Ultrafine electroluminescent fiber and its preparation method and application
Through the composite technology of high-conductive core layer fiber electrode and luminescent powder, ultrafine electroluminescent fibers with fine diameter and high strength were prepared, which solved the problems of existing fiber materials being rough and hard and poor braiding performance, and achieved high brightness and long Lifespan and luminous effects of various colors are suitable for a variety of application scenarios.
Patent Information
- Application Number
- CN202111312835.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-08
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2041-11-08
AI Technical Summary
The existing optical fiber materials are rough and hard, have poor braiding performance, high production cost, and are limited in use scenarios, making it difficult to meet different application needs.
Using the composite technology of high-conductive core layer fiber electrode and luminescent powder, a luminescent slurry is formed by stirring the luminescent powder, solvent, adhesive and dispersant, uniformly coated on the core layer fiber electrode, and loaded on the surface of the electroluminescent layer. The shell conductive components are insulated and packaged to prepare ultrafine electroluminescent fibers with fine diameter, high strength and good flexibility.
It realizes electroluminescent fibers with high luminous brightness, long service life and diverse colors. They are suitable for different weaving methods, low cost and simple process, suitable for industrial production, controllable fiber size, and are suitable for intelligent clothing and pattern decoration.
Smart Images

Figure BDA0003342686070000111 
Figure HDA0003342686080000011 
Figure HDA0003342686080000012
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of textile chemical fibers and relates to an ultrafine electroluminescent fiber and a preparation method and application thereof. Background Art
[0002] In recent years, the application of luminescent materials (mainly luminescent fibers and luminescent fabrics) in clothing has received widespread attention. Clothing containing luminescent materials plays an important role in transportation, fire protection, clothing design, stage performances and other fields. Currently, the luminescent fibers on the market are mostly luminous fibers and fluorescent fibers. They mainly absorb energy through light and then convert it into light radiation. Generally, polyester, nylon or polypropylene is used as the base material, rare earth long afterglow luminescent materials and nano-level functional additives are added, and light conversion functional fibers are made through special spinning processes. The fiber has various colors when there is visible light, and can emit light of various colors when there is no visible light. However, this photoluminescent material has low brightness and short luminescence time, which is difficult to meet the requirements of use.
[0003] Electroluminescent fibers overcome this shortcoming and better meet the requirements of use, such as light-emitting diodes and cold light. Light-emitting diodes (LEDs) have high brightness and bright colors. They can emit light directly using direct current. They are widely used in holiday decorations, luminous advertisements, traffic guidance, instrument indication, digital display, and safety markings. However, light-emitting diodes cannot be made into fibers, so it is difficult to integrate them effectively on fabrics. Another type is optical fibers, which are brightly colored and thin in diameter. However, the brightness of the light gradually decreases with the increase of length, and the flexibility is poor, and it cannot be bent and woven. Cold light (EL line) is a new technology developed in recent years. Its appearance is like a telephone line, and its interior is a "sandwich" structure, that is, the light-emitting layer is sandwiched between the inner and outer electrodes, and the surface is encapsulated with a colored plastic sleeve. It can emit light by AC excitation. The light is soft and uniform, and the colors are diverse. The fiber is relatively soft and bendable, and is used in fire suits, headphones, data cables, etc. However, the diameter of cold light is relatively thick and hard, basically above 0.8mm, which is difficult to weave, and its use on smart fabrics is limited.
[0004] Therefore, it is necessary to develop an electroluminescent fiber with a thin diameter, high strength and good flexibility, and weave it in various ways to obtain luminous fabrics to meet the needs of different scenarios. Summary of the invention
[0005] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art, such as coarse and hard luminescent materials, poor weavability, high preparation cost and limited usage scenarios, and to provide an ultrafine electroluminescent fiber and its preparation method and application.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] A method for preparing an ultrafine electroluminescent fiber comprises the following steps:
[0008] Step 1) mixing luminescent powder, solvent, adhesive and dispersant, and stirring to obtain luminescent slurry;
[0009] Step 2) uniformly coating the luminescent slurry on the surface of the core fiber electrode, and drying to form an electroluminescent layer on the surface of the core fiber electrode;
[0010] Step 3) loading a shell conductive component on the surface of the electroluminescent layer to form a shell conductive layer;
[0011] Step 4) The core fiber electrode loaded with the shell conductive layer obtained in step 3) is insulated and packaged, and then dried and wound to obtain the ultrafine electroluminescent fiber.
