Coated steel wire and method for producing the same
Through the design of zinc alloy plating and double impregnation process, combined with the appropriate cooling rate, the corrosion resistance and processing of galvanized steel wire in severe environments is solved, and the efficient corrosion resistance and processing of coated steel wire is improved. .
Patent Information
- Application Number
- CN201980097811.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-06-26
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2039-06-26
AI Technical Summary
The existing galvanized steel wires are insufficient in severe corrosive environments and have poor processability, making it difficult to meet the needs of industrialization and resource conservation.
Using zinc alloy plating, containing 1.0% to 3.0% Al, 1.0% to 2.0% Mg, 0.5% to 5.0% Fe, Zn/MgZn2/Al ternary eutectic structure and Zn single-phase structure, zinc alloy plating is formed The average thickness is 1/5 to 1/2 of the base wire. The coated wire is made by a hot-dip galvanizing bath and a hot-dip galvanizing alloy bath, and the cooling rate is controlled from 15°C/sec to 50°C/ Second.
It significantly improves the corrosion resistance and processability of the plated steel wire, ensures the adhesion between the zinc alloy coating and the foundation steel wire, prevents cracks and peeling, extends the occurrence time of red rust, and meets the corrosion resistance requirements under severe oxidation environments.
Smart Images

Figure CN114072533B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a plated steel wire and a method of manufacturing the same, and more particularly, to a plated steel wire and a method of manufacturing the same that effectively ensures workability and corrosion resistance. Background Art
[0002] The galvanizing method is excellent in anti-corrosion characteristics and cost-effectiveness, and is therefore widely used to manufacture steel having high corrosion resistance. In particular, hot-dip galvanized steel, in which a coating is formed by immersing steel in a hot-dip galvanizing bath, has a simple manufacturing process and a low product price compared to electrogalvanized steel. Therefore, the demand for hot-dip galvanized steel is increasing in various fields.
[0003] In hot-dip galvanized steel formed with a zinc coating, a sacrificial corrosion protection property is exhibited in which zinc (Zn) having a lower oxidation-reduction potential than iron (Fe) is first corroded when exposed to a corrosive environment and corrosion of the steel is suppressed, and the steel is protected from an oxidizing atmosphere by dense corrosion products formed on the surface of the steel as Zn of the zinc coating is oxidized. Therefore, the corrosion resistance of the steel can be effectively improved.
[0004] However, with high industrialization, air pollution has increased and the deterioration of the corrosive environment has accelerated, and due to strict regulations on resource and energy conservation, the demand for developing steel having corrosion resistance superior to that of conventional galvanized steel has increased.
[0005] In order to meet such a demand, Zn-Al alloy plated steel wire has been developed. Generally, Zn-Al alloy plated steel wire can be manufactured by subjecting the steel wire to a cleaning operation such as pickling, washing or degreasing, subjecting the cleaned steel wire to a flux treatment for interfacial reaction activation with zinc, and then immersing the steel wire in a Zn-based plating bath containing Al.
[0006] (Related technical literature)
[0007] (Patent Document) Korean Patent Publication No. 10-2016-0078670 (published on July 5, 2016)
[0008] Public Content
[0009] Technical issues
[0010] One aspect of the present disclosure may provide a plated steel wire effectively ensuring workability and corrosion resistance, and a method of manufacturing the same.
[0011] The purpose of the present disclosure is not limited to the above description. It will not be difficult for those skilled in the art to understand the other purposes of the present disclosure based on the overall description of this specification.
[0012] Technical Solution
[0013] According to one aspect of the present disclosure, a coated steel wire includes: a base steel wire and a zinc alloy coating, wherein the zinc alloy coating contains, by weight%, 1.0% to 3.0% Al, 1.0% to 2.0% Mg, 0.5% to 5.0% Fe, and the balance Zn and inevitable impurities, the zinc alloy coating contains a Zn / MgZn2 / Al ternary eutectic structure, a Zn single-phase structure, and a Fe-Zn-Al based crystal structure, and the Fe-Zn-Al based crystal structure is formed adjacent to the base steel wire and has an average thickness of 1 / 5 to 1 / 2 of the average thickness of the zinc alloy coating.
