A three-dimensional graphene porous silicon composite negative electrode material and its preparation method and application
Three-dimensional graphene porous silicon composite materials are prepared by combining freeze-drying and magnesia thermal reduction, which solves the problems of pulverization and poor conductivity of silicon anode materials, achieves high cycle stability and high capacity of lithium-ion batteries, and is suitable for industrial production.
Patent Information
- Application Number
- CN202111287611.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-02
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2041-11-02
AI Technical Summary
The silicon anode material in existing lithium-ion batteries is easily pulverized during the lithiation and delithiation processes, resulting in reduced conductivity and attenuation of battery capacity and cycle life. It is also difficult to prepare high-performance three-dimensional graphene-silicon composite materials on a large scale.
Using a method that combines freeze-drying with magnesia-thermal reduction, nano-silica particles are evenly dispersed in a graphene oxide aqueous solution by ultrasonic, and magnesium powder is added and then freeze-dried and calcined at high temperature to form a three-dimensional graphene porous silicon composite material. Ensure that the nano-silica particles are completely covered by graphene to improve the uniformity and dispersion of the material.
The efficient preparation of three-dimensional graphene porous silicon composite materials has been achieved, which significantly improved the cycle stability and reversible capacity of the battery, maintaining a high capacity of 1131mAh g-1 after 500 cycles. The process is simple and low-cost, making it suitable for industrial production.
Smart Images

Figure CN113991056B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of new energy materials and preparation thereof, and relates to a three-dimensional graphene porous silicon composite negative electrode material and a preparation method and application thereof. Background Art
[0002] In recent years, lithium-ion batteries have been used more and more widely, mainly in the fields of consumer electronics and power batteries, and at the same time, users have higher and higher requirements for the performance of lithium-ion batteries. Whether it is the requirements for battery life in the consumer electronics field or the requirements for battery life in power battery applications, higher requirements are placed on the energy density of lithium-ion batteries.
[0003] In order to improve the energy density of lithium-ion batteries, increasing the specific capacity of positive and negative electrode materials is the most effective method. The theoretical capacity limit of traditional graphite negative electrode materials is 372 mAh / g, but in fact, the capacity of graphite negative electrode materials currently used on a large scale is mostly distributed between 350 mAh / g and 365 mAh / g, which is close to the theoretical limit and has limited room for improvement. The theoretical capacity limit of silicon negative electrode materials can reach 4200 mAh / g, which is a significant improvement compared to graphite and has the potential to significantly increase the energy density of lithium-ion batteries. Therefore, silicon materials are considered to be the most promising new generation of lithium-ion battery negative electrode materials to replace graphite because of their ultra-high theoretical lithium storage capacity (4200 mAh / g) and abundant resources.
[0004] However, silicon particles undergo lithiation (forming Li x During the process of adding Si and removing lithium (reforming Si into single substance), severe pulverization will occur to form tiny particles. In addition, the conductivity of silicon particles is relatively poor. After pulverization, more discontinuous small particles are formed, which further weakens the conductivity. These phenomena will eventually lead to a sharp decline in the capacity and cycle life of the battery. The volume expansion effect and poor conductivity have become the main bottlenecks hindering the development of silicon negative electrode materials.
[0005] In order to overcome the above problems and improve the overall electrochemical performance of silicon negative electrodes, people have used a variety of methods to prepare silicon-based electrode materials. An effective strategy is to reduce the size of silicon particles to the nanoscale. Representative nanostructures, including nanowires, nanopores, nanotubes, nanocable arrays, and hollow nanoparticles, can not only reduce the mechanical stress caused by volume changes, but also reduce the transport length of lithium ions and electrons. Porous nanomaterials have attracted much attention due to their low density, large specific surface area, and high porosity. For example, some researchers have prepared nanoporous silicon from metallurgical silicon by ball milling and etching, and some researchers have prepared spherical micron-sized porous silicon with excellent electrochemical properties by SiO2 microemulsion method and magnesium thermal reduction method. However, the surface of nanosilicon is directly exposed to the electrolyte, causing serious side reactions, and there are still great hidden dangers. In addition, due to the low intrinsic conductivity of silicon, it is difficult to avoid capacitance attenuation no matter how the microstructure is designed. Therefore, it is necessary to further introduce conductive materials to improve its electronic conductivity.
