Preparation method of amorphous silicon passivation layer for silicon heterojunction solar cell
By adopting RF-PECVD technology in silicon heterojunction solar cells, silicon oxide and intrinsic amorphous silicon thin film are deposited step by step, and hydrogen content is controlled to inhibit epitaxial growth, which solves the problems of epitaxial growth and plasma damage, and improves the battery Open circuit voltage and conversion efficiency.
Patent Information
- Application Number
- CN202110872638.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-07-30
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2041-07-30
AI Technical Summary
Existing silicon heterojunction solar cells are prone to epitaxial growth and plasma damage during the preparation of amorphous silicon passivation layer, which affects the interface passivation effect and leads to a low open circuit voltage of the battery.
Using RF-PECVD technology, first deposit the silicon oxide passivation layer through carbon dioxide gas, then step by step deposit the first and second intrinsic amorphous silicon thin films to control the low hydrogen content to inhibit epitaxial growth, and the deposition process of the second layer Hydrogen gas is introduced into it to passivate the crystalline silicon interface.
It effectively reduces damage to the substrate surface, improves the interface passivation effect, improves the open circuit voltage and conversion efficiency of the battery, and the open circuit voltage reaches more than 745mV, which is more than 0.15% higher than conventional passivation methods.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of silicon heterojunction solar cells, and in particular relates to a method for preparing an amorphous silicon passivation layer of a silicon heterojunction solar cell. Background Art
[0002] Among many types of solar cells, silicon heterojunction solar cells have gradually established a significant advantage in the photovoltaic industry due to their high conversion efficiency, low temperature coefficient, no LID and PID attenuation and other advantages. An important reason for the high efficiency of silicon heterojunction cells is that the excellent passivation effect of the intrinsic amorphous silicon film on the surface of the crystalline silicon substrate ensures the high open circuit voltage of the cell. The passivation effect of the intrinsic amorphous silicon film on the crystalline silicon surface is closely related to the film deposition process. By optimizing the film deposition process to reduce the recombination of carriers at the amorphous silicon / crystalline silicon interface, the interface passivation ability is improved, thereby increasing the open circuit voltage of the cell.
[0003] There are two main methods for preparing the passivation layer in the prior art:
[0004] One method is to use a single layer of intrinsic amorphous silicon film to passivate the crystalline silicon surface. During the deposition process, a large amount of hydrogen is introduced to dilute the silane to reduce the defect density in the film and improve the quality of the film itself. In this method, an epitaxial growth layer is easily formed at the interface between crystalline silicon and intrinsic amorphous silicon. This epitaxial layer will cause a large number of dangling bonds on the interface to be unpassivated, thus causing serious damage to the interface passivation effect.
[0005] The other is to use a laminated intrinsic amorphous silicon film to passivate the crystalline silicon surface. The first layer of intrinsic amorphous silicon film close to the crystalline silicon substrate is a porous structure with poor quality to avoid epitaxy. In order to ensure plasma stability and prepare the first layer of amorphous silicon with a diameter of 3-10nm, the power required for the first layer process is usually 50-80mW / cm 2 Keep it for 20-50s; a large amount of hydrogen is introduced into the second layer of intrinsic amorphous silicon film during the deposition process, and the dangling bonds at the crystalline silicon interface are passivated by hydrogen atoms to achieve a better passivation effect. The higher power of this technology during the deposition of the first layer of amorphous silicon will damage the plasma on the substrate surface, increase the surface defect density of the silicon wafer, and thus seriously affect the passivation performance of the interface between amorphous silicon and crystalline silicon, which is not conducive to the increase of the open circuit voltage of the battery.
