Polyimide and method for producing the same

By adjusting the polyimide molecular structure and processing conditions to improve its adhesion and maintain mechanical properties, the problem in the prior art that polyimide resins sacrifice mechanical properties when improving adhesion is solved and high adhesion is achieved. A combination of strength and dimensional stability.

CN114096588BActive Publication Date: 2024-10-29PI ADVANCED MATERIALS CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN201980098437.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-11-28
Publication Date
2024-10-29
Estimated Expiration
2039-11-28

AI Technical Summary

Technical Problem

When existing polyimide resins improve adhesion, they often sacrifice mechanical properties such as elongation and tensile strength, and it is difficult to maintain appropriate glass transition temperature and dimensional stability.

Method used

By adjusting the light transmittance in the polyimide molecular structure and oxidizing part of the chain to form short chains, thereby improving adhesion while maintaining mechanical properties, a combination of specific diamine monomers and dianhydride monomers are used, combining oxygen and Nitrogen imidization treatment adjusts the weight average molecular weight and glass transition temperature of the polymer.

Benefits of technology

Excellent adhesion of polyimide is achieved while maintaining its inherent strength, chemical resistance, weather resistance and heat resistance, ensuring dimensional stability and appropriate glass transition temperature.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003469216030000091
    Figure BDA0003469216030000091
  • Figure BDA0003469216030000101
    Figure BDA0003469216030000101
Patent Text Reader

Abstract

The present invention relates to a polyimide and a method for producing the same, thereby providing a polyimide and a method for producing the same that can achieve excellent adhesion while maintaining inherent properties of the polyimide.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Cross-references and related applications

[0002] The present invention claims priority based on Korean Patent Application No. 10-2019-0055736, dated May 13, 2019, the disclosure of which is incorporated herein by reference in its entirety. Technical Field

[0003] The present invention relates to polyimide and a method for producing the same. Background Art

[0004] Polyimide (PI) is a thermally stable polymer material based on a rigid aromatic backbone. It has excellent mechanical properties such as strength, chemical resistance, weather resistance, and heat resistance due to the chemical stability of the imide ring.

[0005] In addition, polyimide has insulating properties and excellent electrical properties such as a low dielectric constant, and therefore has attracted much attention as a highly functional polymer material for use in a wide range of industrial fields such as electronics, communications, and optics.

[0006] However, in general, polyimide resins are hardly considered to have high adhesion among polymer resins, and various studies have been conducted to further improve the adhesion.

[0007] For example, in order to improve the adhesion of polyimide resins, approaches to limiting the monomer content have been attempted in some cases, but adhesion is slightly improved, while mechanical properties such as elongation and tensile strength may be reduced, and dimensional stability may be sacrificed.

[0008] Therefore, there is a need for a novel polyimide resin that can ensure appropriate levels of glass transition temperature and dimensional stability while having better adhesion than conventional polyimide resins. Summary of the invention

[0009] Technical issues

[0010] An object of the present invention is to provide a polyimide capable of achieving excellent adhesion by solving the above-mentioned conventional problems while maintaining the inherent characteristics of the polyimide, and a method for producing the same.

[0011] Technical Solution

[0012] The present invention relates to polyimide. The polyimide of the present invention is suitable for use in fields requiring adhesion of varnishes (such as displays, enamels, semiconductors, and adhesives) or requiring dimensional stability.

[0013] An exemplary polyimide comprises a polymer of a diamine monomer and a dianhydride monomer, and its average transmittance in the wavelength region of 380nm to 780nm is in the range of 49% to 61%, and the transmittance of the wavelength of 550nm is in the range of 40% to 64%. In this specification, the transmittance can be measured using a UV-visible spectrophotometer. In an example, the lower limit of the average transmittance in the wavelength region of 380nm to 780nm can be 49.5%, 50%, 51%, 53%, 54%, 55%, 56% or 56.5%, and the upper limit thereof can be 60.8%, 60.5%, 60.3%, 60%, 58%, 55%, 53% or 50%. In addition, in one embodiment, the lower limit of the transmittance at a wavelength of 550nm may be 45%, 50%, 53%, 54.1%, 54.5%, 55%, 56% or 58%, and the upper limit thereof may be 63.8%, 63.5%, 63.3%, 63%, 61%, 58%, 56%, 55%, 54% or 52%. In the present invention, by adjusting the transmittance of the polyimide as described above, an adhesion promoter may be formed in the polyimide molecular structure, and accordingly, the adhesion of the polyimide with conventional low adhesion may be implemented at a desired level. The method for adjusting the transmittance is not particularly limited.