[0014] In a cross section of the zinc alloy plating layer, an area fraction occupied by the Zn single phase structure in an area occupied by the Zn / MgZn2 / Al ternary eutectic structure and the Zn single phase structure may be 60% or more.
[0015] In a cross section of the zinc alloy plating layer, an average distance between columnar crystals in the Zn single-phase structure may be 1 μm to 5 μm.
[0016] According to another aspect of the present disclosure, a method for manufacturing a coated steel wire includes: primarily dipping a base steel wire in a hot-dip galvanizing bath to provide a galvanized steel wire; secondarily dipping the primarily dipped galvanized steel wire in a hot-dip galvanizing alloy bath to provide a galvanized alloy steel wire; and cooling the secondarily dipped galvanized alloy steel wire at a cooling rate of 15°C / sec to 50°C / sec, wherein the hot-dip galvanizing alloy bath contains, by weight%, 1.0% to 3.0% Al, 1.0% to 2.0% Mg, and the balance Zn and unavoidable impurities.
[0017] The base steel wire may be initially dipped in a hot dip galvanizing bath at 440° C. to 460° C. for 10 seconds to 20 seconds.
[0018] The primary dipped galvanized steel wire may be cooled to a temperature equal to or lower than the melting point of Zn, and the cooled galvanized steel wire may be secondary dipped in a hot-dip zinc alloy bath.
[0019] The galvanized steel wire may be secondary dipped in a hot-dip galvanizing alloy bath at 440°C to 460°C for 10 seconds to 20 seconds.
[0020] Beneficial Effects
[0021] As described above, according to an exemplary embodiment in the present disclosure, a plated steel wire having effectively improved processability and corrosion resistance and a method for manufacturing the same may be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is a FE-SEM image obtained by observing the cross section of Inventive Example 1.
[0023] Figure 2 This is a FE-SEM image obtained by observing the surface of the plated layer of Inventive Example 1.
[0024] Figure 3 This is a FE-SEM image obtained by observing the cross section of Comparative Example 1.
[0025] Figure 4 This is a FE-SEM image obtained by observing the surface of the plated layer of Comparative Example 1.
[0026] Figure 5 This is a SEM image obtained by observing the surface of Invention Example 1 after wire drawing.
[0027] Figure 6 This is a SEM image obtained by observing the surface of Comparative Example 1 after wire drawing. DETAILED DESCRIPTION
[0028] The present disclosure relates to coated steel wire and a method for manufacturing the same. Hereinafter, preferred exemplary embodiments in the present disclosure will be described. The exemplary embodiments in the present disclosure may be modified in various forms, and the scope of the present disclosure should not be construed as being limited to the exemplary embodiments set forth below. These exemplary embodiments are provided to describe the present disclosure in more detail to those skilled in the art to which the present disclosure belongs.
[0029] The coated steel wire according to one aspect of the present disclosure may include a base steel wire and a zinc alloy coating. The base steel wire of the present disclosure is not limited to a specific type of steel wire and may be construed to include all types of steel wires for hot-dip galvanizing or hot-dip galvanneal coating.
[0030] Furthermore, the zinc alloy plating layer of the plated steel wire according to one aspect of the present disclosure may include, by weight %, 1.0% to 3.0% Al, 1.0% to 2.0% Mg, 0.5% to 5.0% Fe, and the balance of Zn and inevitable impurities.
[0031] Hereinafter, the composition of the zinc alloy plating layer of the present disclosure will be described in more detail. Hereinafter, unless otherwise specifically stated, % related to the alloy composition content refers to weight %.