[0006] Compared with other carbonaceous materials, graphene has better electrical, thermal and mechanical properties due to its unique atomic layer structure. It has double the theoretical capacity of graphite (744 mAh / g). The results show that by combining graphene with silicon in a certain way, an electrode material with better performance can be obtained, which has become one of the hot topics of current research. Graphene is composed of a layer of carbon atoms in a honeycomb lattice, and it is one of the most ideal conductive substrates due to its super conductivity and flexibility. Among the prepared silicon / graphene composite materials, the most common is the two-dimensional structure material, but silicon-based materials with a three-dimensional graphene coating structure can usually obtain more stable cycle performance. The preparation methods of three-dimensional graphene / nano-silicon composite materials can generally be divided into two categories: the first is to prepare composite materials using commercial nano-silicon particles as raw materials, which is costly and has a small design space; the second is to use SiO2 as a precursor and prepare silicon / graphene composite materials by magnesium thermal reduction, which provides a relatively feasible and low-cost method for converting SiO2 into silicon. However, magnesium thermal reduction reaction usually requires uniform grinding of SiO2 / graphene and magnesium powder, which may destroy the three-dimensional structure formed. In addition, due to the high crystallization barrier of porous silicon nanoparticles, it is difficult to prepare high-performance porous silicon nanoparticles using simple and low-cost methods. Therefore, the large-scale preparation of three-dimensional graphene silicon-based composite materials with excellent performance remains a difficult problem. Summary of the invention
[0007] The purpose of the present invention is to provide a three-dimensional graphene porous silicon composite negative electrode material and a preparation method thereof to overcome the deficiencies of the above-mentioned prior art. The technical contents of the present invention are as follows:
[0008] The present invention discloses a three-dimensional graphene porous silicon composite negative electrode material, comprising a three-dimensional structure composed of graphene and nanoporous silicon particles uniformly dispersed in the three-dimensional structure, wherein the particle size of the nanoporous silicon particles is 1 to 200 nm, the nanoporous silicon is highly dispersed in the three-dimensional structure of the graphene and is completely covered by the graphene, and the nanoporous silicon particles account for 5 to 95% of the weight of the entire composite negative electrode material.
[0009] The present invention also discloses a method for preparing a three-dimensional graphene porous silicon composite negative electrode material, comprising the following steps:
[0010] Step 1: uniformly dispersing nano-silicon dioxide particles in a graphene oxide aqueous solution by ultrasonication, adding magnesium powder and stirring to mix, and then freeze-drying the mixed solution;
[0011] Step 2: The freeze-dried product is calcined at high temperature in an oxygen-free atmosphere to reduce graphene oxide and silicon dioxide. The calcined product is washed and freeze-dried again to obtain a three-dimensional graphene porous silicon composite negative electrode material.
[0012] Furthermore, in step 1 and step 2, the freeze-drying temperature is -80 to 10°C, and the pressure is 0 to 101000Pa.
[0013] Furthermore, the mass ratio of the graphene oxide to nano-silicon dioxide is 1:(0.2-5), the mass ratio of the graphene oxide to water dissolving the graphene oxide is 1:(0.2-5), and the mass ratio of the graphene oxide to magnesium powder is 1:(0.2-5).
[0014] Furthermore, the heating rate of the high temperature calcination is 0.5-40°C / min.
[0015] Furthermore, the temperature of the high temperature calcination is 500-1000°C.
[0016] Furthermore, the oxygen-free atmosphere is nitrogen, argon or a hydrogen-argon mixture with a hydrogen volume fraction of 1 to 20%.
[0017] The present invention also discloses the application of the aforementioned three-dimensional graphene porous silicon composite negative electrode material in the preparation of lithium-ion batteries.
[0018] Furthermore, when the current density is 600 mA g -1 The composite anode material can maintain 1131 mAh g after 500 cycles. -1 reversible capacity.