[0012] Preferably, the luminescent powder is an inorganic material, specifically a mixture of any one or more of SiO2-based luminescent powder, metal sulfide-type luminescent powder, GaN, and Zn2SiO4;
[0013] The adhesive is a solvent-based adhesive, specifically any one or more of polyvinyl alcohol, polyurethane, vinyl acetate, acrylic adhesive, epoxy water-based adhesive, phenolic water-based adhesive, and silicone water-based adhesive;
[0014] The solvent is ethanol, acetone or deionized water;
[0015] The dispersant is any one or more of water-based silicones, sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, Tween 80, and hexadecyltrimethylammonium chloride;
[0016] The core fiber electrode is any one or more of metal conductive fiber, metal composite fiber and carbon fiber;
[0017] The shell conductive component is any one of silver nanowires, adhesives containing metal particles, metal wires, chemical fibers containing metal particles, and carbon nanofibers.
[0018] Preferably, the SiO2-based luminescent powder is SiO2:Ge or SiO2:Er;
[0019] The metal sulfide luminescent powder is any one of CaS, SrS, ZnS, CaGa2S4, and SrGa2S4;
[0020] The particle size of the luminescent powder is 50nm~100μm;
[0021] The diameter of the core fiber electrode is 100-250 μm, and the conductivity is 10 -2 ~10 2 S / cm;
[0022] When the shell conductive component is silver nanowires or an adhesive containing metal particles, the thickness of the shell conductive layer is 5-20 μm;
[0023] The diameter of the metal wire is 20-100 μm; the diameter of the chemical fiber containing metal particles is 20-100 μm, and the diameter of the carbon nanofiber is 20-100 μm;
[0024] The chemical fiber containing metal particles is any one of copper-plated yarn, tin-plated yarn and stainless steel yarn.
[0025] Preferably, in step 4), the specific operation of the insulating package is: immersing the core fiber electrode loaded with the shell conductive layer in a solvent-based solid transparent resin for 5 to 30 seconds to obtain an insulating layer with a thickness of 5 to 50 μm on the surface of the shell conductive layer.
[0026] Preferably, the weight average molecular weight of the solvent-based solid transparent resin is 50,000 to 200,000;
[0027] The solvent-based solid transparent resin is any one or more of epoxy resin, acrylate resin, polyurethane resin, polytetrafluoroethylene resin, polyvinylidene fluoride resin and silicone resin.
[0028] Preferably, the drying conditions in step 2) are: temperature 60-150° C., time 5-15 s;
[0029] In step 4), the drying temperature is 60 to 150° C. and the winding speed is 5 to 20 m / min.
[0030] Preferably, in the luminescent slurry, the mass ratio of the luminescent powder to the solvent is (1-8):1;
[0031] The thickness of the electroluminescent layer is 10-100 μm.
[0032] An ultrafine electroluminescent fiber obtained based on the preparation method, the diameter of the ultrafine electroluminescent fiber is 0.15-0.5 mm, and the brightness is 20-200 cd / m 2 .
[0033] An application of the ultrafine electroluminescent fiber in the field of textile manufacturing,
[0034] When woven flat, the diameter of the ultrafine electroluminescent fiber is 0.2 to 0.35 mm;
[0035] When woven, the diameter of the ultrafine electroluminescent fibers is 0.3 to 0.4 mm;
[0036] When sewing, the diameter of the ultrafine electroluminescent fiber is 0.35 to 0.5 mm;
[0037] When embroidering, the diameter of the ultrafine electroluminescent fiber is 0.15 to 0.25 mm;
[0038] When knitted, the diameter of the ultrafine electroluminescent fiber is 0.2 to 0.3 mm.
