Preparation method of coating sample for root penetration resistance test of waterproof coating for green roof
By using coating sample preparation method on planting roofs, the problem of lack of root puncture performance test of waterproof coatings in the prior art is solved, and the actual construction conditions are simulated and the test structure is optimized, and the performance detection is met to meet the actual construction needs. .
Patent Information
- Application Number
- CN202111060430.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-09-10
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2041-09-10
AI Technical Summary
The prior art lacks a test method for root puncture resistance performance for planting roof waterproof coatings, which makes it impossible to truly obtain the root puncture resistance performance measurement of the waterproof layer formed by the waterproof coating.
A coating sample preparation method is adopted, including selecting a square sample frame, laying the molded film and pasting it in the sample cavity, dividing it into multiple coating areas and applying waterproof coating in sequence, forming overlapping parts, and forming a molded film. The film is coated and cured under specific environmental conditions, and finally released and put into a test chamber for testing.
This method can simulate the working conditions in which waterproof coating construction cannot be completed in one go, optimize the structure of the coating sample, ensure that the test performance meets actual construction needs, and improve the accuracy and reliability of the test.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of waterproof coatings, and in particular relates to a method for preparing a coating sample for a root penetration resistance test of a waterproof coating for a planted roof. Background Art
[0002] As we all know, waterproof membranes are different from waterproof coatings. In actual use, waterproof membranes need to be overlapped one by one to form a complete waterproof layer on a plane, thereby protecting the main body of the building from external water damage; while waterproof coatings are waterproof layers formed by direct brushing.
[0003] The domestic national standard GB / T 35468-2017 "Root penetration resistant waterproof membrane for green roofs" stipulates the test method for green roofs of waterproof membrane. The first international research on root penetration resistance test was conducted by FLL (German Beautification and Environmental Development Association), which was also aimed at waterproof membrane. Later, the root penetration resistance test method stipulated in the European standard EN 13948:2007 "Flexible waterproof membrane-bituminous, plastic and rubber roofing waterproof membrane-Determination of root penetration resistance" was also developed on the basis of the FLL association test method. It is basically similar to the FLL method, and only stipulates the test of waterproof membrane, and does not involve waterproof coatings.
[0004] Then, for the most important root penetration resistance test of green roof waterproofing materials, the test methods for waterproof coatings and waterproof membranes are also different. This also requires the redesign and research of the root penetration resistance test of waterproof coatings. Therefore, the industry also needs a specimen and test method that can truly obtain the root penetration resistance performance of the waterproof layer formed by the waterproof coating. Summary of the invention
[0005] The technical problem to be solved by the present invention is to overcome the deficiencies of the prior art and provide a method for preparing a coating sample for a root penetration resistance test of a waterproof coating for a planted roof.
[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0007] A method for preparing a coating sample for a root penetration resistance test of a waterproof coating for a planted roof, the method comprising the following steps:
[0008] S1. Select a sample frame, which includes a square frame bottom plate and square side frame plates arranged around the square frame bottom plate, wherein the square side frame plates and the square frame bottom plate form a sample cavity with an open top and a rectangular shape;
[0009] S2. Sample preparation, including: 1) using a formed film to lay and relatively fit the inner wall of the sample cavity, and turn outward from the edge of the open mouth; 2) Forming of the waterproof coating, first divide the inner cavity formed by the formed film into multiple coating areas up and down and left and right, then apply waterproof coating to multiple coating areas in turn, and after each waterproof layer of the coating area is formed, the waterproof coating of the next adjacent coating area is applied, wherein the overlapping part formed between each two adjacent coating areas or three coating areas has a width of L, L ≥ 100mm, and a thickness of H. The thickness of each waterproof layer is equal and is h1, and the number of overlapping layers is N, N = 2 or N = 3, wherein H = 2h1-1; when N = 3, H = 3h1-2; finally, when each coating area forms a waterproof layer, it is cured under the environmental conditions specified in the scope of waterproof coating construction, and the curing time is at least 1 day. At the same time, the waterproof layer, the overlapping part and the formed film constitute a coating sample;
[0010] S3, demoulding, demoulding the above-mentioned coating sample from the sample frame, and placing it in a planting test box with a matching inner cavity to complete the preparation of the coating sample.
[0011] Preferably, when coating each coating area, the coating is carried out in layers, wherein the number of layers is m, m ≥ 2, and is an integer, and after one layer of coating is completed, the next layer of coating is carried out until the thickness of the formed waterproof layer h1 ≥ 2 mm. In this way, the thickness of the formed waterproof layer can meet the test requirements and ensure the accuracy of the test.