[0019] Due to the adoption of the above technical solution, the present invention has the following technical effects:
[0020] 1. The present invention creatively adopts a method combining freeze drying and heat treatment (magnesium thermal reduction). The synthesis method is simple and easy, does not require the use of expensive instruments, and does not have cumbersome experimental steps. The raw materials used are abundant, cheap and easy to obtain, the product yield is high, the solvent used can also be recycled, the entire experimental process is efficient, controllable, low cost, and suitable for industrial production.
[0021] 2. In the synthesis process of the present invention, graphene oxide, silicon dioxide and magnesium powder are first mixed evenly and then instantaneously freeze-dried, and then magnesium thermal reduction is performed. Such a preparation process is conducive to achieving the following three effects: First, instantaneous freeze-drying can ensure the uniformity and dispersibility of the material, so that the silicon dioxide particles are fully in contact with the magnesium powder, improve the efficiency of the in-situ magnesium thermal reduction reaction during the heat treatment process, and obtain silicon particles with a porous structure; Third, the instantaneous freeze-drying process is conducive to constructing a three-dimensional porous structure of graphene. Adding magnesium powder before freeze-drying can avoid the destruction of the three-dimensional structure of graphene due to mixing operations such as grinding; Second, during the instantaneous freeze-drying process, graphene oxide shrinks slightly, limiting the silicon-based particles in its three-dimensional structure, and then combined with the further shrinkage and curling of graphene during the heat treatment process, a composite material of three-dimensional graphene-coated silicon-based particles is finally obtained. In short, the above process makes the present invention finally obtain a three-dimensional porous graphene-coated porous nano-silicon composite material, and the porous silicon particles are highly dispersed and uniform in morphology.
[0022] 3. In the composite material synthesized by the present invention, the three-dimensional interconnected network of highly conductive flexible reduced graphene oxide (rGO) sheets and the porous structure of silicon-based particles can alleviate the volume effect of silicon and provide a fast transmission channel for electrons and ions.
[0023] 4. The synthesized three-dimensional graphene / porous silicon composite negative electrode material was used in lithium-ion batteries. When the current density was 600 mAg -1 The optimal capacity is 1131 mAh g after 500 cycles. -1 The high reversible capacity shows excellent cycling stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a SEM image of the three-dimensional graphene / porous silicon composite negative electrode material prepared in Example 1 of the present invention;
[0025] Figure 2 TEM image of the three-dimensional graphene / porous silicon composite negative electrode material prepared in Example 1 of the present invention;
[0026] Figure 3The three-dimensional graphene / porous silicon composite material obtained in Example 1 is used to assemble a lithium-ion battery of the present invention at a current density of 50 mA / g and a voltage range of 0.05 to 2V for the first five charge and discharge curves. DETAILED DESCRIPTION
[0027] All features disclosed in this specification, or steps in all methods or processes disclosed, except mutually exclusive features and / or steps, can be combined in any manner.
[0028] Any feature disclosed in this specification, unless otherwise stated, can be replaced by other equivalent or alternative features with similar purposes. That is, unless otherwise stated, each feature is only an example of a series of equivalent or similar features.
[0029] The invention discloses a three-dimensional graphene porous silicon composite negative electrode material, comprising a three-dimensional structure composed of graphene and nanoporous silicon particles uniformly dispersed in the three-dimensional structure, wherein the particle size of the nanoporous silicon particles is 1 to 200 nm, and the nanoporous silicon particles account for 5 to 95% of the weight of the entire composite negative electrode material.
[0030] The present invention also discloses a method for preparing a three-dimensional graphene porous silicon composite negative electrode material, comprising the following steps:
[0031] Step 1: uniformly dispersing nano-silicon dioxide particles in a graphene oxide aqueous solution by ultrasonication, adding magnesium powder and stirring to mix, and then freeze-drying the mixed solution;
[0032] Step 2: The freeze-dried product is calcined at high temperature in an oxygen-free atmosphere to reduce graphene oxide and silicon dioxide, and the calcined product is washed and freeze-dried again to obtain a three-dimensional graphene porous silicon composite negative electrode material. The washing process can be acid washing and water washing, preferably using 0.1-1 mol / L dilute hydrochloric acid and deionized water for washing.