[0039] Compared with the prior art, the present invention has the following beneficial effects:
[0040] The present invention discloses a method for preparing ultrafine electroluminescent fibers, which are composited with a highly conductive core fiber electrode as a carrier and a luminescent material as an active layer through a controllable coating process. By adjusting the ratio of the luminescent slurry and the dip coating process parameters, an electroluminescent fiber with high luminous brightness, long service life and various colors can be obtained. The luminescent fiber prepared by the present invention has a diameter of 0.15-0.5mm and a brightness of 20-200cd / m 2 Adjustable, various colors. The preparation process of the invention is simple, mild, green and environmentally friendly, low cost, and suitable for industrial production. The prepared luminous fiber has controllable size, high brightness, various colors, good flexibility, easy weaving, and wide application.
[0041] The present invention also discloses an ultra-fine electroluminescent fiber, which is obtained based on the above preparation method. The fiber has a luminous brightness of 20 to 200 cd / m 2 Adjustable, service life is 3000h, washable and resistant to friction. The fiber has good flexibility and diameter is adjustable between 0.15mm-0.5mm to meet the needs of different weaving methods. It has high application value in the field of smart clothing and pattern decoration. The luminous fiber can be woven, knitted, sewn, embroidered, knitted, etc. with industrial textile equipment. Its fabric and pattern have both functional indication and aesthetic effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 Schematic diagram of luminescent fiber;
[0043] Figure 2 For embroidering luminous figures;
[0044] Wherein: 1-core conductive fiber; 2-shell conductive fiber; 3-luminescent active layer; 4-resin protective layer. DETAILED DESCRIPTION
[0045] The present invention is further described in detail below in conjunction with the accompanying drawings:
[0046] Example 1
[0047] Step 1: At room temperature 25°C, add 50g SiO2:Ge luminescent powder (diameter 10μm) to 30g ethanol solvent, then add 19.5g polyvinyl alcohol adhesive, 0.5g sodium dodecylbenzene sulfonate surfactant and other additives, and stir magnetically for 30min at a stirring speed of 300rpm to obtain a uniformly dispersed luminescent slurry.
[0048] Step 2: Turn on the dip coating device and evenly coat the luminescent slurry on the surface of the copper wire fiber (diameter 100 μm) at a speed of 10 m / min, then dry it online at 100°C, and finally collect and wind it on a bobbin.
[0049] Step 3: Turn on the external electrode loading device and incorporate the copper wire fiber (30 μm in diameter) into the fiber in a winding manner.
[0050] Step 4: Turn on the packaging device, evenly coat the 50wt% aqueous epoxy resin solution on the fiber surface at a speed of 8m / min, then dry it online at 100°C, and finally collect and wind it on the bobbin. The thickness of the packaging layer is controlled at about 25μm, and the diameter of the final fiber is controlled at 0.2mm.
[0051] Step 5: Turn on the embroidery machine and embroider the luminous fiber on the polyester fabric at an embroidery speed of 400 stitches / min, a top thread tension of 120gf, and a bottom thread tension of 30gf. Then, two electrodes are led out of the luminous sample and lit up with a driving power supply at an effective AC voltage of 80V and a driving frequency of 2000Hz.
[0052] Example 2
[0053] Step 1: At room temperature 25°C, add 40g CaS luminescent powder (diameter 30μm) to 30g acetone solvent, then add 29 polyurethane adhesive, 1.0g hexadecyltrimethylammonium chloride surfactant and other additives, magnetically stir for 20min at a stirring speed of 500rpm to obtain a uniformly dispersed luminescent slurry.
[0054] Step 2: Turn on the dip coating device and evenly coat the luminescent slurry on the surface of the graphene conductive fiber (diameter 200 μm) at a speed of 15 m / min, then dry it online at 150°C, and finally collect and wind it on a bobbin.
[0055] Step 3: Turn on the external electrode loading device, apply the conductive silver paste on the surface of the light-emitting active layer at a speed of 5 m / min, and then dry it online at 100°C.
[0056] Step 4: Turn on the packaging device, evenly coat the 30wt% polyvinylidene fluoride resin solution on the fiber surface at a speed of 10m / min, then dry it online at 150℃, and finally collect and wind it on the bobbin. The thickness of the packaging layer is controlled at about 6μm, and the diameter of the final fiber is controlled at 0.28mm.