[0032] Mg: 1.0% to 2.0%
[0033] Mg is an element that plays a very important role in improving the corrosion resistance of zinc alloy coatings. Mg is included in the zinc alloy coating, so that the generation of zinc oxide-based corrosion products with a small corrosion resistance improvement effect in severe corrosive environments can be suppressed, and zinc hydroxide-based corrosion products that are dense and have a large corrosion resistance improvement effect can be stabilized on the surface of the coating. Therefore, in order to achieve these effects, the Mg content of the present disclosure may be 1.0% or more. However, when the added Mn content is too much, the corrosion resistance improvement effect according to the addition of Mg is saturated, and the oxidized slag generated by the oxidation of Mg increases rapidly at the liquid level of the hot-dip zinc alloy bath. Therefore, the Mg content of the present disclosure may be 2.0% or less.
[0034] Al: 1.0% to 3.0%
[0035] Al is an element added to reduce the slag produced by the oxidation reaction of Mg in a hot-dip galvanizing alloy bath to which Mg is added. In addition, Al is an element that can be combined with Zn and Mg to improve the corrosion resistance of the plated steel wire. Therefore, in order to achieve these effects, the Al content of the present disclosure may be 1.0% or more. The preferred Al content may be 1.5% or more. However, when the Al content added is too much, the amount of Fe eluted from the steel wire immersed in the hot-dip galvanizing alloy bath increases rapidly, and thus Fe alloy-based slag may be produced. In addition, an Al-Zn metal structure is formed in the hot-dip galvanizing alloy bath, so the temperature of the plating bath increases, and the Al-Zn metal structure formed in the zinc alloy coating may inhibit the processability of the zinc alloy coating. Therefore, the Al content of the present disclosure may be 3.0% or less. The preferred Al content may be 2.8% or less.
[0036] Fe: 0.5% to 5.0%
[0037] The Fe contained in the zinc alloy coating of the present disclosure is an element introduced into the zinc alloy coating by Fe-Zn formed by the reaction of Fe in the base steel wire with Zn in the hot-dip galvanizing alloy bath. The present disclosure aims to ensure the adhesion of the coating by forming a crystal structure based on Fe-Zn-Al at the interface portion of the zinc alloy coating. Therefore, the Fe content contained in the zinc alloy coating of the present disclosure may be 0.5% or more, and the preferred Fe content may be 0.8% or more. On the other hand, when the Fe content introduced into the zinc alloy coating is too much, the hardness of the zinc alloy coating may be excessively increased, and a phenomenon in which local corrosion resistance is reduced may occur. Therefore, the Fe content contained in the zinc alloy coating of the present disclosure may be 5.0% or less, and the preferred Fe content may be 4.3% or less.
[0038] The zinc alloy coating of the present disclosure may contain a balance of Zn and other unavoidable impurities. Unavoidable impurities from raw materials or the surrounding environment are inadvertently incorporated during the ordinary steel manufacturing process and may not be completely eliminated. Since these impurities can be recognized by those skilled in the art during the ordinary steel manufacturing process, all of them are not specifically described in the present disclosure.
[0039] Hereinafter, the metal structure of the zinc alloy plating layer of the present disclosure will be described in more detail.
[0040] The zinc alloy coating of the present disclosure may include a Zn / MgZn2 / Al ternary eutectic structure, a Zn single phase structure, and a crystal structure based on Fe-Zn-Al. The crystal structure based on Fe-Zn-Al may be formed adjacent to the base steel wire and may have an average thickness of 1 / 5 to 1 / 2 of the average thickness of the zinc alloy coating. That is, the crystal structure based on Fe-Zn-Al is formed from the interface with the base steel wire to a region of 1 / 5 to 1 / 2 of the average thickness of the zinc alloy coating, so that the adhesion between the zinc alloy coating and the base steel wire can be effectively ensured. Therefore, when the plated steel wire of the present disclosure is processed, cracks in the zinc alloy coating or peeling of the zinc alloy coating can be effectively prevented, so that the plated steel wire of the present disclosure can ensure excellent processability.
