A solvent-free UV light-curable biodegradable biomimetic adhesive
By combining gallic acid analogs with polymers and resins, UV photocuring bionic adhesives are formed, which solves the problem of insufficient bonding performance of the adhesive in water and on inert substrates, and achieves efficient underwater bonding and Biodegradability.
Patent Information
- Application Number
- CN202111337918.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-12
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2041-11-12
AI Technical Summary
The adhesive performance of existing adhesives in water and on inert substrates is insufficient, making it difficult to meet certain application needs.
Using gallic acid analogs to combine with polymers containing multiple carbon-carbon double bonds and tackifying composite resins to form a solvent-free UV photocuring bionic adhesive, using catechol groups to improve underwater adhesion and carbon Carbon double bond groups achieve UV photocuring and enhance cohesion.
It realizes excellent bonding properties of the adhesive under water and effective bonding to inert substrates, has extremely fast curing speed and good mechanical properties, and has biodegradation and green environmental protection characteristics.
Smart Images

Figure CN114181066B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of adhesives, and in particular to a gallic acid analogue and a preparation method and application thereof. Background Art
[0002] Adhesive is a substance with excellent bonding properties. Through the coordination between its own surface adhesion and cohesion, it can bond two objects of different properties together. Due to its own characteristics, adhesives have very wide applications in the market, including aerospace, intelligent manufacturing, daily necessities, electronic product packaging and other fields.
[0003] However, in water or for some inert substrates, the bonding performance of adhesives is not very high, and it is necessary to improve the bonding strength of adhesives in water and on inert substrates. In nature, many intertidal marine organisms such as mussels, sandcastle worms, barnacles and polychaetes show very excellent bonding ability, which is unmatched by human synthetic adhesives. Therefore, since mussels were reported as smart coatings in 2007, mussel-like adhesives have been the focus of research scholars in various countries. This is because mussels can attach themselves to the surfaces of organic and inorganic materials, such as wet rocks and corroded ship bottoms. Therefore, the preparation of mussel-like adhesives is one of the effective ways to solve the problem that ordinary adhesives have low underwater bonding and weak bonding to inert substrates. Summary of the invention
[0004] Based on the technical problems existing in the background technology, the present invention proposes a gallic acid analogue and a preparation method and application thereof. The gallic acid analogue of the present invention can be used in an adhesive, and cooperates with a polymer containing multiple carbon-carbon double bonds and a tackifying composite resin, so that the adhesive has excellent underwater adhesion and can effectively bond to inert substrates, and at the same time has good cohesion. The adhesive is solvent-free, biodegradable, and green and environmentally friendly.
[0005] The present invention provides a gallic acid analogue, the structural formula of which is shown in formula (I):
[0006]
[0007] The present invention also proposes a method for preparing the above-mentioned gallic acid analogue, comprising the following steps: taking gallic acid and an allyl reagent, reacting them in an inert gas atmosphere in the presence of a catalyst, an antioxidant and an alkaline substance to obtain the gallic acid analogue.
[0008] Preferably, the catalyst is at least one of potassium iodide and sodium iodide.
[0009] Preferably, the antioxidant is at least one of sodium sulfite, sodium bisulfite, sodium pyrosulfite and sodium thiosulfate.
[0010] Preferably, the allyl reagent is at least one of allyl chloride and allyl bromide.
[0011] Preferably, the alkaline substance is at least one of potassium carbonate, sodium carbonate and sodium hydroxide.
[0012] Preferably, the reaction temperature is 65-89° C. and the reaction time is 18-24 h.
[0013] Preferably, the molar ratio of gallic acid to catalyst is 1:0.6-1.1.
[0014] Preferably, the molar ratio of gallic acid to antioxidant is 1:2-3.5.
[0015] Preferably, the molar ratio of gallic acid to alkaline substance is 1:12-15.