[0033] As a preferred solution, in step 1 and step 2, the freeze-drying temperature is -80 to 10°C and the pressure is 0 to 101000 Pa. If it is higher than this range, the requirements for instruments and freeze-drying equipment will be very high, thereby greatly increasing the production cost; if it is lower than this range, it will be difficult to ensure the freezing effect.
[0034] As a preferred embodiment, the mass ratio of graphene oxide to nano-silicon dioxide is 1:(0.2-5), the mass ratio of graphene oxide to water for dissolving the graphene oxide is 1:(0.2-5), and the mass ratio of graphene oxide to magnesium powder is 1:(0.2-5). The ratio of graphene oxide to silicon dioxide, the ratio of graphene oxide to water for dissolution (preferably deionized water), and the ratio of graphene oxide to magnesium powder can fully disperse silicon dioxide and magnesium powder in the graphene oxide solution.
[0035] As a preferred solution, the heating rate of the high temperature calcination is 0.5-40°C / min. This heating rate can ensure that the graphene oxide is effectively reduced to graphene without causing obvious expansion effect.
[0036] Further, the temperature of high-temperature calcination can be selected to be 200-1200° C., within this calcination temperature range, graphene oxide can be reduced to graphene, and the reduction effect cannot be achieved below 200° C., and the requirements for calcination equipment will be very high above 1200° C., resulting in increased production costs, and the preferred range is 500-1000° C. Further preferably, the temperature of the high-temperature calcination is 600-700° C., and the calcination time is 7-8 hours.
[0037] As a preferred solution, the oxygen-free atmosphere is nitrogen, argon or a hydrogen-argon mixture with a hydrogen volume fraction of 1 to 20%.
[0038] The graphene oxide mentioned in this specific embodiment can be purchased commercially or prepared by the following method: add 2 to 5 g of potassium persulfate and 2 to 5 g of phosphorus pentoxide to 30 to 100 mL of concentrated sulfuric acid in a water bath at 0 to 20°C, raise the temperature to 60 to 90°C, add 4 to 8 g of flake graphite while stirring, stir for 5 to 6 hours, centrifuge, repeatedly wash with deionized water and dry, then add 100 to 200 mL of concentrated sulfuric acid, add 10 to 20 g of potassium permanganate while stirring, stir for 2 to 4 hours, add 300 to 500 mL of deionized water, stir for another 1 to 2 hours, add 30 to 40 mL of 30% mass concentration of hydrogen peroxide solution, stir for 5 to 20 minutes, centrifuge, repeatedly wash with deionized water and dry to obtain graphene oxide.
[0039] The nano-silicon dioxide mentioned in this specific embodiment can be purchased from a commercial source or prepared by the following method: 5 to 10 mL of 28% ammonia water and 15 to 20 mL of anhydrous ethanol are added to 20 to 30 mL of deionized water, and a mixed solution of 100 mL of anhydrous ethanol and 4 to 6 mL of tetraethyl orthosilicate is added during stirring. Stir for 3 to 4 hours, centrifuge, repeatedly wash with isopropanol and dry to obtain silicon dioxide.
