A hydrodesulfurization catalyst and its preparation method and application
By combining polyoxylate with mesoporous ZSM-5 molecular sieve, the carrier is modified with cationic surfactants and loading active metals under hydrothermal conditions to form an Anderson structure, solving the problem of poor synergistic effects between additives and active metals. , which improves the desulfurization activity and metal dispersion of the catalyst, and is suitable for ultra-deep gasoline desulfurization.
Patent Information
- Application Number
- CN202010840132.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-08-19
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2040-08-19
AI Technical Summary
In the existing hydrodesulfurization catalysts, the synergistic effect of the additive metal and the active metal is poor, and the dispersion is poor, making it difficult to achieve efficient catalytic activity and uniform distribution of metal components at the same time.
Using the method of combining polyoxylate with mesoporous ZSM-5 molecular sieve, the surface of the carrier is modified by cationic surfactant and the active metal components are loaded under hydrothermal conditions to form an Anderson structure to promote the edge angle of Co at MoS2 sheet crystals. Position combination improves metal dispersion and synergistic effects.
It significantly improves the desulfurization activity and metal dispersion of the catalyst, realizes the synergistic effect of the additive and the active metal, improves the thiophene removal efficiency of the catalyst, and is suitable for ultra-deep gasoline desulfurization.
Smart Images

Figure CN114073980B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of catalysts and relates to a gasoline hydrodesulfurization catalyst with high metal dispersion, a preparation method thereof and application in gasoline desulfurization. Background Art
[0002] The increasing environmental awareness and increasingly stringent environmental regulations force the oil refining industry to pay more attention to the development of clean fuel production technology. In the future, the automotive fuel in the market will tend to be "ultra-low sulfur", for example, to meet the Euro V emission standards, the sulfur mass fraction is required to be less than 10μg / g, and tend to be "sulfur-free". Fuels that do not meet the emission standards will not be able to enter the market. In addition to the increasingly stringent national standards, the large-scale exploitation of crude oil has also caused the phenomenon of heavy and inferior crude oil to continue to intensify. The sulfur compounds in heavy crude oil are complex and difficult to completely remove, which also hinders the production of ultra-low sulfur clean oil products. Therefore, ultra-deep desulfurization of oil products has received widespread attention. Hydrogenation technology, as a very effective desulfurization method, plays an increasingly important role in the production of clean gasoline and diesel fuels, and the development of new hydrogenation catalysts with high activity and selectivity has become one of the most urgent needs of the oil refining industry. Generally, according to the specific chemical properties of the reaction molecules in the actual oil products and the reaction conditions of the supporting hydrogenation process, the interaction between the metal and the carrier can be adjusted, and the appropriate sulfide metal active phase morphology structure can be designed and constructed to develop an efficient hydrogenation catalyst.
[0003] Hydrodesulfurization catalysts are usually transition metal catalysts, using Co as a promoter and Mo(W) as an active metal. Studies have shown that Co species mainly exist in the following three forms: Co species that combine with the corners of Mo(W)S2 lamellae to form Co-Mo(W)-S active phases, which have high HDS activity; Co species that exist in thermodynamically stable Co9S8 compounds and Co species that enter the Al2O3 lattice to form cobalt aluminates with the support. Studies have shown that Co species in Co9S8 and cobalt aluminates have no promoter effect. Generally, Co-Mo(W)-S active phases include type I and type II Co-Mo(W)-S active phases. The basic structure of type I active phase is a single layer of Mo(W)S2 lamellae, with a low sulfur coordination number, strong interaction with the support, and a large number of Mo(W)-O-Al bonds remaining, making it difficult for Mo(W) to be completely sulfurized. The type II active phase is a highly sulfur-coordinated Co-Mo(W)-S active phase. The active components interact with the support through van der Waals forces, which are weak. The Mo(W) species are fully sulfurized and have high HDS activity.
[0004] Chinese patent CN 108236958A discloses a method for preparing a hydrodesulfurization catalyst, which comprises preparing an impregnation solution containing metal precursors of Co and Mo, adjusting the pH value of the impregnation solution to be lower than the zero electric point of the carrier, impregnating the carrier with the impregnation solution, and then drying and calcining the carrier to obtain a highly dispersed catalyst. Although this method can achieve high dispersion of active components to a certain extent by adjusting the interaction force between the liquid and solid phases to make the metal precursor evenly distributed on the surface of the carrier, Co and Mo need to be introduced separately, and the close contact between the auxiliary metal and the active metal is subject to certain limitations.
[0005] Song Hua et al. (Song Hua, Guo Yuntao, Li Feng, et al. Research progress of hydrorefining catalyst carriers. Petrochemicals, 2010, 39: 941-948) used mesoporous SiO2 as a carrier to improve the dispersion of active metals, such as MCM-41, SBA-15, HMS, and SBA-16. Since pure SiO2 does not have Bronsted acid, it needs to be doped with trivalent ions such as Al 3+ , Ga 3+ , Fe 3+ and B 3+ , where Al 3+ is the most suitable choice because Al 3+ The doping of Mo can produce Lewis and Bronsted acids. However, the dispersion of Mo decreases with the increase of Si content in SiO2-Al2O3 support.