[0006] Therefore, it is necessary to develop a method for preparing an amorphous silicon passivation layer for a silicon heterojunction solar cell that can significantly improve the open circuit voltage of the cell and avoid epitaxial growth of the layer. Summary of the invention
[0007] The present invention is based on the inventor's discovery and understanding of the following facts and problems: Since the technical defects of epitaxial growth and plasma damage occur in the existing preparation process of intrinsic amorphous silicon passivation layer, which affects the interface passivation effect, it is necessary to improve the preparation method of intrinsic amorphous silicon film for silicon heterojunction solar cells.
[0008] The present invention aims to solve at least one of the technical problems in the related art to a certain extent. To this end, an embodiment of the present invention provides a method for preparing an amorphous silicon passivation layer of a silicon heterojunction solar cell, which can reduce damage to the substrate surface on the basis of inhibiting epitaxy, reduce interface carrier recombination, and improve the passivation effect.
[0009] The method for preparing an amorphous silicon passivation layer for a silicon heterojunction solar cell according to an embodiment of the present invention comprises the following steps:
[0010] a. Introduce carbon dioxide gas into the reaction chamber containing the silicon wafer to deposit and form a silicon oxide passivation layer;
[0011] b. After forming the silicon oxide passivation layer, introducing silane gas into the reaction chamber to deposit a first intrinsic amorphous silicon film;
[0012] c. After the first intrinsic amorphous silicon film is formed, a mixed gas of silane and hydrogen is introduced into the reaction chamber to deposit a second intrinsic amorphous silicon film.
[0013] Advantages and technical effects of the method for preparing an amorphous silicon passivation layer for a silicon heterojunction solar cell according to an embodiment of the present invention are as follows: 1. In the method of the embodiment of the present invention, RF-PECVD technology is used to prepare an intrinsic amorphous silicon passivation layer by step-by-step deposition, and carbon dioxide is used to perform surface plasma treatment on a silicon wafer sample to form an extremely thin silicon oxide tunneling layer on the surface of the sample, providing the first passivation for the silicon wafer surface; 2. In the method of the embodiment of the present invention, on the basis of the passivation of the silicon oxide tunneling layer formed in the first step, the first intrinsic amorphous silicon film and the second intrinsic amorphous silicon film are deposited in the second and third steps respectively to form a stacked intrinsic amorphous silicon passivation layer, thereby further enhancing the passivation; 3. In the method of the embodiment of the present invention, the first intrinsic amorphous silicon film is deposited in an environment with very low hydrogen content or even without hydrogen. , effectively inhibiting the epitaxial growth of the film; 4. In the method of the embodiment of the present invention, hydrogen is introduced into the second intrinsic amorphous silicon film during the deposition process to passivate the crystalline silicon interface and form a high-quality film; 5. The method of the embodiment of the present invention is simple and easy to operate, and effectively solves the problems of epitaxial growth and high plasma damage in the preparation process of the intrinsic amorphous silicon film. The formed three-layer passivation structure of silicon oxide + double-layer intrinsic amorphous silicon is beneficial to reducing the surface recombination rate at the interface between crystalline silicon and amorphous silicon, and improving the open circuit voltage and conversion efficiency of the battery. The open circuit voltage of the battery passivated by the method of the present invention is above 745mV, and the battery efficiency is increased by more than 0.15% relative to conventional passivation.
[0014] In some embodiments, in step a, the thickness of the silicon oxide passivation layer is 1-5 nm.
[0015] In some embodiments, in step a, the flow rate of the carbon dioxide gas is 1000-5000 sccm, and the deposition power is 10-40 mW / cm 2 , the deposition time is 1-10s.
[0016] In some embodiments, in step b, the deposition power is 20-60 mW / cm 2 , the deposition time is 3-20s, and the silane gas flow rate is 1000-5000sccm.
[0017] In some embodiments, in step b, hydrogen is introduced into the reaction chamber, and the flow ratio of the hydrogen to the silane gas is 0.1-0.5.
[0018] In some embodiments, in step c, the deposition power is 15-50 mW / cm 2 , the deposition time is 5-50s, the hydrogen flow rate is 3000-20000sccm, and the hydrogen to silane flow ratio is 2-25.