[0014] In one example, the polyimide of the present invention can be derived from polyamic acid in which diamine monomers and dianhydride monomers are polymerized. In one embodiment, the material derived from polyamic acid means that the polyamic acid is imidized to form the polyimide of the present invention.

[0015] Polyamic acid is a polyimide precursor composition that can form long polymer chains during imidization. However, short chains may be produced in the process. Since the short chains act as impurities in the composition, the adhesion is reduced. The present invention can increase the adhesion by oxidizing the short chains. In the present invention, since the transmittance of the polyimide film is reduced, some chains may be oxidized. Therefore, by adjusting the transmittance of the wavelength region of 380nm to 780nm and the wavelength region of 550nm to the above range, the present invention can oxidize some chains in the polyimide molecular structure, thereby improving the adhesion.

[0016] In an embodiment of the present invention, the polymer of the present invention includes a first chain and a second chain shorter than the first chain, wherein the second chain may be in an oxidized state. If the first chain is the above-mentioned polymer long chain, the second chain may be a short chain. In this specification, long chain and short chain are relative, and absolute values ​​are not limited. On the contrary, by the above-mentioned 380nm to 780nm wavelength region and the transmittance range of 550nm wavelength, it can be known whether the second chain is oxidized. In an example, the second chain may be included in the range of 5wt% or less in the total polymer. The upper limit of the content of the second chain may be 4.8wt%, 4.5wt%, 4.3wt%, 4.0wt%, 3.8wt%, 3.5wt%, 3.3wt%, 3.0wt%, 2.8wt%, 2.5wt%, 2.3wt%, 2.0wt%, 1.5wt%, 1.0wt% or 0.8wt%. In addition, the lower limit of the second chain content may be 0 wt%, 0.3 wt%, 0.5 wt%, 0.7 wt%, 1.0 wt% or 1.3 wt%. The present invention can provide a polyimide having excellent adhesion while maintaining mechanical properties such as inherent polyimide strength, chemical resistance, weather resistance and heat resistance through the oxidized second chain.

[0017] The dianhydride monomer that can be used to prepare the polyamic acid solution can be an aromatic tetracarboxylic dianhydride, wherein the aromatic tetracarboxylic dianhydride can be exemplified by pyromellitic dianhydride (or PMDA), 3,3',4,4'-biphenyl tetracarboxylic dianhydride (or BPDA), 2,3,3'4'-biphenyl tetracarboxylic dianhydride (or a-BPDA), oxidized diphthalic dianhydride (or ODPA), diphenyl sulfone-3,4,3',4'-tetracarboxylic dianhydride (or DSDA), bis(3,4-dicarboxyphenyl) sulfide dianhydride, 2,2-bis(3,4-dicarboxyphenyl)-1,1,1,3,3,3-hexafluoropropane dianhydride, 2,3,3',4'-benzophenone tetracarboxylic dianhydride, 3,3',4,4'-diphenyltetracarboxylic dianhydride (or BTDA), bis(3,4-dicarboxyphenyl) dianhydride 1,4-bis(3,4-dicarboxyphenoxy)phthalic acid anhydride, 1,4-bis(3,4-dicarboxyphenoxy)phthalic acid anhydride, 2,2-bis(3,4-dicarboxyphenoxy)propane dianhydride, p-phenylene dianhydride (trimellitic acid monoester anhydride), p-biphenyl dianhydride (trimellitic acid anhydride), m-terphenyl-3,4,3',4'-tetracarboxylic acid dianhydride, p-terphenyl-3,4,3',4'-tetracarboxylic acid dianhydride, 1,3-bis(3,4-dicarboxyphenoxy)phthalic acid anhydride, 1,4-bis(3,4-dicarboxyphenoxy)phthalic acid anhydride, 1,4-bis(3,4-dicarboxyphenoxy)biphenyl dianhydride, 2,2-bis[(3,4-dicarboxyphenoxy)phenyl]propane dianhydride (BPADA), 2,3,6,7-naphthalenetetracarboxylic acid anhydride, 1,4,5,8-naphthalenetetracarboxylic acid anhydride, 4,4'-(2,2-hexafluoroisopropyl)dibenzoic acid anhydride, and the like.