[0040] The specific implementation also involves the application of three-dimensional graphene porous silicon composite negative electrode material in the preparation of lithium-ion batteries. The assembly and testing methods of lithium-ion batteries are as follows:
[0041] The three-dimensional graphene / porous silicon composite negative electrode material of the present invention is mixed with 20 wt.% of a binder (styrene-butadiene rubber-sodium carboxymethyl cellulose emulsion with a solid content of 2 wt.% or a polyvinylidene fluoride N-methylpyrrolidone solution with a concentration of 0.02 g / mL) and 20 wt.% of a conductive agent (Super P conductive carbon black), stirred evenly, coated on a copper foil, and placed in an oven to dry at 60-80°C. Then, a punch with a diameter of 12-16 mm is used to punch out a pole piece, placed in a vacuum oven at 60-120°C for 8-12 hours, and then transferred to a glove box filled with argon. Metal lithium sheet was used as counter electrode, ENTEK PE porous membrane was used as separator, 1 mol / L lithium hexafluorophosphate mixed solution of ethylene carbonate and dimethyl carbonate (volume ratio 1:1) was used as electrolyte, and 10% (volume fraction) fluoroethylene carbonate was added to the electrolyte to assemble CR2016 button cells. Constant current charge and discharge performance tests were carried out on the LAND battery test system (provided by Wuhan Jinnuo Electronics Co., Ltd.). The charge and discharge cut-off voltage relative to Li / Li + 0.05~2 V.
[0042] The electrolyte of the lithium-ion battery is not limited to the mixed solution of ethylene carbonate and dimethyl carbonate of lithium hexafluorophosphate mentioned above, and it can be an electrolyte composed of lithium salt, solvent and electrolyte additive, wherein the lithium salt includes inorganic salts such as lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4) or lithium perchlorate (LiClO4) and organic salts such as lithium bis(oxalate) borate (LiBOB) and lithium bis(trifluoromethylsulfonic acid) imide (LiTFSI), the solvent includes at least one of ethylene carbonate (EC), propylene carbonate (PC), dimethyl carbonate (DMC) and diethyl carbonate (DEC), and the lithium salt concentration in the electrolyte is less than 2 mol / L. The electrolyte additive includes fluoroethylene carbonate (FEC), vinylene carbonate (VC), etc.
[0043] The above scheme is used for a specific example.
[0044] Example 1
[0045] This embodiment relates to a method for preparing a three-dimensional graphene / porous silicon composite negative electrode material, the method comprising the following steps:
[0046] 85.7 mg of silica particles with a particle size of about 100 nm and 45 mg of graphene oxide were ultrasonically dispersed in 30 ml of deionized water, and 137 mg of magnesium powder was added and stirred. After freeze drying at -40 ° C and pressure of 5 Pa for 72 hours, the dried sample was placed in a tube furnace, argon was introduced, and the temperature was increased to 660 ° C at 5 ° C / min for high temperature annealing treatment. The temperature was kept for 7.5 hours to reduce the graphene oxide and silica, and then naturally cooled to room temperature. The product was washed with 0.1-1 mol / L dilute hydrochloric acid and deionized water for many times, and then freeze dried again at -40 ° C and pressure of 5 Pa for 72 hours to obtain a lithium-ion battery silicon graphene composite negative electrode material.
[0047] The SEM image of the three-dimensional graphene porous silicon composite negative electrode material prepared in this embodiment is as follows: Figure 1 As shown in the TEM image Figure 2 As shown in the SEM and TEM images, the three-dimensional structure of the entire composite negative electrode material remains excellent, and the nano-scale silicon particles are evenly distributed. The first five charge and discharge curves of the material at a current density of 50 mA / g in the voltage range of 0.05 to 2V are shown in the figure. Figure 3 shown.
[0048] Example 2
[0049] This embodiment relates to a method for preparing a three-dimensional graphene / porous silicon composite negative electrode material, the method comprising the following steps:
[0050] 85.7 mg of silica particles with a particle size of about 100 nm and 45 mg of graphene oxide were ultrasonically dispersed in 30 ml of deionized water, and 137 mg of magnesium powder was added and stirred. After freeze drying at -40 ° C and pressure of 5 Pa for 72 hours, the dried sample was placed in a tube furnace, argon was introduced, and the temperature was increased to 660 ° C at 5 ° C / min for high temperature annealing treatment. The temperature was kept for 5 hours to reduce the graphene oxide and silica, and then naturally cooled to room temperature. The product was washed with 0.1-1 mol / L dilute hydrochloric acid and deionized water for many times, and then freeze dried again at -40 ° C and pressure of 5 Pa for 72 hours to obtain a lithium-ion battery silicon graphene composite negative electrode material.