[0041] In the cross section of the zinc alloy coating, the area fraction occupied by the Zn single-phase structure in the area occupied by the Zn / MgZn2 / Al ternary eutectic structure and the Zn single-phase structure can be 60% or more, and the preferred area fraction of the Zn single-phase structure can be 60% to 90%. In addition, the columnar crystals in the Zn single-phase structure can be uniformly distributed at an average distance of 1 μm to 5 μm. Therefore, the Zn / MgZn2 / Al ternary eutectic structure can be uniformly distributed between the Zn single-phase structures. Therefore, the zinc alloy coating of the present disclosure contains a uniform Zn single-phase structure and a Zn / MgZn2 / Al ternary eutectic structure, so that the zinc alloy coating of the present disclosure can have uniform corrosion resistance.
[0042] Hereinafter, the method for manufacturing a plated steel wire of the present disclosure will be described in more detail.
[0043] According to one aspect of the present disclosure, a method for manufacturing a coated steel wire may include: primarily dipping a base steel wire in a hot-dip galvanizing bath to provide a galvanized steel wire; secondarily dipping the primarily dipped galvanized steel wire in a hot-dip zinc alloy bath to provide a zinc alloy-coated steel wire; and cooling the secondarily dipped zinc alloy-coated steel wire at a cooling rate of 15°C / sec to 50°C / sec.
[0044] The hot-dip galvanizing bath of the present disclosure refers to a plating bath containing Zn as a main component, and may contain impurities unintentionally incorporated during the preparation of an ordinary plating bath. In addition, the hot-dip galvanizing bath of the present disclosure may refer to a plating bath of nearly pure Zn to which a large amount of alloy components (such as Al and Mg) are not artificially added. Therefore, the hot-dip galvanizing bath of the present disclosure may contain 95% or more Zn, preferably 98% or more Zn, and more preferably 99% or more Zn.
[0045] Since the composition content of the hot-dip galvanizing alloy bath of the present disclosure corresponds to the reason for defining the composition content of the zinc alloy coating layer, the description of the reason for defining the composition content of the hot-dip galvanizing alloy bath of the present disclosure is replaced by the description of the reason for defining the composition content of the zinc alloy coating layer. However, since the Fe component of the zinc alloy coating layer is a component introduced from the base steel wire, the description related to the Fe component in the description of the composition content of the zinc alloy coating layer may not be included in the description of the composition content of the hot-dip galvanizing alloy bath of the present disclosure.
[0046] Pretreatment and initial impregnation
[0047] The base steel wire may be subjected to a cleaning process through processes such as pickling, washing, and degreasing, and the cleaned base steel wire may be subjected to a flux treatment. The base steel wire subjected to such a pretreatment process may be primarily dipped in a hot-dip galvanizing bath at 440° C. to 460° C. for 10 to 20 seconds to manufacture a galvanized steel wire. Thus, a zinc plating layer containing Zn as a main component may be formed in the primarily dipped galvanized steel wire.
[0048] Preparation of hot-dip galvanizing bath
[0049] A hot-dip galvanizing alloy bath containing 1.0% to 3.0% Al, 1.0% to 2.0% Mg, and the balance of Zn and inevitable impurities in weight % can be prepared by using a predetermined Zn-Al-Mg-containing composite ingot or a Zn-Mg ingot and a Zn-Al ingot containing individual components. A suitable temperature for melting these ingots may be 440°C to 520°C. Since the melting temperature of the ingot is high, fluidity and uniform composition in the plating bath can be ensured and the amount of floating slag generated can be reduced. Therefore, the ingot can be melted by heating to 440°C or higher. However, when the temperature of the hot-dip galvanizing alloy bath is higher than 520°C, ash-like surface defects are very likely to occur due to the evaporation of Zn. Therefore, it is preferred to also limit the melting temperature of the ingot to 520°C or lower. It is preferred that in the early stage of melting the ingot, melting is started while the temperature of the hot-dip galvanizing alloy bath is maintained at 500 to 520°C, and then melting is completed while the hot-dip galvanizing alloy bath is stabilized at 440 to 480°C.
[0050] Secondary impregnation
[0051] The primary dip galvanized steel wire is cooled to a temperature equal to or lower than the melting point of Zn, and the cooled galvanized steel wire may be dipped in a hot dip galvanizing alloy bath prepared by the above process.