[0057] Step 5: Turn on the flat knitting machine and knit the luminous fiber at a speed of 600 needles / min. Then lead out two electrodes of the luminous sample and light it up with a driving power supply at an effective AC voltage of 100V and a driving frequency of 1500Hz.
[0058] Example 3
[0059] Step 1: At room temperature 25°C, add 30g GaN luminescent powder (diameter 10μm) into 30g deionized water, then add 39.6g polyurethane adhesive, 0.4g Tween 80 surfactant, and stir magnetically for 30min at a stirring speed of 400rpm to obtain a uniformly dispersed luminescent slurry.
[0060] Step 2: Turn on the dip coating device and evenly coat the luminescent slurry on the surface of the carbon black conductive fiber (diameter 250 μm) at a speed of 8 m / min, then dry it online at 120°C, and finally collect and wind it on a bobbin.
[0061] Step 3: Turn on the external electrode loading device and incorporate the carbon nanotube fiber multifilament (diameter 20 μm) into the fiber in a parallel arrangement.
[0062] Step 4: Turn on the packaging device, evenly coat the 40wt% acrylic resin solution on the fiber surface at a speed of 5m / min, then dry it online at 80℃, and finally collect and wind it on the bobbin. The thickness of the packaging layer is controlled at about 15μm, and the diameter of the final fiber is controlled at 0.30mm.
[0063] Step 5: Turn on the rapier loom, use the luminous fiber as the warp and the ordinary cotton fiber as the weft, and weave flat, with a density of 30×30 and a speed of 120 turns / min. Then lead out two electrodes of the luminous sample and light it up with a driving power supply at an effective AC voltage of 120V and a driving frequency of 1000Hz.
[0064] Example 4
[0065] Step 1: At room temperature 25°C, add 80g ZnS luminescent powder (diameter 10μm) to 10g ethanol, then add 9.6g polyurethane adhesive, 0.4g sodium dodecyl sulfate surfactant, magnetic stirring for 30min, stirring speed of 400rpm, to obtain a uniformly dispersed luminescent slurry.
[0066] Step 2: Turn on the dipping device and evenly coat the luminescent slurry on the surface of polyester conductive fiber (diameter 200 μm) at a speed of 8 m / min, then dry it online at 120°C, and finally collect and wind it on a bobbin.
[0067] Step 3: Turn on the external electrode loading device and incorporate the carbon nanotube fiber multifilament (diameter 20 μm) into the fiber in a winding manner.
[0068] Step 4: Turn on the packaging device, evenly coat the 40wt% acrylate resin solution on the fiber surface at a speed of 5m / min, then dry it online at 80℃, and finally collect and wind it on the bobbin. The thickness of the packaging layer is controlled at about 15μm, and the diameter of the final fiber is controlled at 0.35mm.
[0069] Step 5: Turn on the household sewing machine and sew the luminous fiber on the cotton fabric at a speed of 500 stitches / min, with a surface thread tension of 100gf and a bottom thread tension of 25gf. Then, two electrodes are led out of the luminous sample and lit up with a driving power supply at an effective AC voltage of 100V and a driving frequency of 2000Hz.
[0070] Example 5
[0071] Step 1: At room temperature 30°C, add 60g Zn2SiO4 luminescent powder (diameter 50nm) to 30g ethanol, then add 9.5g vinyl acetate adhesive, 0.5g sodium dodecyl sulfate surfactant, magnetically stir for 30min at a stirring speed of 400rpm to obtain a uniformly dispersed luminescent slurry.
[0072] Step 2: Turn on the dip coating device and evenly coat the luminescent slurry on the surface of nylon conductive fiber (diameter 140 μm) at a speed of 8 m / min, then dry it online at 120°C, and finally collect and wind it on a bobbin.
[0073] Step 3: Turn on the external electrode loading device and incorporate the stainless steel yarn (20 μm in diameter) into the fiber in a winding manner.
[0074] Step 4: Turn on the encapsulation device, evenly coat the 40wt% polyurethane resin solution on the fiber surface at a speed of 5m / min, then dry it online at 80℃, and finally collect and wind it on the bobbin. The thickness of the encapsulation layer is controlled at about 15μm, and the diameter of the final fiber is controlled at 0.32mm.