[0018] The above-mentioned dianhydride monomers can be used alone or in combination with two or more monomers as needed, but considering the above-mentioned bond dissociation energy, the present invention includes, for example, pyromellitic dianhydride (PMDA), 3,3',4,4'-biphenyltetracarboxylic dianhydride (s-BPDA) or 2,3,3',4'-biphenyltetracarboxylic dianhydride (a-BPDA).

[0019] In addition, the diamine monomer that can be used to prepare the polyamic acid solution is an aromatic diamine, which can be classified and exemplified as follows.

[0020] 1) Diamines with a relatively rigid structure, such as diamines with a benzene nucleus in the structure, such as 1,4-diaminobenzene (or p-phenylenediamine, PDA), 1,3-diaminobenzene, 2,4-diaminotoluene, 2,6-diaminotoluene, 3,5-diaminobenzoic acid (or DABA), etc.;

[0021] 2) Diamines with two benzene nuclei in the structure, such as diaminodiphenyl ether such as 4,4'-diaminodiphenyl ether (or oxidized diphenylamine, ODA), 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenylmethane (methylenediamine), 3,3'-dimethyl-4,4'-diaminodiphenyl, 2,2'-dimethyl-4,4'-diaminodiphenyl, 2,2'-bis(trifluoromethyl)-4,4'-diaminodiphenyl, 3,3'-dimethyl-4,4'-diaminodiphenyl Benzene, 3,3'-dicarboxy-4,4'-diaminodiphenylmethane, 3,3',5,5'-tetramethyl-4,4'-diaminodiphenylmethane, bis(4-aminophenyl) sulfide, 4,4'-diaminobenzamide, 3,3'-dichlorobenzidine, 3,3'-dimethylbenzidine (or o-toluidine), 2,2'-dimethylbenzidine (or m-toluidine), 3,3'-dimethoxybenzidine, 2,2'-dimethoxybenzidine, 3,3'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl sulfide, 3,4'-diaminodiphenyl sulfide, 4,4'-diaminodiphenyl sulfide, 3,3'-diaminodiphenyl sulfone, 3,4'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl sulfone, 4'-diaminodiphenyl sulfone, 3,3'-diaminophenyl sulfone, 4'-diaminodiphenyl sulfone, 3,3'-diaminophenyl sulfone, 4'-diaminophenyl sulfone, 3,3'-diaminophenyl sulfone, 4'-diaminophenyl sulfone, 3,3'-diamino-4,4'-dichlorobenzophenone, 3,3'-diamino-4,4 '-Dimethoxybenzophenone, 3,3'-diaminodiphenylmethane, 3,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylmethane, 2,2-bis(3-aminophenyl)propane, 2,2-bis(3-aminophenyl)-1,1,3,3,3-hexafluoropropane, 2-bis(4-aminophenyl)-1,1,1,3,3,3-hexafluoropropane, 3,3'-diaminodiphenyl sulfoxide, 3,4'-diaminodiphenyl sulfoxide, 4,4'-diaminodiphenyl sulfoxide, etc.;