[0006] By using metal chelates as metal precursors, the dispersion of metal components can be significantly improved (MA Lélias, EL Guludec, L Mariey. Effect of EDTA addition on the structure and activity of the active phase of cobalt-molybdenum sulfide hydrotreatment catalysts. Catalysis Today, 2010, 150: 179-185). However, metal chelates have low stability and are easily decomposed during the loading process, resulting in uneven dispersion of metal components and low catalytic activity.
[0007] In summary, the technologies currently reported in patents or literatures are difficult to simultaneously achieve high synergy and good dispersion of the auxiliary metal and active metal in the catalyst. Therefore, this problem has become a technical problem that needs to be solved urgently in this field. Summary of the invention
[0008] The main purpose of the present invention is to provide a hydrodesulfurization catalyst and a preparation method and application thereof. The metal dispersion in the catalyst is good, and the auxiliary agent and the active metal can have a good synergistic effect.
[0009] In order to achieve the above object, the present invention provides a method for preparing a hydrodesulfurization catalyst, comprising the following steps:
[0010] Step 1, dissolving a molybdenum source in water to prepare a solution A, dissolving a cobalt source in water and adding hydrogen peroxide to prepare a solution B, mixing the solution A and the solution B, heating, and filtering to obtain a polyoxometalate;
[0011] Step 2, dispersing polyoxometalates on mesoporous ZSM-5 molecular sieve to obtain CoMo-POM / ZSM-5;
[0012] Step 3, impregnating CoMo-POM / ZSM-5 with a cobalt source solution, and sulfiding to obtain a hydrodesulfurization catalyst.
[0013] The method for preparing the hydrodesulfurization catalyst of the present invention, wherein the step 2 is: dispersing the mesoporous ZSM-5 molecular sieve in water, adding a cationic surfactant, and then adding a solution formed by the polyoxometalate to react to obtain CoMo-POM / ZSM-5.
[0014] The preparation method of the hydrodesulfurization catalyst of the present invention, wherein the cationic surfactant is one or more of dodecyltrimethylammonium bromide, hexadecyltrimethylammonium bromide, hexamethylammonium bromide, didecyldimethylammonium bromide and amino acid salt; the molar ratio of the cationic surfactant to the polyoxometalate is (1-10):1.
[0015] The method for preparing a hydrodesulfurization catalyst of the present invention comprises the following steps: the molybdenum source is ammonium heptamolybdate tetrahydrate, and the cobalt source is cobalt acetate; the step of mixing solution A and solution B comprises the following steps: adding solution B dropwise into solution A; and the heating temperature is higher than 100°C.
[0016] The method for preparing the hydrodesulfurization catalyst of the present invention further comprises the step of heating solution A before mixing solution A and solution B; the heating temperature is 100-200°C.
[0017] In the method for preparing the hydrodesulfurization catalyst of the present invention, the hydrogen peroxide is added in the form of a hydrogen peroxide solution, and the concentration of the hydrogen peroxide solution is 25-35%.
[0018] The method for preparing the hydrodesulfurization catalyst of the present invention, wherein the mesoporous ZSM-5 molecular sieve is obtained by alkali treatment and ammonium exchange of the microporous ZSM-5 molecular sieve; and / or the cobalt source solution in step 3 is a cobalt nitrate solution or a cobalt acetate solution, and a complexing agent is also added to the cobalt source solution.
[0019] The preparation method of the hydrodesulfurization catalyst of the present invention, wherein the alkali used in the alkali treatment is a NaOH solution, and the concentration of the NaOH solution is 0.1-0.5 mol / L; the complexing agent is one or more of citric acid, ethylenediaminetetraacetic acid, and nitrilotriacetic acid, and the molar ratio of the cobalt source in the cobalt source solution, calculated as metallic cobalt, to the complexing agent is 1: (0.5-3.0).
[0020] The method for preparing the hydrodesulfurization catalyst of the present invention comprises the following steps: the reaction is a hydrothermal deposition reaction, the reaction temperature is 100-200° C., the reaction time is 20-30 hours, and the reaction is carried out in a closed container.
[0021] The method for preparing the hydrodesulfurization catalyst described in the present invention, wherein the sulfurization step is:
[0022] The CoMo-POM / ZSM-5 impregnated with the cobalt source solution was loaded into the reactor and heated for 700-900 h. -1 H2 was introduced into the catalyst bed at a rate of 5-10 h. -1 Inject 2-5wt% sulfide oil at a liquid hourly space velocity to make the volume ratio of H2:sulfide oil 200-500;
[0023] Then, the catalyst bed is heated to 350-400° C. and maintained at that temperature for 4-8 hours to complete the sulfidation.
[0024] In order to achieve the above object, the present invention also provides a hydrodesulfurization catalyst obtained by the above-mentioned method for preparing the hydrodesulfurization catalyst.
[0025] In order to achieve the above object, the present invention further provides the use of the above hydrodesulfurization catalyst in gasoline desulfurization.