[0075] Step 5: Weaving, weaving the luminous fiber and cotton yarn on a weaving machine at a speed of 600 needles / min. Then the luminous sample is led out with two electrodes and lit up with a driving power supply at an effective AC voltage of 100V and a driving frequency of 2000Hz.
[0076] Example 6
[0077] Step 1: At room temperature 30°C, add 68g SrGa2S4 luminescent powder (diameter 100μm) to 10g ethanol, then add 20g α-cyanoacrylate adhesive, 0.2g sodium dodecyl sulfate surfactant, magnetically stir for 30min at a stirring speed of 400rpm to obtain a uniformly dispersed luminescent slurry.
[0078] Step 2: Turn on the dip coating device and evenly coat the luminescent slurry on the surface of the graphene conductive fiber (diameter 180 μm) at a speed of 8 m / min, then dry it online at 120°C, and finally collect and wind it on a bobbin.
[0079] Step 3: Turn on the external electrode loading device and incorporate the copper wire (diameter 40 μm) into the fiber in a winding manner.
[0080] Step 4: Turn on the packaging device, evenly coat the 40wt% polytetrafluoroethylene resin solution on the fiber surface at a speed of 5m / min, then dry it online at 80℃, and finally collect and wind it on the bobbin. The thickness of the packaging layer is controlled at about 15μm, and the diameter of the final fiber is controlled at 0.38mm.
[0081] Step 5: Turn on the household sewing machine and sew the luminous fiber on the cotton fabric at a speed of 500 stitches / min, with a surface thread tension of 100gf and a bottom thread tension of 25gf. Then, two electrodes are led out of the luminous sample and lit up with a driving power supply at an effective AC voltage of 100V and a driving frequency of 2000Hz.
[0082] Example 7
[0083] Step 1: At room temperature 30°C, add 50g SiO2:Er luminescent powder (diameter 500nm) to 10g ethanol, then add 38g polyvinyl formal adhesive and 2g Tween 80 surfactant, stir magnetically for 30min at a stirring speed of 400rpm to obtain a uniformly dispersed luminescent slurry.
[0084] Step 2: Turn on the dipping device and evenly coat the luminescent slurry on the surface of polyester conductive fiber (diameter 220 μm) at a speed of 8 m / min, then dry it online at 120°C, and finally collect and wind it on a bobbin.
[0085] Step 3: Turn on the external electrode loading device and incorporate the carbon nanotube fiber multifilament (diameter 20 μm) into the fiber in a winding manner.
[0086] Step 4: Turn on the encapsulation device, evenly coat the 40wt% polysiloxane solution on the fiber surface at a speed of 5m / min, then dry it online at 80℃, and finally collect and wind it on the bobbin. The thickness of the encapsulation layer is controlled at about 15μm, and the diameter of the final fiber is controlled at 0.45mm.
[0087] Step 5: Turn on the household sewing machine and sew the luminous fiber on the cotton fabric at a speed of 600 stitches / min, with a surface thread tension of 120gf and a bottom thread tension of 30gf. Then, two electrodes are connected to the luminous sample and the driving power supply is used to light it up at an effective AC voltage of 100V and a driving frequency of 2000Hz.
[0088] Example 8
[0089] Step 1: At room temperature 30°C, add 60g CaGa2S4 luminescent powder (diameter 50μm) to 30g ethanol, then add 7g phenolic aqueous adhesive, 3g hexadecyltrimethylammonium chloride surfactant, magnetically stir for 30min at a stirring speed of 400rpm to obtain a uniformly dispersed luminescent slurry.
[0090] Step 2: Turn on the dip coating device and evenly coat the luminescent slurry on the surface of the stainless steel conductive fiber (diameter 130 μm) at a speed of 8 m / min, then dry it online at 120°C, and finally collect and wind it on a bobbin.
[0091] Step 3: Turn on the external electrode loading device and coat the conductive silver paste (particle size 30 nm) on the fiber surface with a coating thickness of 5 μm.
[0092] Step 4: Turn on the packaging device, evenly coat the 40wt% acrylate resin solution on the fiber surface at a speed of 5m / min, then dry it online at 80℃, and finally collect and wind it on the bobbin. The thickness of the packaging layer is controlled at about 15μm, and the diameter of the final fiber is controlled at 0.15mm.
