A casting method for solving shrinkage of castings

By casting bolts into bosses and increasing the machining allowance, combined with the use of chilled iron rings and chilled iron blocks, the shrinkage porosity problem in the hot spot area of ​​the casting was solved, improving the finished product quality and yield of the casting.

CN114029454BActive Publication Date: 2024-11-05XIXIA ZHONGDE AUTOMOBILE PART CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111307241.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-05
Publication Date
2024-11-05
Estimated Expiration
2041-11-05

AI Technical Summary

Technical Problem

In existing casting processes, shrinkage defects are prone to occur in the hot spot area at the bolt location, and the inability to install risers leads to low yield, high cost, and quality problems.

Method used

The bolt is cast into a boss, and an allowance machining area is added at the end of the boss away from the central axis of the casting. Cold iron rings and cold iron blocks are set to improve the cooling effect and avoid non-machined areas. The specific shape of the allowance area is determined by MAGMA simulation.

Benefits of technology

It improved the yield rate of the process, solved quality defects such as shrinkage porosity and shrinkage cavities, and reduced production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114029454B_ABST
    Figure CN114029454B_ABST
Patent Text Reader

Abstract

The present invention discloses a casting method for solving the shrinkage problem of castings, which is applied to castings designed with bolts, and the bolts are in an isolated hot spot area. During casting, the bolts are cast into bosses, the middle part of the boss is a threaded hole processing area, and the periphery of the boss is a non-processing area; a residual processing area is extended to increase the end of the boss away from the central axis of the casting, so that the shrinkage area avoids the non-processing area of ​​the boss. The casting method disclosed by the present invention does not need to set a riser, casts the bolts into a boss, and extends to increase the residual processing area at the end of the boss away from the central axis of the casting, so that the shrinkage area of ​​the boss is in the residual processing area and the threaded hole processing area of ​​the boss, avoiding the non-processing area of ​​the boss, thereby ensuring the quality of the finished product, improving the process yield, and solving the problem that the product is prone to shrinkage quality defects due to the inability to place a riser.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of casting, and more particularly to a casting method for solving the problem of shrinkage of castings. Background Art

[0002] Nowadays, automobile parts, such as automobile exhaust pipes or turbocharger housings, are designed with bolts. The bolts are used to facilitate assembly with other parts. When the product is cast, the position where the bolts are connected to the tube wall will form a hot spot. The existing casting production process requires the installation of risers at the hot spot to compensate for the shrinkage of the hot spot through the risers to solve the shrinkage defects of the hot spot. However, this production process has a low process yield and high production cost. It is also necessary to remove the risers and clean them up, which is a cumbersome process. In addition, since the position of the bolts is not fixed, the number of bolts on each product is about 3 to 6. Some bolts can be placed with risers according to the casting parting process, but some bolts are located on the tube wall of the casting. According to the casting parting, these bolts cannot be placed with risers, so it is impossible to avoid shrinkage and other quality defects in the product.

[0003] Therefore, how to provide a casting method that can solve the above problems is a technical problem that technicians in this field urgently need to solve. Summary of the invention

[0004] The purpose of the present invention is to provide a casting method for solving shrinkage of castings, so as to solve the problems of low process yield and high production cost when solving shrinkage defects in hot spots by setting risers; and the problem that risers cannot be set in isolated hot spots, and quality defects such as shrinkage cannot be avoided in finished products.

[0005] The object of the present invention is achieved through the following technical solutions: A casting method for solving the shrinkage of castings, which is applied to castings designed with bolts, and the bolts are in an isolated hot node area. During casting, the bolts are cast into bosses, the middle part of the bosses is a threaded hole processing area, and the periphery of the bosses is a non-processing area;

[0006] An additional processing area is extended at one end of the boss away from the central axis of the casting, so that the shrinkage area avoids the non-processing area.

[0007] Preferably, in the above-mentioned casting method for solving the shrinkage problem of castings, the axial height of the excess processing area is 4 to 8 mm.

[0008] Preferably, in the above-mentioned casting method for solving the shrinkage problem of castings, during the casting molding, a cold iron ring is placed in the circumference of the boss cavity.

[0009] Preferably, in the above-mentioned casting method for solving the shrinkage problem of castings, the thickness of the cooling iron ring is 10 to 20 mm.

[0010] Preferably, in the above-mentioned casting method for solving the shrinkage problem of castings, during the molding of the casting, a chill block is embedded in the core, and the central axis of the chill block is coaxial with the central axis of the boss.

[0011] Preferably, in the above-mentioned casting method for solving the shrinkage problem of castings, the sand separation distance between the boss and the cold iron block is 2 to 3 mm.

