and 4 to 6 parts by mass of acetone are added to 100 to 120 parts by mass of water under stirring.

7. The preparation method according to claim 6, characterized in that: The sulfite is anhydrous sodium sulfite, and the usage amount is 1 to 2 parts by weight.

8. The preparation method according to claim 7, characterized in that: The pH value of the system is 10-12, and the temperature of the polymerization reaction is 60-70°C.

9. The preparation method according to claim 8, characterized in that: The stirring rate is 300-350 rpm; the polymerization reaction time is 3-5 hours.

10. Use of the tea polyphenol modified resin fluid loss reducer according to any one of claims 1 to 4 in drilling fluid.