[0022] 3) Diamines with three benzene nuclei in the structure, such as 1,3-bis(3-aminophenyl)benzene, 1,3-bis(4-aminophenyl)benzene, 1,4-bis(3-aminophenyl)benzene, 1,4-bis(4-aminophenyl)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(3-aminophenoxy)benzene (or TPE-Q), 1,4-bis(4-aminophenoxy)benzene (or TPE-Q), 1,3-bis(3-aminophenoxy)-4-trifluoromethylbenzene, 3,3'-diamino-4-(4-phenyl)phenoxybenzophenone , 3,3'-diamino-4,4'-bis(4-phenoxy)benzophenone, 1,3-bis(3-aminophenylene sulfide)benzene, 1,3-bis(4-aminophenylene sulfide)benzene, 1,4-bis(4-aminophenylene sulfide)benzene, 1,3-bis(3-aminophenyl sulfone), 1,3-bis(4-aminophenyl sulfone), 1,4-bis(4-aminophenyl sulfone)benzene, 1,3-bis[2-(4-aminophenyl)isopropyl]benzene, 1,4-bis[2-(3-aminophenyl)isopropyl]benzene, 1,4-bis[2-(4-aminophenyl)isopropyl]benzene, etc.;

[0023] 4) Diamines having four benzene nuclei in their structure, such as 3,3'-bis(3-aminophenoxy)biphenyl, 3,3'-bis(4-aminophenoxy)biphenyl, 4,4'-bis(3-aminophenoxy)biphenyl, 4,4'-bis(4-aminophenoxy)biphenyl, bis[3-(3-aminophenoxy)phenyl]ether, bis[3-(4-aminophenoxy)phenyl]ether, bis[4-(3-aminophenoxy)phenyl]ether, bis[4-(4-aminophenoxy)phenyl]ether, bis[3-(3-aminophenoxy)phenyl]ether -aminophenoxy)phenyl] ketone, bis[3-(4-aminophenoxy)phenyl] ketone, bis[4-(3-aminophenoxy)phenyl] ketone, bis[4-(4-aminophenoxy)phenyl] ketone, bis[3-(3-aminophenoxy)phenyl] sulfide, bis[3-(4-aminophenoxy)phenyl] sulfide, bis[4-(4-aminophenoxy)phenyl] sulfide, bis[3-(3-aminophenoxy)phenyl] sulfone, bis[3-(4-aminophenoxy)phenyl] sulfone, bis[4-(4-aminophenoxy)phenyl] sulfide, bis[3-(3-aminophenoxy)phenyl]sulfone, bis[4-(4-aminophenoxy)phenyl]sulfone, bis[3-(3-aminophenoxy)phenyl]methane, bis[3-(4-aminophenoxy)phenyl]methane, bis[4-(4-aminophenoxy)phenyl]methane, 2,2-bis[3-(3-aminophenoxy)phenyl]propane, 2-bis[3-(4-aminophenoxy)phenyl]propane, 2,2-bis[4-(3-aminophenoxy)phenyl]propane, 2,2-bis[4-(4-aminophenoxy)phenyl]propane Hexafluoropropane (BAPP), 2,2-bis[3-(3-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, 2,2-bis[3-(4-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, 2,2-bis[4-(3-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, 2,2-bis[4-aminophenoxy]phenyl-1,1,1,3,3,3-hexafluoropropane, and the like.

[0024] As required, the diamine monomer may be used alone or in combination of two or more monomers, and may include, for example, 3,5-diaminobenzoic acid, 3,3-dihydroxy-4,4-diaminobiphenyl, 2,5-dihydroxy-p-phenylenediamine, 4,6-diaminoresorcinol, 1,4-diaminobenzene (PPD), 1,3-diaminobenzene (MPD), 2,4-diaminotoluene, 2,6-diaminotoluene or 4,4'-methylenediamine (MDA).

[0025] In an embodiment of the present invention, the diamine monomer may include at least one or more hydroxyl groups in the molecular structure. As described above, the present invention can adjust the substituents in the molecular structure of the polyimide, and in one example, since the diamine monomer includes one or more hydroxyl groups, it can achieve excellent adhesion while maintaining the existing physical properties of the polyimide. In addition, the dianhydride monomer may include at least one or more hydroxyl groups in the molecular structure.