[0012] Preferably, in the above-mentioned casting method for solving the shrinkage problem of castings, the specific shape and size of the excess processing area are determined through process simulation.

[0013] Preferably, in the above-mentioned casting method for solving the shrinkage problem of castings, MAGMA simulation software is used to perform process simulation.

[0014] It can be seen from the above technical solution that, compared with the prior art, the present invention discloses a casting method for solving the shrinkage problem of castings. There is no need to set a riser, and the bolts are cast into a boss, and an excess processing area is extended at the end of the boss away from the central axis of the casting, so that the shrinkage area is within the excess processing area and the threaded hole processing area of ​​the boss, avoiding the non-processing area of ​​the boss, thereby ensuring the quality of the finished product, improving the process yield, and solving the problem that the product is prone to quality defects such as shrinkage and shrinkage holes due to the inability to place a riser. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0016] Figure 1 This is the main view of the casting when no machining allowance is added;

[0017] Figure 2 for Figure 1 A partial enlarged view of the shrinkage area;

[0018] Figure 3 It is the side view of the casting when the machining allowance is not increased;

[0019] Figure 4 The front view of the casting when the machining allowance is increased according to the present invention;

[0020] Figure 5 This is a simulation diagram of the shrinkage state of the casting obtained by MAGMA simulation software when the machining allowance is not increased;

[0021] Figure 6 A simulation diagram of the shrinkage state of a casting obtained by MAGMA simulation software when machining allowance is increased for the present invention.

[0022] Figure 1 to Figure 6 middle:

[0023] 1 is the threaded hole processing area, 2 is the non-processing area, 3 is the excess processing area, 4 is the cold iron ring, 5 is the cold iron block, and 6 is the shrinkage area. DETAILED DESCRIPTION

[0024] To make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be described in detail below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other implementation methods obtained by ordinary technicians in this field without creative work belong to the scope of protection of the present invention.

[0025] The following embodiments are described in detail with reference to the accompanying drawings. In addition, the embodiments shown below do not limit the content of the invention described in the claims. In addition, the entire content of the structure represented by the following embodiments is not limited to the solution required as the invention described in the claims.

[0026] Please refer to the attached Figures 1 to 3 and 5

[0027] Comparative Example 1

[0028] The casting method for solving the shrinkage of castings is applied to castings designed with bolts, and the bolts are in an isolated hot zone. During casting, the bolts are cast into bosses, the middle part of the bosses is a threaded hole processing area 1, and the periphery of the bosses is a non-processing area 2;

[0029] During casting, a cold iron ring 4 is placed around the boss cavity; the thickness of the cold iron ring is 15 mm;

[0030] When casting, a chill block 5 is embedded in the core, and the central axis of the chill block 5 is coaxial with the central axis of the boss; the sand separation distance between the boss and the chill block 5 is 2.5 mm.

[0031] Please see attached Figure 4 and 6

[0032] Example 1

[0033] The casting method for solving the shrinkage of castings is applied to castings designed with bolts, and the bolts are in an isolated hot zone. During casting, the bolts are cast into bosses, the middle part of the bosses is a threaded hole processing area 1, and the periphery of the bosses is a non-processing area 2;

[0034] An excess machining area 3 is extended at one end of the boss away from the central axis of the casting; the axial height of the excess machining area 3 is 6 mm;

[0035] During casting, a cold iron ring 4 is placed around the boss cavity; the thickness of the cold iron ring is 15 mm;

[0036] When casting, a chill block 5 is embedded in the core, and the central axis of the chill block 5 is coaxial with the central axis of the boss; the sand separation distance between the boss and the chill block 5 is 2.5 mm.

[0037] Example 2

[0038] The casting method for solving the shrinkage of castings is applied to castings designed with bolts, and the bolts are in an isolated hot zone. During casting, the bolts are cast into bosses, the middle part of the bosses is a threaded hole processing area 1, and the periphery of the bosses is a non-processing area 2;

[0039] An excess machining area 3 is extended at one end of the boss away from the central axis of the casting; the axial height of the excess machining area 3 is 4 mm;

[0040] During casting, a cold iron ring 4 is placed around the boss cavity; the thickness of the cold iron ring is 20 mm;

[0041] When casting, a chill block 5 is embedded in the core, and the central axis of the chill block 5 is coaxial with the central axis of the boss; the sand separation distance between the boss and the chill block 5 is 2 mm.