[0026] Beneficial effects of the present invention:
[0027] (1) The polyoxometalate prepared by the present invention has an Anderson structure, that is, the auxiliary atom Co is wrapped in the main atom Mo, which can promote the binding of Co at the corners of MoS2 platelets, thereby improving the effective utilization rate of active metals; at the same time, this structure is easy to form an active phase during sulfurization.
[0028] (2) This preparation method modifies the negatively charged carrier surface by adding a cationic surfactant and combines hydrothermal conditions to load the active metal components. This not only avoids direct contact between the metal components and the carrier and weakens the interaction between the metal and the carrier, but also improves the dispersion of the metal active components, effectively regulates the stacking degree, and improves the accessibility between metals, thereby promoting the synergistic effect of the main and auxiliary metals and greatly improving the desulfurization activity of the catalyst. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is the FT-IR image of the polyoxometalate crystal CoMoAm prepared in Example 1 of the present invention;
[0030] Figure 2 The XRD spectra of ZSM-5 without alkali modification and alkali modification in Example 1 of the present invention are shown;
[0031] Figure 3 The N2 adsorption-desorption isotherms of microporous and mesoporous ZSM-5 before and after alkali treatment in Example 1;
[0032] Figure 4 The pore size distribution diagram of microporous and mesoporous ZSM-5 before and after alkali treatment in Example 1;
[0033] Figure 5 This is a HRTEM image of CoMoS-PZ prepared in Example 3 of the present invention;
[0034] Figure 6 This is a HRTEM image of CoMoS-PCZ prepared in Example 4 of the present invention;
[0035] Figure 7 This is the HRTEM photo of CoMoS-IM prepared in Comparative Example 2. DETAILED DESCRIPTION
[0036] In order to have a clearer understanding of the technical features, purposes and beneficial effects of the present invention, the technical solution of the present invention is now described in detail below, but it should not be understood as limiting the scope of the present invention. In the embodiments, all raw reagent materials are commercially available unless otherwise specified, and the experimental methods without specific conditions are conventional methods and conventional conditions well known in the art, or according to the conditions recommended by the instrument manufacturer.
[0037] The present invention provides a method for preparing a hydrodesulfurization catalyst, comprising the following steps:
[0038] Step 1, dissolving a molybdenum source in water to prepare a solution A, dissolving a cobalt source in water and adding hydrogen peroxide to prepare a solution B, mixing the solution A and the solution B, heating, and filtering to obtain a polyoxometalate;
[0039] Step 2, dispersing polyoxometalates on mesoporous ZSM-5 molecular sieve to obtain CoMo-POM / ZSM-5 (wherein POM refers to polyoxometalates);
[0040] Step 3, impregnating CoMo-POM / ZSM-5 with a cobalt source solution, and sulfiding to obtain a hydrodesulfurization catalyst.
[0041] The present invention first prepares the main agent metal Mo and the auxiliary agent metal Co into a polyoxometalate, which has an Anderson structure, that is, the auxiliary agent atom Co is wrapped in the main agent atom Mo, which can promote the binding of Co at the corners of MoS2 platelets, thereby improving the effective utilization rate of active metals; at the same time, the structure is easy to form an active phase by sulfurization.
[0042] In one embodiment, the molybdenum source in step 1 is ammonium heptamolybdate tetrahydrate, and the cobalt source is cobalt acetate. The cobalt source is dissolved in water and hydrogen peroxide is added to prepare a B solution. In one embodiment, the hydrogen peroxide is added in the form of a solution, that is, the hydrogen peroxide is first prepared into a hydrogen peroxide solution with a concentration of 25-35wt%, and then added to the cobalt source aqueous solution to form a B solution.
[0043] In one embodiment, the A solution is first heated, for example, to 100-200°C, and then the A solution and the B solution are mixed. In one embodiment, the mixing method is: the B solution is added dropwise to the A solution, and then heated until the solution boils, the boiling time is, for example, 0.5-5h, and then allowed to stand, filtered, and polyoxometalates are obtained. In another embodiment, the mass concentration of the molybdenum source in the A solution is 8%-13%, and the mass concentration of the cobalt source in the B solution is 5%-7%; the molybdenum source in the A solution is calculated as molybdenum, and the cobalt source in the B solution is calculated as cobalt, and the molar ratio of the two is: 8-11:2.
[0044] In one embodiment, the obtained polyoxometalate structure is (NH4)6[Co2Mo 10 O 38 H4]·7H2O.
[0045] In one embodiment, the mesoporous ZSM-5 molecular sieve in step 2 is obtained by alkali treatment and ammonium exchange of the microporous ZSM-5 molecular sieve. The microporous ZSM-5 molecular sieve is, for example, a conventional commercially available microporous ZSM-5 molecular sieve. The alkali used in the alkali treatment is, for example, a NaOH solution, and the concentration of the NaOH solution is, for example, 0.1-0.5 mol / L. The alkali treatment method is, for example, adding the microporous ZSM-5 molecular sieve to an alkali solution in a certain proportion, and carrying out a constant temperature stirring treatment at a certain temperature, but the present invention is not limited thereto. The ammonium exchange method is, for example, adding the ZSM-5 molecular sieve after the alkali treatment to an ammonium salt solution in a certain proportion, and carrying out a constant temperature stirring treatment at a certain temperature, and the ammonium salt is, for example, ammonium chloride, but the present invention is not limited thereto. In this way, after the microporous ZSM-5 molecular sieve is alkali treated and ammonium exchanged, a mesoporous ZSM-5 molecular sieve can be obtained.