[0052] Generally, when the Al content in the components of the plating bath increases, the melting point increases, and therefore, the equipment inside the plating bath is corroded, resulting in a shortened device life, and the amount of Fe alloy slag in the plating bath increases, resulting in degradation of the surface of the plated material. However, the Al content in the hot-dip zinc-based plating bath of the present disclosure is 1.0 to 2.0%, which is relatively low. Therefore, it is not necessary to set the temperature of the hot-dip galvanizing alloy bath to be higher than necessary. Therefore, the common plating bath temperature can be applied to the temperature of the hot-dip galvanizing alloy bath set for secondary dipping, and a temperature of 440°C to 480°C can be preferably applied. In addition, the time of the secondary dipping can also be appropriately applied in consideration of the thickness of the zinc alloy coating, etc., and the secondary dipping can preferably be performed for 10 to 20 seconds.
[0053] The zinc plating layer formed on the surface of the base steel wire by the primary dipping may be partially or entirely remelted during the secondary dipping, at which time, the Al component contained in the zinc alloy plating solution may diffuse and move toward the interface with the base steel wire.
[0054] cool down
[0055] The secondary dipped galvanized alloy steel wire may be cooled at a cooling rate of 15°C / sec to 50°C / sec, and the galvanized alloy steel wire may preferably be cooled at a cooling rate of 15°C / sec to 50°C / sec immediately after the secondary dip is completed. That is, the cooling may start from the bath surface of the hot-dip galvanized alloy bath. In order to prevent the coarsening of the columnar crystals in the Zn single-phase structure and to prevent the formation of the Zn / MgZn2 binary eutectic structure, the cooling rate of the present disclosure may be 15°C / sec or greater. When the average distance between the columnar crystals in the Zn single-phase structure exceeds 5 μm, the columnar crystals in the Zn single-phase structure are excessively coarsened. Therefore, uniform corrosion resistance may not be ensured. In addition, the Zn / MgZn2 binary eutectic structure formed in the coating causes cracks during the processing of the plated steel wire, which may impair uniform corrosion resistance and processability. On the other hand, when the cooling rate is too large, the columnar crystals in the Zn single-phase structure may be excessively refined, resulting in locally non-uniform corrosion resistance, and the diffusion of the Fe-Zn-Al-based structure is insufficient, resulting in the formation of a crystalline structure caused by the concentration of the Fe-Zn-Al-based structure at the interface layer. Therefore, the bonding force between the zinc alloy coating and the base steel wire is insufficient. Therefore, the processability of the plated steel wire may be deteriorated.
[0056] The cooling of the present disclosure may be performed by supplying an inert gas such as nitrogen, argon, or helium, and relatively inexpensive nitrogen may be preferred in terms of reducing manufacturing costs.
[0057] Embodiments of the invention
[0058] Hereinafter, the present disclosure will be described in more detail with reference to inventive examples.
[0059] (Invention Example)
[0060] A steel wire containing, by weight %, 0.82% of C, 0.2% of Si, 0.5% of Mn, 0.003% of P, and the balance of Fe and inevitable impurities and having a diameter of 5 mm was prepared as a sample, subjected to degreasing and pickling, and subjected to flux treatment using a flux containing zinc chloride (ZnCl2) and ammonium chloride (NH4Cl) as main components. Thereafter, the steel wire treated with the flux was primarily immersed in a hot-dip galvanizing bath containing 0.2 weight % of Al and heated to 460°C for 15 seconds, the average thickness of the hot-dip galvanized layer was adjusted to 20 μm, and the hot-dip galvanized layer was cooled to a temperature equal to or lower than the melting point of Zn. Thereafter, the hot-dip galvanized layer was immersed in a Zn-Mg-Al-based plating bath containing a composition corresponding to the plating composition shown in Table 1 (excluding the Fe component) at 460°C for 15 seconds, and then, the plated steel wire was manufactured by applying different cooling conditions.