[0042] Example 3

[0043] The casting method for solving the shrinkage of castings is applied to castings designed with bolts, and the bolts are in an isolated hot zone. During casting, the bolts are cast into bosses, the middle part of the bosses is a threaded hole processing area 1, and the periphery of the bosses is a non-processing area 2;

[0044] An excess machining area 3 is extended at one end of the boss away from the central axis of the casting; the axial height of the excess machining area 3 is 8 mm;

[0045] During casting, a cold iron ring 4 is placed around the boss cavity; the thickness of the cold iron ring is 10 mm;

[0046] When casting, a chill block 5 is embedded in the core, and the central axis of the chill block 5 is coaxial with the central axis of the boss; the sand separation distance between the boss and the chill block 5 is 3 mm.

[0047] The comparison results of the shrinkage area and the quality of the finished casting in Comparative Example 1 with the shrinkage area and the quality of the finished casting in Examples 1 to 3 are shown in Table 1.

[0048] Table 1

[0049]

[0050] Conclusion: In Examples 1 to 3 of the present application, the bolts are cast into bosses, and the excess processing area is increased by extending the end of the boss away from the central axis of the casting, thereby ensuring that the shrinkage area is within the excess processing area and the threaded hole processing area of ​​the boss, avoiding the non-processing area of ​​the boss, thereby ensuring the quality of the finished product, improving the process yield, and solving the problem of quality defects such as shrinkage and shrinkage holes in the product due to the inability to place risers.

[0051] By arranging a cold iron ring on the circumference of the boss and embedding a cold iron block in the core near the connection position between the boss and the tube wall, the cooling rate of the outer periphery of the boss and the cooling rate of the connection between the boss and the tube wall are guaranteed, thereby ensuring that the final shrinkage area has a V-shaped structure and is located at the top center of the excess processing area and the boss threaded hole processing area, so that the shrinkage area cleverly avoids the non-processing area of ​​the boss.

[0052] It should be noted that in Examples 1 to 3, the specific shape and size of the residual processing area 3 are determined through process simulation.

[0053] Furthermore, the process simulation was performed using MAGMA simulation software.

[0054] The specific shape and size of the excess processing area 3 can be determined by process simulation using the MAGMA simulation software, thereby ensuring that the shrinkage area avoids the non-addition area of ​​the boss while minimizing the material used in the excess processing area.

[0055] The present invention discloses a casting method for solving the shrinkage problem of castings. The bolts are cast into bosses without setting risers. A surplus processing area is extended at one end of the boss away from the central axis of the casting. At the same time, a cold iron ring is set in the circumference of the boss. A cold iron block is embedded in the molding sand near the connection position between the boss and the tube wall, thereby ensuring the cooling rate of the periphery of the boss and the cooling rate of the connection between the boss and the tube wall, thereby ensuring that the final shrinkage area has a V-shaped structure and is located at the top center of the surplus processing area and the threaded hole processing area of ​​the boss, so that the shrinkage area cleverly avoids the non-processing area of ​​the boss, thereby ensuring the quality of the finished product, improving the process yield, and solving the problem that the product is prone to shrinkage, shrinkage holes and other quality defects due to the inability to place risers.

[0056] It is understood that the same or similar parts in the above embodiments can refer to each other, and the content not described in detail in some embodiments can refer to the same or similar content in other embodiments. The multiple solutions provided by the present invention include the basic solution itself, which are independent of each other and do not restrict each other, but they can also be combined with each other without conflict to achieve multiple effects together.

[0057] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. A casting method for solving shrinkage of castings, applied to castings designed with bolts, and the bolts are located in an isolated hot spot area, characterized in that: During casting, the bolt is cast into a boss, the middle portion of the boss is a threaded hole processing area (1), and the periphery of the boss is a non-processing area (2); An excess processing area (3) is extended at one end of the boss away from the central axis of the casting, so that the shrinkage area avoids the non-processing area (2); and the shrinkage area is located within the excess processing area (3) and the threaded hole processing area (1) of the boss; The axial height of the excess processing area (3) is 4-8 mm.

2. A casting method for solving casting shrinkage according to claim 1, characterized in that: During casting, a cold iron ring (4) is placed around the boss cavity.

3. A casting method for solving casting shrinkage according to claim 2, characterized in that: The thickness of the cold iron ring (4) is 10-20 mm.

4. A casting method for solving casting shrinkage according to claim 1, characterized in that: During casting molding, a cold iron block (5) is embedded in the core, and the central axis of the cold iron block (5) is coaxial with the central axis of the boss.

5. A casting method for solving shrinkage porosity of castings according to claim 4, characterized in that: The sand separation distance between the boss and the cold iron block (5) is 2-3 mm.

6. A casting method for solving casting shrinkage according to claim 1, characterized in that: The specific shape and size of the excess processing area (3) are determined through process simulation.

7. A casting method for solving casting shrinkage according to claim 1, characterized in that: The process simulation was performed using MAGMA simulation software.