[0019] In some embodiments, in the step b, hydrogen plasma treatment is performed after the first intrinsic amorphous silicon film is deposited; and / or, in the step c, hydrogen plasma treatment is performed after the second intrinsic amorphous silicon film is deposited.
[0020] In some embodiments, in step b and / or step c, the hydrogen plasma treatment power is 15-160 mW / cm 2 The range is 5000~25000sccm for hydrogen flow rate and 5~50s for processing time.
[0021] In some embodiments, in the step b, the thickness of the first intrinsic amorphous silicon film is 2 to 10 nm; and / or, in the step c, the thickness of the second intrinsic amorphous silicon film is 3 to 15 nm.
[0022] The embodiment of the present invention also provides a method for preparing an amorphous or microcrystalline silicon-based passivation layer of a silicon heterojunction solar cell, comprising the following steps:
[0023] a. Introduce carbon dioxide gas into the reaction chamber containing the silicon wafer to deposit and form a silicon oxide passivation layer;
[0024] b. After forming the silicon oxide passivation layer, depositing a first intrinsic amorphous or microcrystalline silicon-based thin film;
[0025] c. After the first intrinsic amorphous silicon-based film is formed, a second intrinsic amorphous or microcrystalline silicon-based film is deposited.
[0026] According to the advantages and technical effects of the method for preparing an amorphous or microcrystalline silicon-based passivation layer for a silicon heterojunction solar cell according to an embodiment of the present invention, the method of the embodiment of the present invention first uses carbon dioxide to perform surface plasma treatment on a silicon wafer sample to form an extremely thin silicon oxide tunneling layer on the surface of the sample, providing a first passivation for the silicon wafer surface, which is similar to the advantages of the method for preparing an amorphous silicon passivation layer for a silicon heterojunction solar cell according to an embodiment of the present invention and will not be repeated here.
[0027] In some embodiments, the first or second intrinsic amorphous or microcrystalline silicon-based thin film is a-SiCx:H, μc-SiCx:H, a-SiOx:H or μc-SiOx:H.
[0028] In some embodiments, in step a, the deposition power is 10-40 mW / cm 2 , the deposition time is 1-10s, the flow rate of the carbon dioxide gas is 1000-5000sccm, and the thickness of the silicon oxide passivation layer is 1-5nm. DETAILED DESCRIPTION
[0029] The embodiments described below by reference are exemplary and intended to be used to explain the present invention, but should not be construed as limiting the present invention.
[0030] The method for preparing an amorphous silicon passivation layer for a silicon heterojunction solar cell according to an embodiment of the present invention comprises the following steps:
[0031] a. Introduce carbon dioxide gas into the reaction chamber containing the silicon wafer to deposit and form a silicon oxide passivation layer;
[0032] b. After forming the silicon oxide passivation layer, introducing silane gas into the reaction chamber to deposit a first intrinsic amorphous silicon film;
[0033] c. After the first intrinsic amorphous silicon film is formed, a mixed gas of silane and hydrogen is introduced into the reaction chamber to deposit a second intrinsic amorphous silicon film.