[0012] According to a specific implementation and preferred aspect of the present invention, the inner cavity includes an upper sub-cavity located at the upper part, a lower left sub-cavity located at the left side of the lower part, and a lower right sub-cavity located at the lower part, wherein the waterproof layer and the overlapping part are formed in the order of the upper sub-cavity, the lower left sub-cavity, and the lower right sub-cavity or the upper sub-cavity, the lower right sub-cavity, and the lower left sub-cavity. This embodiment is conducive to the molding of the coating sample and is easy to implement to avoid interference or omissions during the upper and lower coatings. At the same time, it can also best simulate the working conditions where the waterproof coating cannot be implemented in one go, so that the obtained test performance meets the actual needs.
[0013] Preferably, the volume of the upper chamber is equal to the sum of the volumes of the lower left chamber and the lower right chamber. In this way, the upper 1 / 2 of the inner chamber is coated first, then the 1 / 4 of one side of the lower part of the inner chamber is coated, and finally the 1 / 4 of the other side of the lower part of the inner chamber is coated. The waterproof layer formed in three steps makes the overlapping part form two layers and three layers, and will not be at the corners and inner corners. At the same time, it can also simulate the most unfavorable use conditions in practice.
[0014] Furthermore, the volumes of the lower left sub-chamber and the lower right sub-chamber are equal.
[0015] According to another specific implementation and preferred aspect of the present invention, before applying the waterproof coating in S2, the corners and inner corners of the inner cavity are rounded with mortar or a suitable material to avoid the corners and inner corners affecting the quality of the coating sample and affecting the final test results.
[0016] Preferably, carcass material is used to perform detailed processing of corners and internal corners.
[0017] According to another specific implementation and preferred aspect of the present invention, when laying the forming film, the forming film is folded at the corners of the sample cavity, and the folded corners are completely covered, and the folded parts are flat, and the forming film is attached to the inner wall, ensuring that the coating sample shape is completely attached to the inner wall of the test box.
[0018] Furthermore, the forming film is selected from a film or paper sheet with certain strength and toughness but no waterproof effect, and will not be damaged when the waterproof coating is applied. In other words, it must not only have certain strength but also no waterproof performance, which is conducive to the coating and forming of the waterproof layer and does not affect the test effect of root penetration resistance in the later stage.
[0019] In this example, a small amount of glue can be used to stabilize the molded film, which also facilitates demoulding.
[0020] In addition, the square frame bottom plate and the square side frame plate are respectively one of metal plates, plastic plates, cardboard or gypsum boards.
[0021] Due to the implementation of the above technical solution, the present invention has the following advantages compared with the prior art:
[0022] The present invention forms a coating sample by sequentially coating a waterproof layer in the coating area in combination with a formed membrane and an overlapping portion, thereby simulating a working condition where the construction of the waterproof coating cannot be completed in one go, and optimizing the structure of the coating sample with the cooperation of the relatively reduced thickness overlapping portion, so that the performance test results of the coating sample finally tested meet the actual construction needs. DETAILED DESCRIPTION
[0023] In order to make the above-mentioned purposes, features and advantages of the present application more obvious and understandable, many specific details are described in the following description to facilitate a full understanding of the present application. However, the present application can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present application, so the present application is not limited by the specific embodiments disclosed below.
[0024] In the description of the present application, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential" and the like to indicate orientations or positional relationships are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.
[0025] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of this application, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.
[0026] In this application, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.
[0027] In the present application, unless otherwise clearly specified and limited, a first feature being “above” or “below” a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being “above”, “above”, and “above” a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being “below”, “below”, and “below” a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.
[0028] It should be noted that when an element is referred to as being "fixed to" or "disposed on" another element, it may be directly on the other element or there may be a central element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be a central element at the same time. The terms "vertical", "horizontal", "upper", "lower", "left", "right" and similar expressions used herein are for illustrative purposes only and are not intended to be the only implementation method.
[0029] The method for preparing a coating sample for a root penetration resistance test of a waterproof coating for a planted roof in this embodiment comprises the following steps:
[0030] S1. Select the sample frame;
[0031] S2, sample preparation;
[0032] S3. Demoulding.
[0033] Specifically, the sample frame in S1 includes a square frame bottom plate and square side frame plates arranged around the square frame bottom plate, wherein the square side frame plates and the square frame bottom plate form a sample cavity with an open top and a rectangular shape.
[0034] In this example, the square frame bottom plate and the square side frame plates are both metal plates, which are not only convenient for assembly but also have a certain supporting hardness.