[0051] Example 3
[0052] This embodiment relates to a method for preparing a three-dimensional graphene / porous silicon composite negative electrode material, the method comprising the following steps:
[0053] 85.7 mg of silica particles with a particle size of about 100 nm and 45 mg of graphene oxide were ultrasonically dispersed in 30 ml of deionized water, and 137 mg of magnesium powder was added and stirred. After freeze drying at -40 ° C and pressure of 5 Pa for 72 hours, the dried sample was placed in a tube furnace, argon was introduced, and the temperature was increased to 660 ° C at 5 ° C / min for high temperature annealing treatment. The temperature was kept for 10 hours to reduce the graphene oxide and silica, and then naturally cooled to room temperature. The product was washed with 0.1-1 mol / L dilute hydrochloric acid and deionized water for many times, and then freeze dried again at -40 ° C and pressure of 5 Pa for 72 hours to obtain a lithium-ion battery silicon graphene composite negative electrode material.
[0054] Comparative Example 1
[0055] 85.7 mg of silicon dioxide particles with a particle size of about 100 nm and 45 mg of graphene oxide were ultrasonically dispersed in 30 ml of deionized water. After freeze-drying at -40°C and a pressure of 5 Pa for 72 hours, 137 mg of magnesium powder was added to the dried sample and ground and mixed. The mixed sample was then placed in a tube furnace, argon was introduced, and the temperature was increased to 660°C at 5°C / min for high-temperature annealing treatment. The temperature was kept for 7.5 hours to reduce the graphene oxide and silicon dioxide, and then naturally cooled to room temperature. The product was washed with 0.1-1 mol / L dilute hydrochloric acid and deionized water for multiple times and freeze-dried again at -40°C and a pressure of 5 Pa for 72 hours to obtain a lithium-ion battery silicon-graphene composite negative electrode material.
[0056] Comparative Example 2
[0057] 85.7 mg of silicon dioxide particles with a particle size of about 100 nm, 45 mg of graphene oxide, and 137 mg of magnesium powder were ground and mixed. The mixed sample was then placed in a tube furnace, and argon gas was introduced. The temperature was raised to 660°C at 5°C / min for high-temperature annealing treatment. The temperature was kept for 7.5 hours to reduce the graphene oxide and silicon dioxide. The sample was then naturally cooled to room temperature. The product was washed several times with 0.1-1 mol / L dilute hydrochloric acid and deionized water, and then freeze-dried again at -40°C and 5 Pa for 72 hours to obtain a lithium-ion battery silicon-graphene composite negative electrode material.
[0058] Comparative Example 3
[0059] 85.7 mg of silicon dioxide particles with a particle size of about 100 nm and 45 mg of graphene oxide were added to 137 mg of magnesium powder and uniformly dispersed in 30 ml of deionized water. After vacuum drying at 60°C for 72 hours, the dried sample was placed in a tube furnace, argon was introduced, and the temperature was increased to 660°C at 5°C / min for high-temperature annealing treatment. The temperature was kept for 7.5 hours to reduce the graphene oxide and silicon dioxide, and then naturally cooled to room temperature. The product was washed several times with 0.1-1 mol / L dilute hydrochloric acid and deionized water, and then freeze-dried again at -40°C and 5 Pa for 72 hours to obtain a lithium-ion battery silicon-graphene composite negative electrode material.