[0034] According to the method for preparing the amorphous silicon passivation layer of the silicon heterojunction solar cell of the embodiment of the present invention, the RF-PECVD technology is used to prepare the intrinsic amorphous silicon passivation layer by step deposition, and the silicon wafer sample is subjected to surface plasma treatment by carbon dioxide to form an extremely thin silicon oxide tunneling layer on the surface of the sample, thereby providing the first passivation for the silicon wafer surface; in the method of the embodiment of the present invention, on the basis of the passivation of the silicon oxide tunneling layer formed in the first step, the first intrinsic amorphous silicon film and the second intrinsic amorphous silicon film are deposited in the second and third steps respectively to form a laminated intrinsic amorphous silicon passivation layer, thereby further enhancing the passivation; in the method of the embodiment of the present invention, the first intrinsic amorphous silicon film is formed at a very low hydrogen content or even without hydrogen. Deposition in a hydrogen environment effectively inhibits the epitaxial growth of the film; in the method of the embodiment of the present invention, hydrogen is introduced into the second intrinsic amorphous silicon film during the deposition process to passivate the crystalline silicon interface and form a high-quality film; the method of the embodiment of the present invention is simple and easy to operate, and effectively solves the problems of epitaxial growth and high plasma damage in the preparation process of the intrinsic amorphous silicon film. The formed three-layer passivation structure of silicon oxide + double-layer intrinsic amorphous silicon is beneficial to reducing the surface recombination rate at the interface between crystalline silicon and amorphous silicon, and improving the open circuit voltage and conversion efficiency of the battery. The open circuit voltage of the battery passivated by the method of the present invention is above 745mV, and the battery efficiency is increased by more than 0.15% relative to conventional passivation.
[0035] In some embodiments, in step a, the thickness of the silicon oxide passivation layer is 1-5 nm, preferably 1-3 nm. The thickness of the silicon oxide passivation layer is optimized in the embodiment of the present invention to further improve the open circuit voltage and fill factor. If the thickness of the silicon oxide passivation layer is too large, the open circuit voltage and fill factor will be significantly reduced.
[0036] In some embodiments, in step a, the deposition power is 10-40 mW / cm 2 , the deposition time is 1-10s; the flow rate of the carbon dioxide gas is 1000-5000sccm. In the embodiment of the present invention, low-power deposition is used to form an extremely thin tunneling silicon oxide passivation layer, providing the first passivation for the surface of the silicon wafer. If the power is too high, it will damage the surface of the substrate and significantly reduce the open circuit voltage of the battery. In the embodiment of the present invention, the flow rate of carbon dioxide gas is preferably selected. If the flow rate is too high, the reaction rate is too fast, making the thickness of the silicon oxide passivation layer difficult to control. If the flow rate is too low, the quality of the silicon oxide film will be reduced, the passivation effect will be reduced, and the open circuit voltage of the battery will be reduced.
[0037] In some embodiments, in step b, the deposition power is 20-60 mW / cm 2, the deposition time is 3-20s, and the silane gas flow rate is 1000-5000sccm. In the embodiment of the present invention, hydrogen can also be introduced into the reaction chamber of step b, and the flow ratio of hydrogen to the silane gas is 0.1-0.5. In the embodiment of the present invention, a trace amount of hydrogen is introduced into step b, which can improve the quality of the film, further enhance the passivation effect, and increase the open circuit voltage and conversion efficiency.
[0038] In some embodiments, in step c, the deposition power is 15-50 mW / cm 2 , the deposition time is 5-50s, the hydrogen flow rate is 3000-20000sccm, and the hydrogen to silane flow rate ratio is 2 to 25. In the embodiment of the present invention, the deposition conditions of the second intrinsic amorphous silicon film are optimized, and the quality of the passivation layer is further improved.
[0039] In some embodiments, in step b, after the first intrinsic amorphous silicon film is deposited, hydrogen plasma treatment is performed; and / or, in step c, after the second intrinsic amorphous silicon film is deposited, hydrogen plasma treatment is performed. Preferably, the hydrogen plasma treatment power is 15-160 mW / cm 2 In the method of the embodiment of the present invention, after the first intrinsic amorphous silicon film and / or the second intrinsic amorphous silicon film are deposited and formed, hydrogen plasma treatment is performed to further saturate dangling bonds and etch weak bonds, thereby reducing the defect state density and increasing the minority carrier lifetime.
[0040] In some embodiments, in the step b, the thickness of the first intrinsic amorphous silicon film is 2 to 10 nm; and / or, in the step c, the thickness of the second intrinsic amorphous silicon film is 3 to 15 nm.