[0093] Step 5: Turn on the embroidery machine and embroider the luminous fiber on the polyester fabric. The embroidery speed is 600 stitches / min, the surface thread tension is 120gf, and the bottom thread tension is 30gf. Then the luminous sample is led out to two electrodes and lit up with a driving power supply at an effective AC voltage of 80V and a driving frequency of 2000Hz.
[0094] Example 9
[0095] Step 1: At room temperature 30°C, add 65g SrS luminescent powder (diameter 1μm) to 15g ethanol, then add 15g polyvinyl alcohol adhesive, 5g sodium dodecyl sulfate surfactant, and stir magnetically for 30min at a stirring speed of 400rpm to obtain a uniformly dispersed luminescent slurry.
[0096] Step 2: Turn on the dip coating device and evenly coat the luminescent slurry on the surface of the copper conductive fiber (diameter 150 μm) at a speed of 8 m / min, then dry it online at 120°C, and finally collect and wind it on a bobbin.
[0097] Step 3: Turn on the external electrode loading device and incorporate the copper-plated yarn (diameter 95 μm) into the fiber in a winding manner.
[0098] Step 4: Turn on the packaging device, evenly coat the 40wt% acrylate resin solution on the fiber surface at a speed of 5m / min, then dry it online at 80℃, and finally collect and wind it on the bobbin. The thickness of the packaging layer is controlled at about 15μm, and the diameter of the final fiber is controlled at 0.35mm.
[0099] Step 5: Turn on the rapier loom, use the luminous fiber as the warp and the ordinary cotton fiber as the weft, and weave flat, with a density of 30×30 and a speed of 120 turns / min. Then lead out two electrodes of the luminous sample and light it up with a driving power supply at an effective AC voltage of 120V and a driving frequency of 1000Hz.
[0100] The above electroluminescent fibers or fabrics were tested for luminous brightness, luminous life, color fastness to washing, and solvent resistance. The luminous performance of the luminescent fiber was tested using a colorimeter; the luminescent fiber was woven into a luminescent fabric, and then the friction resistance of the fabric was tested according to the FZ / T01011-1996 standard; the soaping and sunlight fastness of the fabric was tested using a color fastness meter; the laboratory prepared different solvents to test the solvent resistance, and the test results are shown in Table 1.
[0101] Table 1. Performance test results of ultrafine electroluminescent fibers prepared in Examples 1-4
[0102]
[0103] It can be seen from the results in Table 1 that the ultrafine electroluminescent fiber has good luminescent properties, and different luminescent materials and material-liquid ratios will affect the luminescent effect; the friction resistance of the luminescent fiber mainly depends on the insulating material of the outer packaging, and the packaging material and packaging process selected by the present invention can achieve better friction resistance; in terms of solvent resistance, due to the use of polymer materials, it is easy to be swollen or dissolved by organic solvents and acid solutions, so it can resist alkaline solutions, but not organic solvents and acid solutions.
[0104] It should be noted that the reagents used in the above examples are all purchased reagents, and various solvents are purchased from Sinopharm Chemical Reagent Co., Ltd. Various equipment in the above examples are commercially available equipment. Room temperature refers to an ambient temperature of 10°C-30°C.
[0105] In summary, the luminescent powder, solvent, adhesive, dispersant and other additives are mixed in a certain proportion, and a uniformly dispersed luminescent slurry is obtained after stirring. The high-strength and high-conductive fiber is used as the core electrode. An automated continuous dipping device is used to coat the luminescent slurry on the surface of the core fiber electrode. After online drying, electroluminescence is formed. Another conductive material is loaded onto the surface of the luminescent active layer in a coaxial, parallel or winding form as a shell conductive component. A transparent resin solution is used to insulate and encapsulate the fiber to increase its safety and wear resistance. After online drying, the fiber is wound and collected. According to the diameter and strength of the fiber, a suitable weaving method is selected to meet the requirements of specific scenarios.
[0106] The above contents are only for explaining the technical idea of the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.