[0016] Preferably, the reaction solvent is at least one of acetone, ethyl acetate, toluene, N,N-dimethylformamide and methanol.
[0017] Preferably, after the reaction, the gallic acid analog is purified.
[0018] Preferably, the specific steps of purification are: after the reaction is completed, concentrating to obtain a concentrate, then dissolving with water, adjusting the pH to 3-4, extracting with an organic solution, taking the organic phase, and concentrating to obtain the gallic acid analogue.
[0019] Preferably, the organic solvent used for extraction is ethyl acetate.
[0020] The present invention also proposes the application of the gallic acid analogue in adhesives.
[0021] The present invention also provides a solvent-free UV light-curable biodegradable biomimetic adhesive, the raw materials of which include: the above-mentioned gallic acid analogue, a polymer containing multiple carbon-carbon double bonds, a tackifying composite resin and a photoinitiator.
[0022] Preferably, in the adhesive, the weight percentages of gallic acid analogues, polymers containing multiple carbon-carbon double bonds, and tackifying composite resins are 25-50%, 45-70%, and 3-8%, respectively, and the total weight percentage of gallic acid analogues, polymers containing multiple carbon-carbon double bonds, and tackifying composite resins is 100%.
[0023] Preferably, the polymer containing multiple carbon-carbon double bonds is a lactide polymer or / and a caprolactone polymer, wherein the structural formula of the lactide polymer is shown in formula (II), and the structural formula of the caprolactone polymer is shown in formula (III):
[0024]
[0025]
[0026] Wherein, R is H or an alkyl group having 1 to 3 carbon atoms, and a, b, c, d, e, m, and n are all integers greater than 0.
[0027] Preferably, the average molecular weight of the polymer containing multiple carbon-carbon double bonds is 500-6000.
[0028] Preferably, the weight of the photoinitiator accounts for 3-6% of the total weight of the gallic acid analogue and the polymer containing multiple carbon-carbon double bonds.
[0029] Preferably, the tackifying composite resin comprises at least one of n-octylphenol-formaldehyde resin, p-tert-octylphenol-formaldehyde resin and alkylphenol-acetylene resin.
[0030] Preferably, the photoinitiator comprises at least one of 4-acryloxybenzophenone, 4-dimethylamino-ethyl benzoate, phenyl-(1-acryloxy)-cyclohexyl ketone, 2-hydroxy-2-methyl-1-phenyl-1-propanone and 1-hydroxy-cyclohexyl phenyl ketone.
[0031] Beneficial effects:
[0032] 1. The catechol group plays a key role in the excellent bonding performance of mussels. The present invention selects gallic acid and an allyl reagent to react under suitable conditions to obtain a gallic acid analogue having a carbon-carbon double bond group and a catechol group; the inventor applies the gallic acid analogue to an adhesive to obtain a biomimetic adhesive, wherein the catechol group enables the adhesive to have excellent underwater bonding and can effectively bond to an inert substrate, wherein the carbon-carbon double bond group can achieve ultraviolet light (i.e., UV light) curing.
[0033] 2. The present invention uses gallic acid analogs, polymers containing multiple carbon-carbon double bonds, tackifying composite resins, and photoinitiators to cooperate with each other to obtain a solvent-free UV light-curable biodegradable biomimetic adhesive, and the adhesive has an extremely fast curing speed; lactide polymers and / or caprolactone polymers with specific structures are selected to form a cross-linked network through UV light cross-linking and curing, which can greatly improve the cohesive force of the adhesive, and the lactide polymers and caprolactone polymers can be degraded to avoid environmental pollution.
[0034] 3. Since the surface adhesion and cohesion of the adhesive are contradictory, the inventors selected polymers with suitable molecular weight and specific structure containing multiple carbon-carbon double bonds, and matched them with gallic acid analogs and tackifying composite resins in appropriate proportions, so that the surface adhesion and cohesion of the adhesive of the present invention are balanced, and have good mechanical properties while having excellent bonding properties. In addition, the adhesive of the present invention does not use solvents, which is green and environmentally friendly. The adhesive of the present invention can be applied to the fields of environmental engineering, biomedical devices, and daily necessities manufacturing. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 This is the infrared spectrum of the gallic acid analogue obtained in Example 1.