[0026] In one embodiment, the thermal decomposition temperature of the polyimide may be 560° C. or higher, or 562° C. or higher. The upper limit is not particularly limited, but may be 1000° C. or lower, or 800° C. or lower. In the polyimide of the present invention, unreacted monomers may be minimized by adjusting the thermal decomposition temperature, thereby providing a polyimide having desired physical properties.

[0027] In one embodiment, the polyimide of the present invention may have a weight average molecular weight in the range of 500 to 100000, 1000 to 80000, 10000 to 70000, 20000 to 60000, 25000 to 55000 or 30000 to 50000. In the present invention, the term weight average molecular weight refers to a value converted to standard polystyrene measured by GPC (gel permeation chromatograph). By adjusting the weight average molecular weight of the polyimide of the present invention, a polyimide having desired physical properties can be provided.

[0028] In addition, in one embodiment, the glass transition temperature of the polyimide may be 360°C or higher, 370°C or higher, 375°C or higher, 380°C or higher, or 400°C or higher. The upper limit is not particularly limited, but may be 600°C or 550°C. In addition, the coefficient of thermal expansion (CTE) of the polyimide may be 15ppm / °C or lower, 13ppm / °C or lower, 10ppm / °C or lower, or 5ppm / °C or lower. The lower limit is not particularly limited, but may be 0ppm / °C or 2ppm / °C. For example, when the temperature is increased or decreased from 100°C to 350°C, the CTE can be measured by adjusting the physical properties of the polyimide, and the present invention can achieve excellent adhesion while maintaining mechanical properties such as the existing excellent strength, chemical resistance, weather resistance, and heat resistance of the polyimide.

[0029] In one embodiment, the polyimide of the present invention can be a polyimide imidized under nitrogen and oxygen atmosphere. In one embodiment, the polyimide can be a polyimide imidized under oxygen and nitrogen atmosphere by polyamic acid. By imidizing polyamic acid under oxygen and nitrogen atmosphere as described above, the present invention can induce an oxidation reaction due to oxygen and improve the adhesion of the entire polyimide by having a relatively low molecular weight chain.

[0030] In the present invention, the polyimide precursor composition is used in the same meaning as the polyamic acid. The organic solvent is not particularly limited as long as it is an organic solvent that can dissolve the polyamic acid, but as an example, the organic solvent may be an aprotic polar solvent.

[0031] The above-mentioned non-protonic polar solvents may include amide-based solvents such as N,N'-dimethylformamide (DMF), N,N'-diethylformamide (DEF), N,N'-dimethylacetamide (DMAc) and dimethylpropaneamide (DMPA), and phenolic solvents such as p-chlorophenol, o-chlorophenol, N-methylpyrrolidone (NMP), γ-butyrolactone (GBL) and dimers, which can be used alone or in combination of two or more.

[0032] In the present invention, the solubility of the polyamic acid may also be adjusted in some cases by using an auxiliary solvent such as toluene, tetrahydrofuran, acetone, methyl ethyl ketone, methanol, ethanol and water.

[0033] In one example, the organic solvent may be, for example, N-methylpyrrolidone (NMP).

[0034] Meanwhile, the polyimide precursor composition of the present invention may contain fillers for improving various properties of the film, such as sliding properties, thermal conductivity, electrical conductivity, corona resistance, and loop stiffness. The fillers to be added are not particularly limited, but may include, for example, silicon dioxide, titanium oxide, aluminum oxide, silicon nitride, boron nitride, calcium hydrogen phosphate, calcium phosphate, mica, and the like.

[0035] The particle size of the filler is not particularly limited and can be determined according to the characteristics of the film to be modified and the type of filler to be added. The average particle size may be 0.05 to 20 μm, 0.1 to 10 μm, 0.1 to 5 μm, or 0.1 to 3 μm. In this specification, unless otherwise specified, the average particle size may be the average particle size measured according to D50 particle size analysis.