Claims
1. A method for preparing an ultrafine electroluminescent fiber, characterized in that: The steps include: Step 1) mixing luminescent powder, solvent, adhesive and dispersant, and stirring to obtain luminescent slurry, wherein the mass ratio of luminescent powder to solvent in the luminescent slurry is (1-8):1; The luminescent powder is an inorganic material, specifically a mixture of any one or more of SiO2-based luminescent powder, metal sulfide-type luminescent powder, GaN, and Zn2SiO4; The solvent is ethanol, acetone or deionized water; The adhesive is a solvent-based adhesive, specifically any one or more of polyvinyl alcohol, polyurethane, vinyl acetate, acrylic adhesive, epoxy water-based adhesive, phenolic water-based adhesive, and silicone water-based adhesive; The dispersant is any one or more of water-based silicones, sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, Tween 80, and hexadecyltrimethylammonium chloride; Step 2) uniformly coating the luminescent slurry on the surface of the core fiber electrode, and drying the electroluminescent layer on the surface of the core fiber electrode, wherein the drying conditions are: temperature 60-150° C., time 5-15s, and the thickness of the electroluminescent layer is 10-100 μm; The core fiber electrode is any one or more of metal conductive fiber, metal composite fiber and carbon fiber; Step 3) loading a shell conductive component on the surface of the electroluminescent layer to form a shell conductive layer; the shell conductive component is incorporated into the core fiber electrode in a winding, coating or parallel arrangement manner; The shell conductive component is any one of silver nanowires, adhesives containing metal particles, metal wires, chemical fibers containing metal particles, and carbon nanofibers; Step 4) The core fiber electrode loaded with a shell conductive layer obtained in step 3) is insulated and packaged, and an ultrafine electroluminescent fiber is obtained after drying and winding, wherein the drying temperature is 60-150°C; the winding speed is 5-20m / min; the specific operation of the insulation packaging is: immersing the core fiber electrode loaded with a shell conductive layer in a solvent-based solid transparent resin for 5-30s, and obtaining an insulating layer with a thickness of 5-50μm on the surface of the shell conductive layer.
2. The method for preparing the ultrafine electroluminescent fiber according to claim 1, characterized in that: SiO2-based luminescent powder is SiO2:Ge or SiO2:Er; The metal sulfide luminescent powder is any one of CaS, SrS, ZnS, CaGa2S4, and SrGa2S4; The particle size of the luminescent powder is 50nm~100μm; The diameter of the core fiber electrode is 100~250μm and the conductivity is 10 -2 ~10 2 S / cm; When the shell conductive component is silver nanowires or an adhesive containing metal particles, the thickness of the shell conductive layer is 5-20 μm; The diameter of the metal wire is 20-100 μm; the diameter of the chemical fiber containing metal particles is 20-100 μm, and the diameter of the carbon nanofiber is 20-100 μm; The chemical fiber containing metal particles is any one of copper-plated yarn, tin-plated yarn and stainless steel yarn.
3. The method for preparing the ultrafine electroluminescent fiber according to claim 1, characterized in that: The weight average molecular weight of the solvent-based solid transparent resin is 50,000 to 200,000; The solvent-based solid transparent resin is any one or more of epoxy resin, acrylate resin, polyurethane resin, polytetrafluoroethylene resin, polyvinylidene fluoride resin and silicone resin.
4. An ultrafine electroluminescent fiber obtained by the preparation method according to any one of claims 1 to 3, characterized in that: The diameter of the ultrafine electroluminescent fiber is 0.15~0.5mm, and the brightness is 20~200cd / m 2 .
5. An application of the ultrafine electroluminescent fiber according to claim 4 in the field of textile manufacturing, characterized in that: When woven flat, the diameter of the ultrafine electroluminescent fiber is 0.2~0.35mm; When woven, the diameter of the ultrafine electroluminescent fibers is 0.3-0.4 mm; When sewing, the diameter of the ultrafine electroluminescent fiber is 0.35~0.5mm; When embroidering, the diameter of the ultrafine electroluminescent fiber is 0.15~0.25mm; When knitted, the diameter of the ultrafine electroluminescent fibers is 0.2~0.3mm.
Citation Information
Cited By
High-performance luminescent fiber driven by safe voltage and preparation method of high-performance luminescent fiber
CN120465167A
A high performance light emitting fiber driven by a safe voltage and a preparation method thereof
CN120465167B