[0041] The embodiment of the present invention also provides a method for preparing an amorphous silicon-based passivation layer of a silicon heterojunction solar cell, comprising the following steps:
[0042] a. Introduce carbon dioxide gas into the reaction chamber containing the silicon wafer to deposit a silicon oxide passivation layer. Preferably, the deposition power is 10-40 mW / cm 2 , the deposition time is 1-10s, the flow rate of carbon dioxide gas is 1000-5000sccm, and the thickness of the deposited silicon oxide passivation layer is 1-5nm, preferably 1-3nm;
[0043] b. After forming the silicon oxide passivation layer, depositing a first intrinsic amorphous or microcrystalline silicon-based thin film;
[0044] c. After the first intrinsic amorphous silicon-based film is formed, a second intrinsic amorphous or microcrystalline silicon-based film is deposited.
[0045] According to the method for preparing an amorphous or microcrystalline silicon-based passivation layer for a silicon heterojunction solar cell according to an embodiment of the present invention, carbon dioxide is first used to perform surface plasma treatment on a silicon wafer sample to form an extremely thin silicon oxide tunneling layer on the sample surface, providing a first passivation for the silicon wafer surface, and then the first and second intrinsic amorphous or microcrystalline silicon-based films are deposited in sequence. The advantages of the method for preparing an amorphous silicon passivation layer for a silicon heterojunction solar cell according to an embodiment of the present invention are similar and will not be repeated here.
[0046] In some embodiments, the first or second intrinsic amorphous or microcrystalline silicon-based film is a-SiCx:H, μc-SiCx:H, a-SiOx:H or μc-SiOx:H. In the embodiments of the present invention, the first or second intrinsic amorphous or microcrystalline silicon-based film can be deposited using existing processes without special restrictions.
[0047] The present invention is described in detail below with reference to embodiments.
[0048] Example 1
[0049] Carbon dioxide gas was introduced into the chamber to perform surface plasma treatment on the silicon wafer sample with a deposition power of 15 mW / cm 2 , the deposition time is 6s, the flow rate of carbon dioxide gas is 2000sccm, and a tunneling silicon oxide passivation layer with a thickness of 1 to 1.2nm is formed on the surface of the sample; after the silicon oxide passivation layer is formed, silane (SiH4) gas is introduced into the reaction chamber to deposit the first intrinsic amorphous silicon film, and the deposition power is 20mW / cm 2 , the deposition time is 4s, the silane gas flow rate is 2000sccm, and the first intrinsic amorphous silicon film with a thickness of 2.5nm is deposited; after the first intrinsic amorphous silicon film is deposited, a mixed gas of silane and hydrogen is introduced into the reaction chamber, and the gas flow rate is adjusted to make the hydrogen to silane flow rate ratio 5, and the second intrinsic amorphous silicon film is deposited, and the deposition power is 35mW / cm 2 The deposition time is 42 s, the hydrogen flow rate is 5000 sccm, and a second intrinsic amorphous silicon film with a thickness of 6 nm is deposited.
[0050] A silicon heterojunction solar cell including the amorphous silicon passivation layer prepared in this embodiment was tested, and the open circuit voltage of the cell was 746.7 mV, and the conversion efficiency was 24.66%.
[0051] Example 2
[0052] The method is the same as that in Example 1, except that carbon dioxide gas is introduced into the chamber, and the deposition power for the surface plasma treatment of the silicon wafer sample is 40 mW / cm 2 , the deposition time is 2s.
[0053] A silicon heterojunction solar cell including the amorphous silicon passivation layer prepared in this embodiment was tested, and the open circuit voltage of the cell was 746.2 mV, and the conversion efficiency was 24.61%.
[0054] Example 3
[0055] The method is the same as that of Example 1, except that the flow rate of carbon dioxide gas introduced into the chamber is 5000 sccm.
[0056] The silicon heterojunction solar cell including the amorphous silicon passivation layer prepared in Example 3 was tested, and the open circuit voltage of the cell was 746.1 mV, and the conversion efficiency was 24.62%.