[0036] By adjusting the particle size range, the present invention may not reduce mechanical properties without damaging surface properties while fully maintaining the modification effect.

[0037] In addition, in the present invention, the amount of filler added is not particularly limited, and it can be determined by the film properties to be modified or the particle size of the filler, etc. In the present invention, the amount of filler added can be 0.01 to 10 parts by weight, 0.01 to 5 parts by weight, or 0.02 to 1 part by weight relative to 100 parts by weight of the polyimide resin. By adjusting the content, the present invention can maintain the modification effect of the filler while not damaging the mechanical properties of the film.

[0038] The method of adding the filler is not particularly limited, and a method known in the art may be used.

[0039] In a specific embodiment, the solid content of the polyimide precursor composition is 5 to 30 wt %, 8 to 25 wt % or 10 to 20 wt % of the total weight.

[0040] By adjusting the solid content of the polyimide precursor composition, the present invention can prevent an increase in manufacturing cost and processing time required to remove a large amount of solvent during the curing process while controlling the increase in viscosity.

[0041] The viscosity of the polyimide precursor composition may be 10000 cP or less, or 9000 cP or less, measured by a Brookfield viscometer in an RV-7 spindle at a temperature of 23° C. and a rotation speed of 0.5 rpm. The lower limit of the viscosity is not particularly limited, but may be 500 cP or more, or 1000 cP or more.

[0042] Meanwhile, the preparation of the polyamic acid solution uses, for example, a method of placing all diamine monomers in a solvent, and then adding a dianhydride monomer thereto so that it is substantially equimolar or in excess of the diamine monomer to be polymerized, or a method of placing all dianhydride monomers in a solvent, and then adding a diamine monomer thereto so that it is equimolar or in excess of the dianhydride monomer to be polymerized, and so on.

[0043] In one embodiment of the present invention, the polyimide may have an adhesion of 0.08 N / cm or more, and the adhesion is measured according to ASTM D 3359. For example, the adhesion may be 0.12 N / cm or more, 0.15 N / cm or more, 0.18 N / cm or more, 0.22 N / cm or more, 0.25 N / cm or more, 0.3 N / cm or more, 0.33 N / cm or more, 0.38 N / cm or more, or 0.45 N / cm or more, and the upper limit thereof is not particularly limited, but may be 5 N / cm, 4 N / cm, 3 N / cm, 2 N / cm, 1 N / cm, 0.8 N / cm, or 0.6 N / cm. The adhesion may be the adhesion measured when the prepared polyimide film is attached to a glass substrate with a width of 10 mm and peeled off at a peeling rate of 20 mm / min and a peeling angle of 180°.

[0044] The present invention also relates to a method for producing polyimide, which can be the method for producing the polyimide described above.

[0045] The manufacturing method may include a step of imidizing the polyimide precursor composition under a nitrogen and oxygen atmosphere. In the imidization step of the present invention, not only nitrogen can be introduced, but also a certain amount of oxygen can be introduced simultaneously. The present invention improves the adhesion of the entire polyimide by inducing oxidation reaction due to oxygen and having a relatively low molecular weight chain.

[0046] In the above steps of the present invention, the volume ratios of nitrogen and oxygen are 95:5 and 5:95, respectively. For example, in the volume ratio, the nitrogen volume ratio can be 94 to 8, 93 to 20, 92 to 40, 91 to 60, or 90 to 82. In addition, the oxygen volume ratio can be adjusted in the range of, for example, 6 to 80, 7 to 60, 8 to 40, or 9 to 18. By adjusting the volume ratio of nitrogen and oxygen, the present invention can oxidize short chains with low molecular weight in polyimide and adjust the adhesion promoter in polyimide, thereby achieving excellent adhesion. In addition, the present invention can also keep the existing physical properties of polyimide within the above volume ratio range.