[0046] In one embodiment, step 2 is: dispersing the mesoporous ZSM-5 molecular sieve in water, adding a cationic surfactant, and then adding a polyoxometalate solution, reacting, and then cooling, filtering, washing, and drying to obtain CoMo-POM / ZSM-5. The polyoxometalate solution is a solution formed by dissolving the polyoxometalate prepared above in water.
[0047] In another embodiment, the cationic surfactant is one or more of dodecyltrimethylammonium bromide, hexadecyltrimethylammonium bromide, hexamethylammonium bromide, didecyldimethylammonium bromide and amino acid salts; the molar ratio of the cationic surfactant to the polyoxometalate is (1-10):1, and the mass ratio of the mesoporous ZSM-5 molecular sieve to the polyoxometalate is, for example, 1:0.1-0.5.
[0048] In one embodiment, the reaction is a hydrothermal deposition reaction, which is carried out in a closed container, such as an autoclave, and more preferably in a stainless steel reactor lined with polytetrafluoroethylene, at a temperature of 100-200° C. and a reaction time of 20-30 hours. In another embodiment, the hydrothermal deposition reaction is carried out under dynamic conditions, such as placing the reactor in a rotating constant temperature oven, so that the polyoxometalate is deposited on the mesoporous ZSM-5 molecular sieve under dynamic conditions.
[0049] In this step, the mesoporous ZSM-5 molecular sieve is first reacted with the cationic surfactant to form colloid particles of uniform size, which are then loaded with active metal components under hydrothermal deposition conditions. This not only avoids direct contact between the metal components and the carrier and weakens the interaction between the metal and the carrier, but also improves the dispersion of the metal active components, effectively regulates the stacking degree, improves the accessibility between active metals, and greatly improves the desulfurization activity of the catalyst.
[0050] Step 3 is to impregnate CoMo-POM / ZSM-5 with a cobalt source solution, and directly sulfide it without calcination to obtain a hydrodesulfurization catalyst.
[0051] In step 3, the cobalt source solution is, for example, a cobalt nitrate solution or a cobalt acetate solution. The present invention does not specifically limit the concentration of the cobalt source solution, and it can be carried out according to the routine operation of those skilled in the art. In one embodiment, the cobalt source solution also includes an acid solution, and the acid solution is, for example, citric acid. In another embodiment, the molar ratio of the cobalt source in the cobalt source solution to the citric acid is 1: (0.5-3.0) in terms of metallic cobalt.
[0052] After the CoMo-POM / ZSM-5 is impregnated with the cobalt source solution, it can be directly sulfided without calcination. In one embodiment, the sulfidation steps are:
[0053] The CoMo-POM / ZSM-5 impregnated with the cobalt source solution was loaded into the reactor and heated for 700-900 h. -1 H2 was introduced into the catalyst bed at a rate of 5-10 h. -1 Inject 2-5wt% sulfide oil at a liquid hourly space velocity to make the volume ratio of H2:sulfide oil 200-500;
[0054] Then, the catalyst bed is heated to 350-400° C. and maintained at that temperature for 4-8 hours to complete the sulfidation.
[0055] The sulfurized oil is, for example, a mixed solution of CS2 and n-heptane.
[0056] The hydrodesulfurization catalyst obtained by the above method of the present invention has a high metal dispersion, a suitable number of MoS2 stacking layers, and a high thiophene removal activity, is suitable for the hydro-reforming of high-sulfur fuel oil, and can achieve ultra-deep desulfurization of gasoline.
[0057] The technical solution of the present invention will be further described in detail below through specific embodiments.
[0058] Example 1
[0059] This embodiment provides a method for preparing a desulfurization catalyst, which comprises the following steps:
[0060] Step 1: First weigh 11.31 g of ammonium heptamolybdate tetrahydrate ((NH4)6Mo7O 24 ·4H2O) was dissolved in 100mL of deionized water, and the above solution was placed in a 120℃ oil bath and heated with stirring to obtain solution A; 3.34g of cobalt acetate tetrahydrate (Co(OOCCH3)2·4H2O) was weighed and dissolved in 50mL of deionized water, and 8mL of hydrogen peroxide (H2O2) solution (35.0wt.%) was slowly added dropwise, and stirred until Co2+ The ions completely changed color, and solution B was obtained. Then, solution B was added dropwise to solution A and boiled for 1 hour. The color of the solution changed from colorless to brown and finally to dark green. It was allowed to stand at room temperature for 7 days, filtered, washed with ethanol and dried to obtain dark green polyoxometalate crystals CoMoAm (i.e. (NH4)6[Co2Mo 10 O 38 H4]·7H2O).