[0036] Figure 2 The infrared spectra of polymer A and lactide polymer prepared in Example 4 are shown.
[0037] Figure 3 The NMR spectra of polymer C and caprolactone polymer prepared in Example 5, wherein a is polymer C and b is caprolactone polymer. DETAILED DESCRIPTION
[0038] The gallic acid analogue of the present invention has a structural formula as shown in formula (I):
[0039]
[0040] The preparation method of the gallic acid analogue comprises the following steps: taking gallic acid and an allyl reagent, reacting them in the presence of a catalyst, an antioxidant and an alkaline substance in an inert gas atmosphere to obtain the gallic acid analogue.
[0041] The inventors have optimized the preparation method of gallic acid analogs. In order to obtain products with higher yield and higher purity, the catalyst is preferably at least one of potassium iodide and sodium iodide; more preferably potassium iodide. The antioxidant is preferably at least one of sodium sulfite, sodium bisulfite, sodium pyrosulfite, and sodium thiosulfate, more preferably sodium sulfite. The allyl reagent is preferably at least one of allyl chloride and allyl bromide, more preferably allyl chloride. The alkaline substance is preferably at least one of potassium carbonate, sodium carbonate and sodium hydroxide, more preferably potassium carbonate.
[0042] The inventors have also screened and optimized the reaction parameters, etc. The reaction temperature is preferably 65-89°C, and the reaction time is preferably 18-24h. The molar ratio of gallic acid to catalyst is preferably 1:0.6-1.1. The molar ratio of gallic acid to antioxidant is preferably 1:2-3.5. The molar ratio of gallic acid to alkaline substance is preferably 1:12-15. The reaction solvent is preferably at least one of acetone, ethyl acetate, toluene, N,N-dimethylamide, and methanol. The amount of the reaction solvent is not limited and can be selected according to actual needs. The molar ratio of gallic acid to the reaction solvent is preferably 1:4.
[0043] The amounts of gallic acid and the allyl reagent are not specified as long as the gallic acid analogue can be obtained. The molar ratio of gallic acid to the allyl reagent is preferably 1:1-1.5; more preferably 1:1.
[0044] After the reaction is completed, purification treatment is required; the specific steps of purification are: after the reaction is completed, concentrate to obtain a concentrate, then dissolve it with water, adjust the pH to 3-4, extract it with an organic solution, take the organic phase, and concentrate it to obtain a gallic acid analog. The organic solvent for extraction is preferably ethyl acetate. The pH can be adjusted with a 1 mol / L HCl aqueous solution.
[0045] There is no limitation on the number of extractions and the amount of the organic solvent used for extraction, which can be selected according to actual needs; the number of extractions is preferably 2 times; and the molar ratio of gallic acid to the organic solvent used for extraction is preferably 1:20-35.
[0046] The gallic acid analogue prepared by the invention has a carbon-carbon double bond group and a catechol group; it can be applied to an adhesive to obtain a bionic adhesive, wherein the catechol group enables the adhesive to have excellent underwater adhesion and can effectively achieve adhesion to an inert substrate, and wherein the carbon-carbon double bond group can achieve UV light curing.
[0047] In order to obtain an adhesive with good surface adhesion and cohesion, the inventors proposed a solvent-free UV light-curable biodegradable biomimetic adhesive, the raw materials of which include: the above-mentioned gallic acid analogue, a polymer containing multiple carbon-carbon double bonds, a tackifying composite resin and a photoinitiator.