[0047] In one embodiment, the processing temperature of the manufacturing method may be 50 to 500° C., 100 to 480° C., or 130 to 470° C. In addition, the polyimide precursor composition may be applied on a carrier or substrate to prepare a polyimide in a thin film form, wherein the polyimide may have a film form with a thickness of 5 to 50 μm or 10 to 20 μm.

[0048] In one embodiment, the present invention may provide a method for manufacturing a polyimide film, comprising the steps of: forming a film of a polyimide precursor composition on a support, and drying the film to prepare a gel film; and curing the gel film.

[0049] Specifically, as for the method of producing a polyimide film by imidizing the above-mentioned polyimide precursor composition, a conventionally known method can be used.

[0050] Specific examples of such imidization may be exemplified by a thermal imidization method, a chemical imidization method, or a composite imidization method using the thermal imidization method and the chemical imidization method in combination.

[0051] Beneficial Effects

[0052] The present invention provides a polyimide and a method for manufacturing the same, wherein the polyimide can achieve excellent adhesion while maintaining inherent properties of the polyimide. DETAILED DESCRIPTION

[0053] Hereinafter, the present invention will be described in more detail through examples according to the present invention and comparative examples, but the scope of the present invention is not limited to the following examples.

[0054] Example 1

[0055] N-methylpyrrolidone (NMP) was introduced into a 500ml reactor equipped with a stirrer and a nitrogen injection and discharge pipe, and nitrogen was injected therein, and after setting the reactor temperature to 30°C, 1,4-diaminobenzene (PPD) as a diamine monomer, and biphenyltetracarboxylic dianhydride (BPDA) and pyromellitic dianhydride (PMDA) as dianhydride monomers were introduced to confirm that they were completely dissolved. The temperature was raised to 40°C under a nitrogen atmosphere, and stirring was continued for 120 minutes while heating, and then a polyamic acid solution with a viscosity of 7000 cP at 23°C was prepared.

[0056] Subsequently, the temperature was raised to 80° C. under a nitrogen atmosphere, and stirring was continued for 2 hours while heating, and then the temperature was cooled to 23° C. to prepare a polyimide precursor composition having a viscosity of 5100 cP.

[0057] The polyimide precursor composition is applied to a WIZUS glass (Asahi Glass) carrier in the form of a thin film, and then heat-treated in the oxygen and nitrogen atmospheres shown in Table 1 below while increasing the temperature from about 110°C to 460°C, and then peeled off from the carrier to prepare a polyimide in the form of a thin film having an average thickness of approximately 15 to 17 μm.

[0058] Examples 2 to 5 and Comparative Examples 1 to 2

[0059] Except that the processing conditions were changed to those shown in Table 1, the rest was prepared according to the same polyimide method as in Example 1.

[0060] [Table 1]

[0061]

[0062] Experimental Example 1-CTE

[0063] Using TA's thermomechanical analyzer Q400 model, the polyimide film was cut into 2 mm width and 10 mm length, and then the temperature was increased from room temperature to 500°C at a rate of 10°C / min while applying a tension of 0.05N in a nitrogen atmosphere, and when cooled again at a rate of 10°C / min, the cross-sectional gradient from 100°C to 350°C was measured. CTE was first measured in the increasing temperature section from 100°C to 350°C, and then in the decreasing temperature section from 350°C to 100°C.

[0064] Experimental Example 2-Glass Transition Temperature

[0065] As for the glass transition temperature, the loss elastic modulus and storage elastic modulus of each polyimide resin were obtained using TMA, and the inflection point in the tangent graph thereof was measured as the glass transition temperature.

[0066] Experimental Example 3-Adhesion

[0067] Adhesion was measured using the method specified in ASTM D 3359. Specifically, the polyimide films prepared in the examples and comparative examples were attached to a glass substrate to form a 10 mm wide film, and the adhesion was measured when peeled at a peeling rate of 20 mm / min and a peeling angle of 180°. The unit of adhesion is N / cm.