[0061] After each manufactured coated steel wire was cut in a direction perpendicular to the longitudinal direction, the cross section was imaged with a field emission scanning electron microscope (FE-SEM), and the area fraction of the Zn single-phase structure in the cross section of the coating, the average distance between columnar crystals in the Zn single-phase structure, and the presence or absence and distribution of each of the Zn / MgZn2 / Al ternary eutectic structure and the Zn / MgZn2 binary eutectic structure were measured based on the imaging results. The area fraction of the Zn single-phase structure refers to the area fraction occupied by the Zn single-phase structure in the area occupied by the Zn single-phase structure and the Zn / MgZn2 / Al ternary eutectic structure in the cross section of the coating.
[0062] Thereafter, each plated steel wire was drawn at a diameter reduction rate of 80% and processed into a 1 mm plated steel wire for processability evaluation, and the surface appearance and corrosion resistance of the processed plated steel wire were evaluated. The surface appearance was evaluated by imaging the surface of the drawn plated steel wire using SEM and determined based on the presence or absence of cracks in the corresponding image. The corrosion resistance was evaluated by subjecting each of the drawn plated steel wires to a salt water spray test. That is, each plated steel wire was loaded into a salt water spray tester, and the red rust occurrence time was measured according to the international standard (ASTM B117-11). Specifically, in the salt water spray tester, the red rust was measured at 2 ml / 80 cm per hour.2 Salt water (temperature: 35°C, pH: 6.8) with a concentration of 5% was sprayed at a spray rate of . When the red rust occurrence time of each plated steel wire was 300 hours or more, it was indicated as "◎", when the red rust occurrence time of each plated steel wire was 200 hours or more and shorter than 300 hours, it was indicated as "○", when the red rust occurrence time of each plated steel wire was 100 hours or more and shorter than 200 hours, it was indicated as "Δ", and when the red rust occurrence time of each plated steel wire was shorter than 100 hours, it was indicated as "×". In general, when the red rust occurrence time is 300 hours or more in the salt water spray test, excellent corrosion resistance can be ensured even in a severe oxidizing environment.
[0063] [Table 1]
[0064]
[0065] In Inventive Examples 1 to 4, the conditions of the present disclosure were satisfied, and therefore, it was confirmed that cracks did not occur after wire drawing, and red rust occurred after 300 hours in the salt water spray evaluation. On the other hand, in Comparative Examples 1 to 4, the conditions of the present disclosure were not satisfied, and therefore, it was confirmed that cracks occurred after wire drawing, and red rust occurred within 200 hours in the salt water spray evaluation.
[0066] Figure 1 is a FE-SEM image obtained by observing the cross section of Inventive Example 1, and Figure 2 This is a FE-SEM image obtained by observing the surface of the plated layer of Inventive Example 1.
[0067] like Figure 1 and Figure 2 As shown, it can be determined that in Inventive Example 1, the area fraction of the Zn single-phase structure is about 85%, and the average distance between the columnar crystals in the Zn single-phase structure is 3 μm, which indicates that the columnar crystals in the Zn single-phase structure are finely formed. In addition, it can be determined that in Inventive Example 1, the Fe-Zn-Al-based crystal structure is formed at a thickness of about 1 / 5 of the thickness of the entire coating from the interface, and the Zn / MgZn2 / Al ternary eutectic structure is uniformly distributed between the Zn single-phase structures.
[0068] Figure 3 is a FE-SEM image obtained by observing the cross section of Comparative Example 1, and Figure 4 This is a FE-SEM image obtained by observing the surface of the plated layer of Comparative Example 1.
[0069] like Figure 3 and Figure 4As shown, it can be determined that in Comparative Example 1, the area fraction of the Zn single-phase structure is about 50%, and the average distance between the columnar crystals in the Zn single-phase structure is 15 μm, which indicates that the columnar crystals in the Zn single-phase structure are coarsely formed. In addition, it can be determined that in Comparative Example 1, the Fe-Zn-Al-based crystal structure is formed at a thin thickness of about 1 / 6 of the thickness of the entire coating layer from the interface, and the structure is unevenly distributed as a whole due to the mixed coarse Zn / MgZn2 binary eutectic structure.