[0048] Preferably, in the adhesive, the weight percentages of gallic acid analogues, polymers containing multiple carbon-carbon double bonds, and tackifying composite resins are 25-50%, 45-70%, and 3-8%, respectively, and the total weight percentage of gallic acid analogues, polymers containing multiple carbon-carbon double bonds, and tackifying composite resins is 100%.
[0049] The inventors selected gallic acid analogs, polymers containing multiple carbon-carbon double bonds, tackifying composite resins, and photoinitiators to cooperate with each other. Multiple carbon-carbon double bonds and carbon-carbon double bonds in gallic acid analogs can be UV-cured and have an extremely fast curing speed.
[0050] The inventors selected lactide polymers and / or caprolactone polymers with specific structures, which were cross-linked and cured by UV light to form a cross-linked network, which can greatly improve the cohesive force of the adhesive. In addition, lactide polymers and caprolactone polymers can be degraded to avoid environmental pollution.
[0051] The polymer containing multiple carbon-carbon double bonds is preferably a lactide polymer or / and a caprolactone polymer, wherein the structural formula of the lactide polymer is shown in formula (II), and the structural formula of the caprolactone polymer is shown in formula (III):
[0052]
[0053]
[0054] Wherein, R is H or an alkyl group having 1 to 3 carbon atoms, and a, b, c, d, e, m, and n are all integers greater than 0.
[0055] The lactide polymer can be prepared according to conventional methods in the art, or according to the following method, which specifically comprises the following steps: in an inert gas atmosphere, glycerol, lactide and a catalyst are subjected to a ring-opening reaction to obtain polymer A; in an inert gas atmosphere, polymer A and substance B are subjected to an esterification reaction to obtain a lactide polymer; wherein the structural formula of substance B is: R is H or an alkyl group having 1 to 3 carbon atoms.
[0056] In the preparation process of the above lactide polymer:
[0057] The catalyst is preferably stannous octoate. The temperature of the ring-opening reaction is preferably 125°C, and the time of the ring-opening reaction is preferably 18 hours; the molar ratio of glycerol to lactide is preferably 1:3-5.5; the amount of the catalyst is 0.005 times the total weight of glycerol and lactide; after the ring-opening reaction, the polymer A is purified; the specific steps of purification are: after the ring-opening reaction is completed, dichloromethane is added and mixed, then extracted with ether, and the ether phase (i.e., the upper liquid) is dried to obtain polymer A; the amount of dichloromethane and ether is not specified, and the amount is determined according to actual conditions; preferably, the amount of dichloromethane is 3 times the total weight of glycerol and lactide, and the amount of ether is 25 times the total weight of glycerol and lactide; the temperature of the esterification reaction is preferably 100°C, and the time of the esterification reaction is preferably 7 hours; the inert gas can be nitrogen, etc.
[0058] The caprolactone polymer can be prepared according to conventional methods in the art, or according to the following method, which specifically comprises the following steps: in an inert gas atmosphere, pentaerythritol, caprolactone and a catalyst are subjected to a ring-opening reaction to obtain a polymer C; in an inert gas atmosphere, polymer C and substance B are subjected to an esterification reaction to obtain a lactide polymer; wherein the structural formula of substance B is: R is H or an alkyl group having 1 to 3 carbon atoms.
[0059] In the preparation process of the above-mentioned caprolactone polymer:
[0060] The catalyst is preferably stannous octoate; the temperature of the ring-opening reaction is preferably 140-160° C., and the time of the ring-opening reaction is preferably 24-36 hours; the molar ratio of pentaerythritol to caprolactone is preferably 1:4-8; the amount of the catalyst is 0.004 times the total weight of pentaerythritol and caprolactone; after the ring-opening reaction, the polymer C is purified; the specific steps of purification are: after the ring-opening reaction is completed, dichloromethane is added and mixed, then extracted with ether, and the ether phase (i.e., the upper liquid) is taken and dried to obtain the polymer C; the amounts of dichloromethane and ether are not specified and are determined according to actual conditions; preferably, the amount of dichloromethane is 2-4 times the total weight of pentaerythritol and caprolactone, and the amount of ether is 20-30 times the total weight of pentaerythritol and caprolactone; the temperature of the esterification reaction is preferably 110° C., and the time of the esterification reaction is preferably 5 hours; the inert gas can be nitrogen, etc.