[0035] Specifically, the sample preparation steps of S2 include:
[0036] 1) The formed film is laid and relatively fitted to the inner wall of the sample cavity, and turned outward from the edge of the open mouth;
[0037] 2) The formation of the waterproof coating, firstly, the inner cavity formed by the forming film is divided into three coating areas up and down and left and right, wherein the inner cavity includes an upper sub-chamber located at the upper part, a lower left sub-chamber located at the left side of the lower part, and a lower right sub-chamber located at the lower part; secondly, the inner wall of the forming film is formed in the order of the upper sub-chamber, the lower right sub-chamber, and the lower left sub-chamber, wherein when coating the upper sub-chamber, a coating layer is formed first, and then two superimposed layers are formed on the coating layer until a waterproof layer with a thickness of 3±0.1mm is formed, and then the waterproof coating is cured under the environmental conditions within the specified range for construction, and the curing time is 7 to 14 days, and then the lower right sub-chamber is coated, and a 3±0.1mm thick waterproof layer is formed by the same coating method, and at the same time, the right The upper part of the lower sub-cavity and the lower part of the upper sub-cavity form two overlapping parts, the width of the overlapping parts is 105±1mm, the thickness of the overlapping parts is 5±0.2mm, and the curing is carried out under the environmental conditions specified in the scope of waterproof coating construction, and the curing time is 7~14 days. Finally, the coating of the lower left sub-cavity is carried out, and the same coating method is adopted to form a 3±0.1mm thick waterproof layer. At the same time, the upper part of the lower left sub-cavity and the lower part of the upper sub-cavity form two overlapping parts, the width of the overlapping parts is 105±1mm, the lower left sub-cavity and the lower right sub-cavity form two layers, and the connecting part with the upper sub-cavity is three layers, of which the thickness of the two overlapping parts is 5±0.2mm, and the thickness of the three overlapping parts is 7±0.3mm. Curing is carried out under the environmental conditions specified in the scope of waterproof coating construction, and the curing time is 7~14 days. Therefore, the three waterproof layers and the corresponding overlapping parts and the formed membrane constitute a waterproof coating (that is, a coating sample).
[0038] In this example, in step 1) of S2, when the forming film is laid, the forming film is folded at the corners of the sample cavity, and the corners are completely covered after folding, and the folded part is flat, and the forming film is attached to the inner wall. Ensure that the coating sample shape is completely attached to the inner wall of the test chamber.
[0039] The forming film is a film or paper that is easily soaked by water and will not be damaged when the waterproof coating is applied. In other words, it must not only have a certain strength, but also a certain water absorption, which is conducive to the application of the waterproof layer.
[0040] In this example, a small amount of glue can be used to stabilize the molded film, which also facilitates demoulding.
[0041] Specifically, the inner cavity includes an upper sub-cavity located at the upper part, a lower left sub-cavity located at the left side of the lower part, and a lower right sub-cavity located at the lower part, wherein the volume of the upper sub-cavity is equal to the sum of the volumes of the lower left sub-cavity and the lower right sub-cavity. In this way, the upper 1 / 2 of the inner cavity is coated first, then the 1 / 4 of one side of the lower part of the inner cavity is coated, and finally the 1 / 4 of the other side of the lower part of the inner cavity is coated. The waterproof layer formed in three times in sequence makes the overlapping part form two layers and three layers, and will not be at the corners and inner corners. At the same time, it can also simulate the worst use conditions.
[0042] In this example, the volumes of the lower left chamber and the lower right chamber are equal.
[0043] At the same time, before applying the waterproof coating on S2, the corners and inner corners of the inner cavity are rounded to avoid the corners and inner corners affecting the quality of the coating sample and affecting the final test results.
[0044] In this case, mortar or matrix material is used to complete the detailed treatment of the corners and internal angles.
[0045] S3, demoulding, demoulding the above-mentioned coating sample from the sample frame, and placing it in a planting test box with a matching inner cavity to complete the preparation of the coating sample.
[0046] Therefore, this embodiment has the following advantages:
[0047] 1. The coating sample formed by the waterproof layer applied in the coating area in sequence, the forming film and the overlapping part can simulate the working condition that the waterproof coating construction cannot be completed in one go, and with the relatively reduced thickness of the overlapping part, the structure of the coating sample is optimized, so that the performance test results of the coating sample finally tested meet the actual construction needs;
[0048] 2. Before applying the waterproof coating, the corners and inner corners of the inner cavity are rounded to avoid the corners and inner corners affecting the quality of the coating sample and affecting the final test results;
[0049] 3. The waterproof layer formed three times in sequence makes the overlapping part form two layers and three layers, and will not be at the corners and inner corners. At the same time, it can also simulate the worst working conditions and further improve the accuracy of the test;
[0050] 4. Selection of forming film and laying of a small amount of adhesive. Fold the forming film at the corners of the sample cavity. After folding, the corners are completely covered, and the folded part is flat. The forming film is attached to the inner wall to ensure that the coating sample shape is completely attached to the inner wall of the test box. At the same time, the forming film will not be damaged when the waterproof coating is applied, and it will not have a waterproof effect. This is conducive to the coating and forming of the waterproof layer and will not affect the effect of the later root penetration resistance test. In addition, a small amount of glue not only improves the stability of the forming film, but also facilitates the subsequent demoulding.