[0061] Step 2: The conventional alkaline modification treatment method of microporous ZSM-5 zeolite is as follows: 20g molecular sieve is 沸石 :V NaOH =1g:30mL ratio was placed in 600mL of NaOH solution (concentration of 0.3mol / L), and stirred in a constant temperature water bath at 65℃ for 6h; the suspension was cooled, filtered, washed with deionized water until the pH was 7, and then dried at 120℃ for 12h to obtain alkali-modified Na-ZSM-5 zeolite. 25g of alkali-modified Na-ZSM-5 zeolite was added to m 沸石 :V NH4Cl =1g:10mL ratio was placed in 250mL of NH4Cl solution and stirred in a constant temperature water bath at 80°C for 2h; the suspension was cooled, filtered, washed with deionized water to pH 7, dried at 120°C for 12h, and calcined at 520°C for 5h to obtain H-ZSM-5 zeolite.
[0062] Step 3: H-ZSM-5 is tableted, molded, and crushed to 20-40 mesh. 0.84 g of the molded H-ZSM-5 is dispersed in 70 mL of deionized water. 0.16 g of decanyltrimethylammonium bromide is added to the mixed solution and stirred until completely dissolved. Then 0.18 g of polyoxometalate is added to the mixed solution and stirred at 25 ° C for 4 h. Finally, the mixed solution is transferred to a closed reactor, and the reactor is placed in a rotary oven at 120 ° C for 24 h. After the reaction is completed, it is taken out, cooled, and filtered. , washed to pH = 7, and the obtained sample was dried at 120 ° C for 6 hours to obtain CoMo-POM / ZSM-5; then impregnated with a mixed solution of cobalt nitrate (Co(NO3)2·6H2O) and citric acid (the molar ratio of Co(NO3)2·6H2O: citric acid is 1:1) according to Co / (Co+Mo)=0.3 (cobalt includes cobalt in polyoxometalate and cobalt to be impregnated), and the obtained sample was dried at room temperature for 12 hours and dried at 120 ° C for 6 hours to obtain a desulfurization catalyst, recorded as CoMo-PZ.
[0063] Example 2
[0064] This embodiment provides a method for preparing a desulfurization catalyst, which comprises the following steps:
[0065] Step 1: First weigh 11.31 g of ammonium heptamolybdate tetrahydrate ((NH4)6Mo7O 24 ·4H2O) was dissolved in 100mL of deionized water, and the above solution was placed in a 120℃ oil bath and heated with stirring to obtain solution A; 3.34g of cobalt acetate tetrahydrate (Co(OOCCH3)2·4H2O) was weighed and dissolved in 50mL of deionized water, and 8mL of hydrogen peroxide (H2O2) solution (35.0wt.%) was slowly added dropwise, and stirred until Co 2+ The ions completely changed color to obtain solution B. Then, solution B was added dropwise to solution A and boiled for 1 hour. The color of the solution changed from colorless to brown and finally to dark green. The solution was allowed to stand at room temperature for 7 days, filtered, washed with ethanol and dried to obtain dark green polyoxometalate crystals CoMoAm.
[0066] Step 2: The conventional alkaline modification treatment method of microporous ZSM-5 zeolite is as follows: 20g molecular sieve is 沸石 :V NaOH =1g:30mL ratio was placed in 600mL of NaOH solution (concentration of 0.3mol / L), and stirred in a constant temperature water bath at 65℃ for 6h; the suspension was cooled, filtered, washed with deionized water until the pH was 7, and then dried at 120℃ for 12h to obtain alkali-modified Na-ZSM-5 zeolite. 25g of alkali-modified Na-ZSM-5 zeolite was added to m 沸石 :V NH4Cl =1g:10mL ratio was placed in 250mL of NH4Cl solution and stirred in a constant temperature water bath at 80°C for 2h; the suspension was cooled, filtered, washed with deionized water to pH 7, dried at 120°C for 12h, and calcined at 520°C for 5h to obtain H-ZSM-5 zeolite.
[0067] Step three, H-ZSM-5 is tableted, molded, and crushed to 20-40 mesh, 0.84g of the molded H-ZSM-5 is dispersed in 70mL of deionized water, 0.21g of hexadecyltrimethylammonium bromide is added to the above-mentioned mixed solution, stirred until completely dissolved, and then 0.18g of polyoxometalate is added to the above-mentioned mixed solution, and stirred at 25°C for 4h; finally, the above-mentioned mixed solution is transferred to a closed reactor, and the reactor is placed in a 120°C rotary oven for reaction for 24h. After the reaction is completed, it is taken out for cooling, filtering, and washing to pH=7. The obtained sample is dried at 120°C for 6h to obtain CoMo-POM-CTAB / ZSM-5; then, a mixed solution of cobalt acetate and ethylenediaminetetraacetic acid (cobalt acetate: ethylenediaminetetraacetic acid molar ratio is 1:1) is impregnated according to Co / (Co+Mo)=0.3, and the obtained sample is dried at room temperature for 12h and dried at 120°C for 6h to obtain a desulfurization catalyst, recorded as CoMo-PCZ.