[0057] Example 4
[0058] The method is the same as that of Example 1, except that the thickness of the silicon oxide passivation layer is 5 nm.
[0059] The silicon heterojunction solar cell including the amorphous silicon passivation layer prepared in Example 4 was tested, and the open circuit voltage of the cell was 745.8 mV, and the conversion efficiency was 24.61%.
[0060] Example 5
[0061] The method is the same as that of Example 1, except that when depositing the first intrinsic amorphous silicon film, a small amount of hydrogen is introduced into the reaction chamber, and the flow ratio of hydrogen to silane gas is 0.2.
[0062] A silicon heterojunction solar cell including the amorphous silicon passivation layer prepared in this embodiment was tested, and the open circuit voltage of the cell was 746.5 mV, and the conversion efficiency was 24.72%.
[0063] Example 6
[0064] The method is the same as that of Example 1, except that after depositing the first intrinsic amorphous silicon film, a mixed gas of silane, hydrogen and carbon dioxide is introduced into the reaction chamber in step c to form a second intrinsic amorphous silicon oxide film.
[0065] A silicon heterojunction solar cell including the silicon-based passivation layer prepared in this embodiment was tested, and the open circuit voltage of the cell was 745.4 mV, and the conversion efficiency was 24.77%.
[0066] Example 7
[0067] The method is the same as that of Example 1, except that after depositing the first intrinsic amorphous silicon film, a mixed gas of silane, hydrogen and methane is introduced into the reaction chamber in step c to form a second intrinsic amorphous silicon carbide film.
[0068] A silicon heterojunction solar cell including the silicon-based passivation layer prepared in this embodiment was tested, and the open circuit voltage of the cell was 745.6 mV, and the conversion efficiency was 24.72%.
[0069] Comparative Example 1
[0070] The method is the same as that of Example 1, except that the step of introducing carbon dioxide to deposit a silicon oxide passivation layer is omitted, and the first intrinsic amorphous silicon film is directly deposited on the surface of the silicon wafer, and then the second intrinsic amorphous silicon film is deposited.
[0071] The silicon heterojunction solar cell including the amorphous silicon passivation layer prepared in Comparative Example 1 was tested, and the open circuit voltage of the cell was 743.2 mV, and the conversion efficiency was 24.48%.
[0072] Comparative Example 2
[0073] The method is the same as that in Example 1, except that the deposition order is different. The first intrinsic amorphous silicon film is first deposited on the surface of the silicon wafer, then carbon dioxide is introduced to deposit a silicon oxide passivation layer, and finally the second intrinsic amorphous silicon film is deposited. The process conditions of each deposition step are the same as those in Example 1.
[0074] The silicon heterojunction solar cell including the amorphous silicon passivation layer prepared in Comparative Example 2 was tested, and the open circuit voltage of the cell was 739 mV, and the conversion efficiency was 24.36%.
[0075] Comparative Example 3
[0076] The method is the same as that in Example 1, except that carbon dioxide gas is introduced into the chamber, and the deposition power for the surface plasma treatment of the silicon wafer sample is 60 mW / cm 2 , the deposition time is 2s.
[0077] The silicon heterojunction solar cell including the amorphous silicon passivation layer prepared in Comparative Example 3 was tested, and the open circuit voltage of the cell was 730 mV, and the conversion efficiency was 24.05%.
[0078] Comparative Example 4
[0079] The method is the same as that of Example 1, except that the thickness of the silicon oxide passivation layer is 8 nm.
[0080] The silicon heterojunction solar cell including the amorphous silicon passivation layer prepared in Comparative Example 4 was tested, and the open circuit voltage of the cell was 722.5 mV, and the conversion efficiency was 22.91%.
[0081] Comparative Example 5
[0082] The method is the same as that of Example 1, except that the flow rate of carbon dioxide gas introduced into the chamber is 8000 sccm.