[0068] Experimental Example 4-Light Transmittance

[0069] For the polyimide film prepared above, the transmittance was measured in the wavelength range of 380 nm to 780 nm using a UV-Vis spectrometer, and the average value was calculated. The transmittance at 550 nm was also measured.

[0070] [Table 2]

[0071]

Claims

1. A polyimide comprising a polymer obtained by polymerization of a diamine monomer and a dianhydride monomer, wherein: The average transmittance in the wavelength region of 380nm to 780nm is in the range of 49% to 61%, and the transmittance at a wavelength of 550nm is in the range of 40% to 64%, wherein the polymer comprises a first chain and a second chain shorter than the first chain, and the second chain is in an oxidized state, and The polyimide is polyimide imidized in a nitrogen and oxygen atmosphere, and the volume ratios of nitrogen and oxygen are 82 to 90 and 10 to 18, respectively.

2. The polyimide according to claim 1, wherein The oxidized second chains account for 5 wt% or less of the total polymer.

3. The polyimide according to claim 1, wherein The diamine monomer includes 3,5-diaminobenzoic acid, 3,3-dihydroxy-4,4-diaminobiphenyl, 2,5-dihydroxy-p-phenylenediamine, 4,6-diaminoresorcinol, 1,4-diaminobenzene (PPD), 1,3-diaminobenzene (MPD), 2,4-diaminotoluene, 2,6-diaminotoluene or 4,4'-methylenediamine (MDA).

4. The polyimide according to claim 1, wherein The dianhydride monomer includes pyromellitic dianhydride (PMDA), 3,3',4,4'-biphenyltetracarboxylic dianhydride (s-BPDA) or 2,3,3',4'-biphenyltetracarboxylic dianhydride (a-BPDA).

5. The polyimide according to claim 1, wherein The diamine monomer contains at least one or more hydroxyl groups in its molecular structure.

6. The polyimide according to claim 1, wherein The polyimide has a thermal decomposition temperature of 560° C. or higher.

7. The polyimide according to claim 1, wherein The polyimide has a glass transition temperature of 360° C. or higher.

8. The polyimide according to claim 1, wherein The coefficient of thermal expansion (CTE) of the polyimide is 15 ppm / ° C. or less.

9. The polyimide according to claim 1, wherein The polyimide was attached to a glass substrate with a width of 10 mm, and the adhesive force measured when it was peeled off at a peeling rate of 20 mm / min and a peeling angle of 180° based on ASTM D 3359 was 0.08 N / cm or more.

10. A method for producing a polyimide, comprising imidizing a polyimide precursor composition under a nitrogen and oxygen atmosphere, in, The polyimide precursor composition comprises polyamic acid obtained by polymerizing diamine monomers and dianhydride monomers. wherein the volume ratios of nitrogen to oxygen are 82 to 90 and 10 to 18 respectively, and The average light transmittance of the polyimide in the wavelength region of 380 nm to 780 nm is in the range of 49% to 61%, and the light transmittance of the polyimide in the wavelength region of 550 nm is in the range of 40% to 64%.

11. The method for producing polyimide according to claim 10, wherein the processing temperature is in the range of 50 to 500°C.

12. The method for producing a polyimide according to claim 10, wherein: The polyimide was produced in the form of a film having a thickness of 5 to 50 μm.

13. The method for producing a polyimide according to claim 10, wherein: The solid content of the polyimide precursor composition is in the range of 5 to 30 wt %.

14. The method for producing polyimide according to claim 10, wherein: The viscosity of the polyimide precursor composition measured by a Brookfield viscometer in an RV-7 spindle under the conditions of a temperature of 23° C. and a rotation speed of 0.5 rpm is 10,000 cP or less.

Citation Information

Patent Citations

  • Maskpack

    KR1020190055736A

  • Method for synthesizing aromatic imide

    CN104558603A

  • Method for producing polyimide laminate and method for producing flexible circuit board

    CN109311297A

  • Polyimide film with an improved light transmittance and preparation method thereof

    KR1020160077694A