[0061] Since the surface adhesion and cohesion of the adhesive are contradictory, the inventors selected a polymer containing multiple carbon-carbon double bonds with a suitable molecular weight and a specific structure, and matched them with gallic acid analogs and tackifying composite resins in a suitable proportion, so that the surface adhesion and cohesion of the adhesive of the present invention are balanced, and the adhesive has excellent bonding properties and good mechanical properties.
[0062] The average molecular weight of the polymer containing multiple carbon-carbon double bonds is preferably 500-6000.
[0063] Preferably, the weight of the photoinitiator is 3-6% based on the total weight of the gallic acid analog and the polymer containing multiple carbon-carbon double bonds.
[0064] The inventors selected appropriate types of tackifying composite resins and photoinitiators to further improve the bonding performance, cohesive force and curing speed of the adhesive.
[0065] The tackifying composite resin preferably includes at least one of n-octylphenol-formaldehyde resin, p-tert-octylphenol-formaldehyde resin, and alkylphenol-acetylene resin.
[0066] The photoinitiator preferably includes at least one of 4-acryloxybenzophenone, 4-dimethylamino-ethyl benzoate, phenyl-(1-acryloxy)-cyclohexyl ketone, 2-hydroxy-2-methyl-1-phenyl-1-propanone, and 1-hydroxy-cyclohexyl phenyl ketone.
[0067] The preparation method of the solvent-free UV light-curable biodegradable bionic adhesive of the present invention comprises the following steps: uniformly mixing a gallic acid analogue, a polymer containing a plurality of carbon-carbon double bonds, and a tackifying composite resin to obtain the adhesive.
[0068] When using, add the photoinitiator and mix well, then apply it evenly on the surface of the substrate, and then irradiate with ultraviolet light. Preferably, the ultraviolet light with a wavelength of 365-390nm is used for light curing for 5-15 minutes, and the ultraviolet light radiation dose is preferably 350mW / cm 2 .
[0069] The adhesive of the present invention does not use any solvent and is biodegradable, green and environmentally friendly. The adhesive can be applied to the fields of environmental engineering, biomedical devices, daily necessities manufacturing, etc.
[0070] The technical solution of the present invention is described in detail below through specific embodiments.
[0071] Example 1
[0072] A method for preparing a gallic acid analogue comprises the following steps:
[0073] Weigh 17g (0.1mol) of gallic acid, 7.65g (0.1mol) of allyl chloride, and 23.23g (0.4mol) of acetone in turn and add them into a three-necked flask equipped with a condenser, stir and mix evenly, then weigh 165.6g (1.2mol) of potassium carbonate, 9.96g (0.06mol) of catalyst potassium iodide and 28.4g (0.23mol) of antioxidant sodium sulfite and pour them into the three-necked flask, introduce nitrogen to exclude air, stir evenly, then control the temperature to 65°C and stir to react for 18h, after the reaction is completed, distill the mixed solution under reduced pressure to remove acetone and unreacted allyl chloride to obtain a concentrate, dissolve the concentrate with deionized water, and then adjust the pH to 3-4 with a 1mol / l HCl aqueous solution, add ethyl acetate to extract twice (the total amount of ethyl acetate is 176g, i.e., 2mol), and take the ethyl acetate phase and distill it under reduced pressure to obtain a gallic acid analogue.
[0074] The gallic acid analogue obtained in Example 1 was tested, and the results were as follows: Figure 1 As shown, Figure 1 This is the infrared spectrum of the gallic acid analogue obtained in Example 1.