[0083] The silicon heterojunction solar cell including the amorphous silicon passivation layer prepared in Comparative Example 5 was tested, and the open circuit voltage of the cell was 742.2 mV, and the conversion efficiency was 24.45%.
[0084] In the present invention, the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" etc. mean that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the described specific features, structures, materials or characteristics may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0085] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A method for preparing an amorphous silicon passivation layer for a silicon heterojunction solar cell. It is characterized in that The steps include: a. Introduce carbon dioxide gas into the reaction chamber containing the silicon wafer to deposit a silicon oxide passivation layer, wherein the deposition power is 10-40 mW / cm 2 , the deposition time is 1-10s, and the flow rate of the carbon dioxide gas is 1000-5000sccm; b. After forming the silicon oxide passivation layer, introducing silane gas and hydrogen gas into the reaction chamber to deposit a first intrinsic amorphous silicon thin film, wherein the flow ratio of the hydrogen gas to the silane gas is 0.1-0.5; c. After the first intrinsic amorphous silicon film is formed, a mixed gas of silane and hydrogen is introduced into the reaction chamber to deposit a second intrinsic amorphous silicon film, wherein the deposition power is 15-35 mW / cm 2 , the flow ratio of hydrogen to silane is 2 to 25.
2. The method for preparing an amorphous silicon passivation layer for a silicon heterojunction solar cell according to claim 1, It is characterized in that In the step a, the thickness of the silicon oxide passivation layer is 1-5 nm.
3. The method for preparing an amorphous silicon passivation layer for a silicon heterojunction solar cell according to claim 1, It is characterized in that In step b, the deposition power is 20-60 mW / cm 2 , the deposition time is 3-20s, and the silane gas flow rate is 1000-5000sccm.
4. The method for preparing an amorphous silicon passivation layer for a silicon heterojunction solar cell according to claim 1, It is characterized in that In the step c, the deposition time is 5-50 s, and the flow rate of the hydrogen is 3000-20000 sccm.
5. The method for preparing an amorphous silicon passivation layer for a silicon heterojunction solar cell according to claim 1, It is characterized in that In the step b, a hydrogen plasma treatment is performed after the first intrinsic amorphous silicon film is deposited; and / or, in the step c, a hydrogen plasma treatment is performed after the second intrinsic amorphous silicon film is deposited.
6. The method for preparing an amorphous silicon passivation layer for a silicon heterojunction solar cell according to claim 5, It is characterized in that In step b and / or step c, the hydrogen plasma treatment power is 15-160 mW / cm 2 The range is 5000~25000sccm for hydrogen flow rate and 5~50s for processing time.
7. The method for preparing an amorphous silicon passivation layer for a silicon heterojunction solar cell according to claim 1, It is characterized in that In the step b, the thickness of the first intrinsic amorphous silicon film is 2-10 nm; and / or, in the step c, the thickness of the second intrinsic amorphous silicon film is 3-15 nm.
8. A method for preparing an amorphous or microcrystalline silicon-based passivation layer for a silicon heterojunction solar cell, It is characterized in that The steps include: a. Introduce carbon dioxide gas into the reaction chamber containing the silicon wafer to deposit a silicon oxide passivation layer. The deposition power is 10-40 mW / cm 2 , the deposition time is 1-10s, the flow rate of the carbon dioxide gas is 1000-5000sccm, and the thickness of the silicon oxide passivation layer is 1-5nm; b. After forming the silicon oxide passivation layer, depositing a first intrinsic amorphous or microcrystalline silicon-based thin film; c. After the first intrinsic amorphous silicon-based film is formed, a second intrinsic amorphous or microcrystalline silicon-based film is deposited, wherein the deposition power is 15-35 mW / cm 2 ; Wherein, the first or second intrinsic amorphous or microcrystalline silicon-based film is a-SiCx:H, μc-SiCx:H, a-SiOx:H or μc-SiOx:H.