[0068] Comparative Example 1
[0069] This comparative example provides a method for preparing a desulfurization catalyst, which is prepared by the following steps:
[0070] 1.69 g of ammonium heptamolybdate tetrahydrate, 1.20 g of cobalt nitrate hexahydrate and 0.79 g of anhydrous citric acid were weighed and dissolved in deionized water. After constant volume, equal volumes were impregnated on 8.31 g of a mesoporous H-ZSM-5 carrier (the carrier was the mesoporous H-ZSM-5 prepared in Example 1), and dried at 120° C. for 6 h to obtain a reference catalyst, recorded as CoMo-IM.
[0071] The prepared polyoxometalates were analyzed by FT-IR. Figure 1 This is the FT-IR graph of the polyoxometalate crystal CoMoAm prepared in Example 1.
[0072] Depend on Figure 1 It can be seen that 1633cm -1 The vibration peak of OH in H2O is 1412cm -1 NH4 + The vibration peaks of NH in 950 and 910 cm -1 The peaks of Mo-O stretching vibration are split because the Co atoms in the crystal are located at different positions of the Mo-O octahedron and produce different vibrations. -1 The absorption peaks at 660 and 528 cm are the stretching vibration absorption peaks of Mo-O-Mo oxygen bridge. -1 The strong peak at is considered to be the Co-O-Mo absorption peak. The FT-IR spectrum confirms that CoMoAm crystals have been successfully prepared.
[0073] XRD was used to analyze the ZSM-5 molecular sieve before and after alkali treatment. Figure 2 These are the XRD peaks of the ZSM-5 molecular sieve before and after alkali treatment in Example 1.
[0074] Depend on Figure 2 It can be seen that the zeolite has obvious ZSM-5 characteristic peaks at 2θ=7.9°, 8.8°, 23.1°, 23.6° and 24.4°, which is a typical MFI structure. After the ZSM-5 zeolite is treated with alkali, the intensity of the characteristic peak decreases, indicating that the degree of destruction of the zeolite framework structure increases with the increase of alkali concentration.
[0075] Table 1 shows the pore structure data of microporous and mesoporous ZSM-5 before and after alkali treatment in Example 1. As can be seen from Table 1, the untreated ZSM-5 zeolite has a higher specific surface area, in which the surface area of micropores is relatively high and the surface area of mesopores is relatively low. After treatment with 0.3 mol / L NaOH solution, the surface area of micropores of zeolite H-ZSM-5 decreases, the surface area of mesopores increases, and the volume of micropores decreases and the volume of mesopores increases.
[0076] Table 1 Pore structure data of ZSM-5 zeolite before and after alkali treatment
[0077]
[0078] Figure 3 The N2 adsorption-desorption isotherms of microporous and mesoporous ZSM-5 before and after alkali treatment in Example 1. As can be seen from the figure, the ZSM-5 zeolite that has not been treated with alkali is a type IV adsorption isotherm, which shows that it is mainly a microporous structure, and the presence of hysteresis loops shows that it also has certain mesopores. After H-ZSM-5 treated with 0.3mol / L alkali solution, obvious H2 hysteresis loops appear in the zeolite within a relatively high relative pressure range, which indicates that after alkali treatment, the zeolite presents a multi-level pore structure and the number of mesopores increases.
[0079] Figure 4 The pore size distribution diagram of microporous and mesoporous ZSM-5 before and after alkali treatment in Example 1. Figure 4 It can be seen that the untreated ZSM-5 zeolite is pure microporous zeolite, and the most probable pore size of H-ZSM-5 is 9.3nm. After being treated with 0.3mol / L alkali solution, the zeolite skeleton structure is destroyed, the pore size increases, and an obvious mesoporous structure appears.
[0080] Table 2 compares the metal component contents in the desulfurization catalyst of Example 1, the desulfurization catalyst of Example 2 and the desulfurization catalyst of Comparative Example 1.
[0081] Table 2 Metal content of catalysts in Examples 1, 2 and Comparative Example 1
[0082] sample Mo (wt.%) Co(wt.%) CoMo-PZ 13.5 3.01 CoMo-PCZ 13.6 3.05 CoMo-IM 13.8 3.08
[0083] Note: The metal content is measured as oxide, that is, the Mo content is measured as the mass fraction of MoO3, and the Co content is measured as the mass fraction of CoO.
[0084] Example 3
[0085] This embodiment provides a method for preparing a sulfurized desulfurization catalyst, which comprises the following steps:
[0086] The CoMo-PZ prepared in Example 1 was diluted with quartz sand in a volume ratio of 1:1 and loaded into a stainless steel reactor with an inner diameter of 8.0 mm and a length of 320 mm. The catalyst was dried at 120° C. for 2 h under H2 conditions, and then a sulfiding agent (3 wt % CS2 in n-heptane solution) was introduced at a sulfiding pressure of 4.0 MPa and a liquid hourly space velocity of 8.0 h -1 , hydrogen-to-oil volume ratio of 300:1, and the temperature was raised to 360°C at a heating rate of 2°C / min and maintained for 6 h to obtain sulfurized CoMo-PZ, denoted as CoMoS-PZ.