[0075] Depend on Figure 1It can be seen that the present invention successfully prepared a gallic acid analogue, the structure of which retains the catechol group and effectively imitates the "universal bonding" property of the mussel organism.
[0076] Example 2
[0077] A method for preparing a gallic acid analogue comprises the following steps:
[0078] Weigh 17g (0.1mol) of gallic acid, 18.15g (0.15mol) of allyl bromide, and 29.2g (0.4mol) of N,N-dimethylamide in sequence and add them into a three-necked flask equipped with a condenser, stir and mix evenly, then weigh 159g (1.5mol) of sodium carbonate, 16.5g (0.11mol) of catalyst sodium iodide and 36.42g (0.35mol) of antioxidant sodium bisulfite and pour them into the three-necked flask, introduce nitrogen to exclude air, stir evenly, then control the temperature to 89°C and stir to react for 18h. After the reaction is completed, the mixed solution is distilled under reduced pressure to remove N,N-dimethylamide and unreacted allyl bromide to obtain a concentrate, the concentrate is dissolved with deionized water, and then the pH is adjusted to 3-4 with a 1mol / l HCl aqueous solution, ethyl acetate is added for extraction twice (the total amount of ethyl acetate is 308g, i.e., 3.5mol), and the ethyl acetate phase is distilled under reduced pressure to obtain a gallic acid analogue.
[0079] Example 3
[0080] A method for preparing a gallic acid analogue comprises the following steps:
[0081] Weigh 17g (0.1mol) of gallic acid, 7.65g (0.1mol) of allyl chloride, and 12.8g (0.4mol) of methanol in turn and add them into a three-necked flask equipped with a condenser, stir and mix evenly, then weigh 52g (1.3mol) of sodium hydroxide, 9.96g (0.06mol) of catalyst potassium iodide and 38.02g (0.2mol) of antioxidant sodium metabisulfite and pour them into the three-necked flask, introduce nitrogen to exclude air, stir evenly, then control the temperature to 65°C and stir to react for 24h. After the reaction is completed, the mixed solution is distilled under reduced pressure to remove methanol and unreacted allyl chloride to obtain a concentrate, the concentrate is dissolved with deionized water, and then the pH is adjusted to 3-4 with a 1mol / l HCl aqueous solution, ethyl acetate is added for extraction twice (the total amount of ethyl acetate is 264g, i.e., 3mol), and the ethyl acetate phase is distilled under reduced pressure to obtain a gallic acid analogue.
[0082] Example 4
[0083] A method for preparing a lactide polymer comprises the following steps:
[0084] 9.209 g (0.1 mol) of glycerol, 43.2 g (0.3 mol) of lactide and 0.262 g of stannous octoate were weighed and added to a three-necked flask in sequence, and nitrogen was passed through for 30 min after being mixed evenly. The mixture was then stirred and reacted at 125° C. for 18 h. After the reaction was completed, 157.2 g of dichloromethane was added and mixed and stirred. Finally, the mixture was extracted with ether three times (the total amount of ether was 1310 g). The mixture was allowed to stand and separated into an upper and lower layer. The ether phase (i.e., the upper layer) was collected and dried in a vacuum oven to remove the solvent to obtain polymer A.
[0085] 10 g of polymer A and 10.05 g (0.065 mol) of methacrylic anhydride were mixed evenly and poured into a single-necked flask, and nitrogen was passed through for 30 minutes. Then, stirring was maintained at 100° C. for 7 hours, and then dried in a vacuum oven to obtain a lactide polymer with a relative molecular mass of 709.
[0086] The lactide polymer obtained in Example 4 was tested and the results were as follows: Figure 2 As shown, Figure 2 The infrared spectra of polymer A and lactide polymer prepared in Example 4 are shown.