[0060] The button cell was subjected to a charge and discharge cycle test: the charge and discharge cut-off voltage was 0.05-2.0V, the charge and discharge rate was 600 mA / g, and the specific charge and discharge data are shown in Table 1
[0061]
[0062] From the above, it can be seen that the present invention creatively adopts a method of first mixing magnesium powder with graphene oxide and silicon dioxide and then freeze-drying and heat-treating, which effectively simplifies the reaction process and perfectly ensures the integrity of the three-dimensional structure of the material. The material synthesis method is simple and easy to implement, does not require the use of expensive instruments, and does not have cumbersome experimental steps. The raw materials used are abundant, cheap and easy to obtain, the product yield is high, and the solvents used can also be recycled. The entire experimental process is efficient, controllable, low-cost, simple and environmentally friendly, and suitable for industrial production;
[0063] In the synthesis process of the present invention, the freeze-drying step after the graphene oxide / silicon dioxide / magnesium powder mixture is evenly mixed effectively improves the uniformity and dispersibility of the material, and allows the silicon dioxide particles to directly contact the magnesium powder, further improving the efficiency of magnesium thermal reduction and promoting the construction of a porous structure. In particular, this method can ensure that the three-dimensional graphene-wrapped structure constructed during the freeze-drying process will not be destroyed by the subsequent addition of magnesium powder. The silicon dioxide and magnesium powder are fixed in the shrunken and agglomerated graphene oxide, and then through further heat treatment, the graphene oxide is reduced while the silicon dioxide is reduced to porous silicon. This simplifies the material preparation method and makes the resulting composite material structure stable and uniform in morphology;
[0064] In the composite material synthesized by the present invention, the three-dimensional interconnected network of highly conductive and flexible rGO sheets and the porous structure of silicon-based particles can alleviate the volume effect of silicon and provide a fast transmission channel for electrons and ions: when the synthesized three-dimensional graphene / porous silicon composite negative electrode material is used in a lithium-ion battery, when the current density is 600 mAg -1 After 500 cycles, the optimal capacity can still maintain 1131 mAh g -1.
[0065] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a three-dimensional graphene porous silicon composite negative electrode material, comprising a three-dimensional structure composed of graphene and nanoporous silicon particles uniformly dispersed in the three-dimensional structure, wherein the particle size of the nanoporous silicon particles is 1 to 200 nm, and the nanoporous silicon particles account for 5 to 95% of the weight of the entire composite negative electrode material, characterized in that: The method comprises the following steps: Step 1: uniformly dispersing nano-silicon dioxide particles in an aqueous solution of graphene oxide with ultrasonic wave, adding magnesium powder and stirring to mix well, and then freeze-drying the mixed solution; Step 2: high-temperature calcining the freeze-dried product in an oxygen-free atmosphere to reduce graphene oxide and silicon dioxide, washing the calcined product and freeze-drying it again to obtain a three-dimensional graphene porous silicon composite negative electrode material.
2. The method for preparing the three-dimensional graphene porous silicon composite negative electrode material according to claim 1, characterized in that: In step 1 and step 2, the freeze-drying temperature is -80 to 10°C and the pressure is 0 to 101000 Pa.
3. The method for preparing the three-dimensional graphene porous silicon composite negative electrode material according to claim 1, characterized in that: The mass ratio of the graphene oxide to nano-silicon dioxide is 1:(0.2-5), the mass ratio of the graphene oxide to water in which the graphene oxide is dissolved is 1:(0.2-5), and the mass ratio of the graphene oxide to magnesium powder is 1:(0.2-5).
4. The method for preparing the three-dimensional graphene porous silicon composite negative electrode material according to claim 1, characterized in that: The heating rate of the high temperature calcination is 0.5-40°C / min.
5. The method for preparing the three-dimensional graphene porous silicon composite negative electrode material according to claim 1, characterized in that: The high temperature calcination temperature is 500-1000°C.
6. The method for preparing the three-dimensional graphene porous silicon composite negative electrode material according to claim 5, characterized in that: The high temperature calcination temperature is 600-700° C., and the calcination time is 7-8 hours.
7. The method for preparing the three-dimensional graphene porous silicon composite negative electrode material according to claim 1, characterized in that: The oxygen-free atmosphere is nitrogen, argon or a hydrogen-argon mixed gas with a hydrogen volume fraction of 1 to 20%.
8. Use of the three-dimensional graphene porous silicon composite negative electrode material as claimed in any one of claims 1 to 7 in the preparation of lithium-ion batteries.
9. The use of the three-dimensional graphene porous silicon composite negative electrode material according to claim 8 in the preparation of a lithium ion battery, characterized in that: When the current density is 600mAg -1 The composite anode material can maintain 1131 mAh g after 500 cycles. -1 reversible capacity.