[0087] Example 4
[0088] This embodiment provides a method for preparing a sulfurized desulfurization catalyst, which comprises the following steps:
[0089] The CoMo-PCZ prepared in Example 2 was diluted with quartz sand in a volume ratio of 1:1 and loaded into a stainless steel reactor with an inner diameter of 8.0 mm and a length of 320 mm. The catalyst was dried at 110° C. for 2 h under H2 conditions, and then a sulfiding agent (3.5 wt % CS2 in n-heptane) was introduced. The sulfiding pressure was 4.5 MPa and the liquid hourly space velocity of the sulfiding agent was 9.0 h -1 , hydrogen-oil volume ratio of 400:1, and the temperature was raised to 365°C at a heating rate of 2.5°C / min and maintained for 6.5h to obtain sulfurized CoMo-PCZ, denoted as CoMoS-PCZ.
[0090] Comparative Example 2
[0091] This comparative example provides a method for preparing a sulfurized desulfurization catalyst, which comprises the following steps:
[0092] The CoMo-IM prepared in Comparative Example 1 was diluted with quartz sand in a volume ratio of 1:1 and loaded into a stainless steel reactor with an inner diameter of 8.0 mm and a length of 320 mm. The catalyst was dried at 120°C for 2 h under H2 conditions, and then a sulfiding agent (3 wt% CS2 in n-heptane solution) was introduced at a sulfiding pressure of 4.0 MPa and a liquid hourly space velocity of 8.0 h -1 , hydrogen-to-oil volume ratio of 300:1, and the temperature was raised to 360°C at a heating rate of 2°C / min and maintained for 6 h to obtain sulfurized CoMo-IM, denoted as CoMoS-IM.
[0093] The sulfided catalyst was analyzed by HRTEM. Figure 5 , Figure 6 and Figure 7 The HRTEM images of CoMoS-PZ, CoMoS-PCZ and CoMoS-IM are shown respectively. By counting 20 images with a total of 300 to 500 MoS2 flakes, the average length of MoS2 flakes is calculated using formula (1-4): Average number of layers and dispersion f Mo , the sheet crystal information of MoS2 on different catalysts was obtained, and the statistical results are listed in Table 3.
[0094]
[0095]
[0096]
[0097] L = 3.2 (2n i -1) / 10 (4)
[0098] Among them, x i is the number of MoS2 lamellae or MoS2 stackings counted; L i is the length of the i-th MoS2 platelet; N i is the number of stacking layers of the i-th MoS2 stack. Mo is the dispersion of MoS2 flakes, Mo e is the number of Mo atoms at the edge position, Mo c is the number of Mo atoms located at the corner positions, Mo T is the total number of Mo atoms, n i is the number of Mo atoms on the edge of MoS2 flakes, and t is the total number of MoS2 flakes counted.
[0099] Table 3 Statistical results of HRTEM of different catalysts
[0100]
[0101] As can be seen from the figure, the introduction method of the metal precursor will affect the morphology of the MoS2 flakes. The catalysts CoMoS-PZ and CoMoS-PCZ prepared by surfactant-assisted hydrothermal deposition have short MoS2 flakes, high stacking layers, and good dispersion. The catalyst CoMoS-IM prepared by impregnation and roasting has long MoS2 flakes, low stacking layers, uneven dispersion, and poor dispersion. This is because the colloid particles formed by the polyoxometalate ions wrapped by decanyltrimethylammonium bromide or hexadecyltrimethylammonium bromide are of uniform size. Under the hydrothermal environment, the solvent viscosity is reduced, which is conducive to the diffusion and deposition of the organic-inorganic composite colloid particles and improves the dispersion of the active components. The polyoxometalate in which Co and Mo are in close contact is used as the active metal precursor. The Co species inhibits the lateral growth of the Mo species, making the MoS2 lamellae of the catalysts CoMoS-PZ and CoMoS-PCZ shorter. The addition of surfactants to the hydrothermal system can also effectively block the contact between the active components and the carrier, reduce the interaction between the two, and increase the number of MoS2 stacking layers. In the catalyst CoMoS-IM prepared by impregnation and calcination, there is a phenomenon of uneven impregnation of active metals, which makes the active metal dispersion poor and the length of the lamellae longer; high-temperature calcination forms a strong Mo-O-Al bond between Mo and the carrier Al2O3, and the active components themselves are severely agglomerated, resulting in the majority of MoS2 being a single layer; in the impregnation method, cobalt nitrate and ammonium heptamolybdate are used as Co source and Mo source respectively, and there is almost no interaction between Co species and Mo species, which makes it difficult for Co species to play an auxiliary role at the corners of MoS2, and Co cannot inhibit the lateral growth of MoS2 lamellae.
[0102] From the CoMoS active phase model, it can be seen that Co atoms bond with the edges of MoS2 lamellae to form CoMoS active phase. The higher the dispersion of the catalyst MoS2 lamellae, the more conducive it is to the effective utilization of Co atoms, thereby forming the CoMoS active phase more efficiently. In addition, the unsaturated edges and corners of MoS2 lamellae have HDS activity, and the basal position of the grain has no contribution to the reaction activity. Therefore, increasing the dispersion of the active phase loaded on the catalyst surface can effectively improve the HDS activity of the catalyst. From the above characterization, it can be seen that the dispersion of MoS2 lamellae of CoMoS-PZ is significantly higher than that of CoMoS-IM, which is more conducive to the formation of the CoMoS active phase in the former, thereby facilitating the synergistic effect between the main and auxiliary agents.