[0070] Figure 5 is a SEM image obtained by observing the surface of Invention Example 1 after wire drawing, and Figure 6 is a SEM image obtained by observing the surface of Comparative Example 1 after wire drawing.
[0071] like Figure 5 As shown in FIG. 1 , it can be confirmed that in Inventive Example 1, no cracks appear on the surface of the plated layer after wire drawing. Figure 6 As shown, it can be confirmed that in Comparative Example 1, cracks occurred on the surface of the plated layer after wire drawing.
[0072] Therefore, according to an exemplary embodiment of the present disclosure, a plated steel wire and a method of manufacturing the same that effectively ensures workability and corrosion resistance may be provided.
[0073] In the above, the present disclosure has been described in detail through exemplary embodiments, but other exemplary embodiments having different forms are possible. Therefore, the technical spirit and scope of the appended claims are not limited to the exemplary embodiments.
Claims
1. A coated steel wire, include: Basic steel wire; and Zinc alloy coating, wherein the zinc alloy coating comprises, by weight%, 1.0% to 3.0% Al, 1.0% to 2.0% Mg, 0.5% to 5.0% Fe, and the balance Zn and unavoidable impurities, The zinc alloy coating comprises Zn / MgZn 2 / Al ternary eutectic structure, Zn single phase structure and Fe-Zn-Al based crystal structure, The Fe—Zn—Al based crystal structure is formed adjacent to the base steel wire and has an average thickness of 1 / 5 to 1 / 2 of the average thickness of the zinc alloy plating layer, and In the cross section of the zinc alloy coating, an average distance between columnar crystals in the Zn single-phase structure is 1 μm to 5 μm.
2. The coated steel wire according to claim 1, wherein in the cross section of the zinc alloy coating, 2 The area fraction occupied by the Zn single-phase structure among the areas occupied by the Zn / Al ternary eutectic structure and the Zn single-phase structure is 60% or more.
3. A method for producing a coated steel wire according to claim 1 or 2, include: Initially dipping the base steel wire into a hot dip galvanizing bath to provide the galvanized steel wire; dipping the primarily dipped galvanized steel wire in a hot dip zinc alloy bath for a second time to provide a zinc alloy coated steel wire; as well as The zinc alloy steel wire after the secondary immersion is cooled at a cooling rate of 15°C / sec to 50°C / sec. The hot-dip galvanizing alloy bath contains, by weight%, 1.0% to 3.0% Al, 1.0% to 2.0% Mg, and the balance Zn and unavoidable impurities.
4. The method according to claim 3, wherein the base steel wire is initially dipped in the hot-dip galvanizing bath at 440°C to 460°C for 10 seconds to 20 seconds.
5. The method according to claim 3, wherein the primary dipped galvanized steel wire is cooled to a temperature equal to or lower than the melting point of Zn, and the cooled galvanized steel wire is secondarily dipped in the hot-dip galvanizing alloy bath.
6. The method according to claim 3, wherein the galvanized steel wire is secondarily dipped in the hot-dip galvanizing alloy bath at 440°C to 460°C for 10 seconds to 20 seconds.
Citation Information
Patent Citations
HOT DIP Zn ALLOY PLATED STEEL WIRE HAVING EXCELLENT ANTI-CORROSION AND METHOD FOR MANUFACTURING THE STEEL WIRE USING THE SAME
KR1020160078670A
Method of constructing highly corrosion-resistant zinc alloy double-coating on surface of steel product
CN107904532A
Zinc alloy plated steel sheet having excellent bending workability and manufacturing method therefor
CN108350555A
Hot dip zn-al-mg plated steel sheet and production method therefor
JP2002285311A
Zn ALLOY PLATED STEEL SHEET HAVING EXCELLENT CORROSION RESISTANCE AND BENDABILITY AND METHOD FOR MANUFACTURING SAME
KR101665883B1