[0051] The above detailed description of the present invention is intended to enable persons familiar with the art to understand the contents of the present invention and implement them. It does not limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a coating sample for a root penetration resistance test of a waterproof coating for a planted roof, characterized in that: The method comprises the following steps: S1. Select a sample frame, which includes a square frame bottom plate and square side frame plates arranged around the square frame bottom plate, wherein the square side frame plates and the square frame bottom plate form a sample cavity with an open top and a rectangular shape; S2. Sample preparation, including: 1) using a formed film to lay and relatively fit the inner wall of the sample cavity, and turn outward from the edge of the open mouth; 2) forming a waterproof coating, firstly dividing the inner cavity formed by the formed film into multiple coating areas up and down and left and right, then coating the multiple coating areas with waterproof coating in sequence, and after each waterproof layer of the coating area is formed, the next adjacent coating area is coated with waterproof coating, wherein the overlapped part formed between each adjacent two coating areas or three coating areas has a width of is L, L≥100mm, the thickness of the overlapping part is Hmm, the thickness of each waterproof layer is equal and is h1mm, the number of overlapping layers is N, N=2 or N=3, where N=2, Hmm=2*h1mm-1mm; when N=3, Hmm=3*h1mm-2mm; finally, when each coating area forms a continuous waterproof coating layer in the entire frame cavity, it is cured under the environmental conditions specified in the construction range of the waterproof coating, and the curing time is at least 1 day. At the same time, the waterproof layer, the overlapping part and the formed film constitute the coating sample; S3, demoulding, demoulding the above-mentioned coating sample from the sample frame, and placing it in a planting test box with a matching inner cavity to complete the preparation of the coating sample.
2. The method for preparing a coating sample for a root penetration resistance test of a waterproof coating for a planted roof according to claim 1, characterized in that: When coating each of the coating areas, the coating is carried out in layers, wherein the number of layers is m, m≥2, and is an integer, and after one layer of coating is completed, the next layer of coating is carried out until the thickness of the formed waterproof layer h1≥2mm.
3. The method for preparing a coating sample for a root penetration resistance test of a waterproof coating for a planted roof according to claim 1, characterized in that: The inner cavity includes an upper sub-chamber located at the upper part, a lower left sub-chamber located at the left side of the lower part, and a lower right sub-chamber located at the lower part, wherein the waterproof layer and the overlapping part are formed in sequence according to the upper sub-chamber, the lower left sub-chamber, and the lower right sub-chamber or in the order of the upper sub-chamber, the lower right sub-chamber, and the lower left sub-chamber.
4. The method for preparing a coating sample for a root penetration resistance test of a waterproof coating for a planted roof according to claim 3, characterized in that: The volume of the upper sub-chamber is equal to the sum of the volumes of the lower left sub-chamber and the lower right sub-chamber.
5. The method for preparing a coating sample for a root penetration resistance test of a waterproof coating for a planted roof according to claim 4, characterized in that: The volumes of the lower left sub-chamber and the lower right sub-chamber are equal.
6. The method for preparing a coating sample for a root penetration resistance test of a waterproof coating for a planted roof according to claim 1, characterized in that: Before applying the waterproof coating on S2, the corners and internal corners of the inner cavity are rounded with mortar or other suitable materials.
7. The method for preparing a coating sample for a root penetration resistance test of a waterproof coating for a planted roof according to claim 5, characterized in that: Use carcass material to do detailed processing of corners and inner corners.
8. The method for preparing a coating sample for a root penetration resistance test of a waterproof coating for a planted roof according to claim 1, characterized in that: When laying the forming film, the forming film is folded at the corners of the sample cavity, and the corners are completely covered after folding, and the folded part is flat, and the forming film is attached to the inner wall.
9. The method for preparing a coating sample for a root penetration resistance test of a waterproof coating for a planted roof according to claim 7, characterized in that: The forming film is a film or paper sheet without waterproof effect, and has certain strength and toughness, and is not easily damaged during the application of waterproof coating.
10. The method for preparing a coating sample for a root penetration resistance test of a waterproof coating for a planted roof according to claim 1, characterized in that: The square frame bottom plate and the square side frame plate are respectively one of metal plates, plastic plates, cardboard or gypsum plates.