[0103] Desulfurization application experiments were carried out on CoMoS-PZ, CoMoS-PCZ and CoMoS-IM prepared in Example 3, Example 4 and Comparative Example 2.
[0104] Thiophene (800 μg g -1The reaction conditions were as follows: pressure 2.0 MPa, hydrogen oil volume ratio 300:1, temperature 270°C, volume space velocity 6.0 h -1 , and samples were taken after the reaction was stable for 48h. The desulfurization rates of CoMoS-PZ, CoMoS-PCZ and CoMoS-IM were 93.8%, 93.5% and 81.2%, respectively. The above results show that CoMoS-PZ and CoMoS-PCZ have excellent desulfurization activity.
[0105] Of course, the present invention may have many other embodiments. Without departing from the spirit and essence of the present invention, technicians familiar with the field may make various corresponding changes and deformations based on the present invention, but these corresponding changes and deformations should all fall within the scope of protection of the claims of the present invention.
Claims
1. A method for preparing a hydrodesulfurization catalyst, characterized in that: The following steps are involved: Step 1, dissolving a molybdenum source in water to prepare a solution A, dissolving a cobalt source in water and adding hydrogen peroxide to prepare a solution B, mixing the solution A and the solution B, heating, and filtering to obtain a polyoxometalate; Step 2, dispersing the mesoporous ZSM-5 molecular sieve in water, adding a cationic surfactant, and then adding the solution formed by the polyoxometalate to react to obtain CoMo-POM / ZSM-5; Step 3, impregnating CoMo-POM / ZSM-5 with a cobalt source solution and sulfiding to obtain a hydrodesulfurization catalyst; The molybdenum source in solution A is calculated as molybdenum, and the cobalt source in solution B is calculated as cobalt, and the molar ratio of the two is 8-11:2; The molybdenum source is ammonium heptamolybdate tetrahydrate, and the cobalt source in step 1 is cobalt acetate; The cationic surfactant is one or more of decanyltrimethylammonium bromide, hexadecyltrimethylammonium bromide, hexamethylammonium bromide, and didecyldimethylammonium bromide; the molar ratio of the cationic surfactant to the polyoxometalate is (1-10):
1.
2. The method for preparing a hydrodesulfurization catalyst according to claim 1, characterized in that: The step of mixing solution A and solution B is: adding solution B dropwise into solution A; and the heating temperature is higher than 100°C.
3. The method for preparing a hydrodesulfurization catalyst according to claim 2, characterized in that: Before mixing solution A and solution B, the method further includes heating solution A; the temperature of heating solution A is 100-200°C.
4. The method for preparing a hydrodesulfurization catalyst according to claim 1, characterized in that: The hydrogen peroxide is added in the form of a hydrogen peroxide solution, and the concentration of the hydrogen peroxide solution is 25-35 wt %.
5. The method for preparing a hydrodesulfurization catalyst according to claim 1, characterized in that: The mesoporous ZSM-5 molecular sieve is obtained by alkali treatment and ammonium exchange of the microporous ZSM-5 molecular sieve; and / or the cobalt source solution in step 3 is a cobalt nitrate solution or a cobalt acetate solution, and a complexing agent is also added to the cobalt source solution.
6. The method for preparing a hydrodesulfurization catalyst according to claim 5, characterized in that: The alkali used in the alkali treatment is a NaOH solution, and the concentration of the NaOH solution is 0.1-0.5 mol / L; the complexing agent is one or more of citric acid, ethylenediaminetetraacetic acid, and nitrilotriacetic acid; the molar ratio of the cobalt source in the cobalt source solution, calculated as metallic cobalt, to the complexing agent is 1:(0.5-3.0).
7. The method for preparing a hydrodesulfurization catalyst according to claim 1, characterized in that: The reaction is a hydrothermal deposition reaction, the reaction temperature is 100-200°C, the reaction time is 20-30 h; and the reaction is carried out in a closed container.
8. The method for preparing a hydrodesulfurization catalyst according to claim 6, characterized in that: The steps of the vulcanization are: The CoMo-POM / ZSM-5 impregnated with the cobalt source solution was loaded into the reactor and heated for 700-900 h. -1 H2 was introduced into the catalyst bed at a rate of 5-10 h. -1 2-5 wt% of sulfurized oil is injected at a liquid hourly space velocity to make the volume ratio of H2:sulfurized oil 200-500; Then, the catalyst bed is heated to 350-400° C. and maintained at that temperature for 4-8 hours to complete the sulfidation.
9. The hydrodesulfurization catalyst obtained by the preparation method of the hydrodesulfurization catalyst according to any one of claims 1 to 8.
10. Use of the hydrodesulfurization catalyst according to claim 9 in gasoline desulfurization.
Citation Information
Patent Citations
Preparation method of hydrodesulfurization catalyst
CN108236958A
Deep hydrodesulfurization solid-acid catalyst of gasoline and preparation method thereof
CN101767032A
Method for the hydrocracking of hydrocarbon fractions using a catalyst based on heteropolyanions trapped in a mesostructured oxide support
CN103270140A