[0087] Example 5
[0088] A method for preparing a caprolactone polymer comprises the following steps:
[0089] 11.10 g (0.08 mol) of pentaerythritol, 37.2 g (0.32 mol) of caprolactone and 0.19 g of stannous octoate were weighed and added into a three-necked flask in sequence, and nitrogen was passed through for 20 min after being mixed evenly. Then, the mixture was stirred and reacted at 140° C. for 24 h. After the reaction was completed, 78.22 mL of dichloromethane was added and mixed and stirred. Finally, the mixture was extracted with ether for three times (the total amount of ether was 1352.9 mL). The mixture was allowed to stand and separated into an upper and lower layer. The ether phase (i.e., the upper layer) was collected and dried in a vacuum oven to remove the solvent to obtain polymer C.
[0090] 10g of polymer C and 15.76g (0.12mol) of acrylic anhydride were mixed evenly and poured into a single-necked flask, and nitrogen was passed through for 20min. Then, stirring was maintained at 110°C for 5h, and then dried in a vacuum oven to obtain a caprolactone polymer with a relative molecular mass of 1260.
[0091] The caprolactone polymer obtained in Example 5 was tested and the results were as follows: Figure 3 As shown, Figure 3 The NMR spectra of polymer C and caprolactone polymer prepared in Example 5, wherein a is polymer C and b is caprolactone polymer.
[0092] Example 6-Example 15, Comparative Examples 1-3
[0093] The gallic acid analogue prepared in Example 1, the lactide polymer prepared in Example 4, and the caprolactone polymer prepared in Example 5 were used to prepare solvent-free UV light-curable biodegradable biomimetic adhesives, respectively. The formulas of each group are shown in Table 1.
[0094] Table 1 Formula table of Examples 6-15 and Comparative Examples 1-3
[0095]
[0096]
[0097] Note: The UV radiation dose in Table 1 is 350mW / cm 2 .
[0098] The preparation methods of the formulations in Table 1 are the same, which are: weigh each component by weight, and stir and mix the components except the photoinitiator.
[0099] Each group of adhesives in Table 1 was tested for performance. The specific testing method is as follows:
[0100] ① Adhesion performance test method: add the photoinitiators of each group in Table 1 to each mixture and mix them evenly, then evenly apply them between two transparent glass plates, and cure them according to the UV light curing conditions in Table 1. The overlapping area of the two glass sheets is 2cm×2.5cm, and then use a universal testing machine to test the shear resistance at a test rate of 150mm / min, and finally record the bonding strength.
[0101] ②Underwater bonding performance test method: Same as ①, the difference is that underwater bonding is to apply glue underwater and UV cure.
[0102] ③ Biodegradability test: The adhesives in each group in Table 1 were UV-cured into circular samples (4 cm in diameter and 0.1 cm in thickness). The samples were then placed in a 0.01 mol / l phosphate buffer solution with a pH of 7.3 and oscillated at a constant speed for 30 days. The degradation rate was used to evaluate the biodegradability. The degradation rate = ((W0-W1) / W0) × 100%, where W0 is the initial sample mass and W1 is the mass after immersion for 30 days.
[0103] Monomer conversion rate: Tracking the C=C (1636cm -1 ) changes in the intensity of the absorption peak in FT-IR, with C=O (1722 cm -1 ) as the internal standard. The monomer conversion rate can be calculated as shown in the following formula.
[0104]
[0105] In the formula,
[0106] ——After UV curing, C=C at 1636cm -1 The peak area of
[0107] ——After UV curing, C=O is at 1722cm -1 The peak area of
[0108] ——Before UV curing, C=C is 1636cm -1 The peak area of
[0109] ——Before UV curing, C=O is at 1722cm -1 The peak area of .
[0110] The test results are shown in Table 2.
[0111] Table 2 Test results
[0112]
[0113]
[0114] It can be seen from Table 2 that the adhesive obtained by combining gallic acid analogs, lactide polymers, caprolactone polymers, and tackifying composite resins in appropriate proportions has extremely fast curing speed, biodegradability, excellent underwater adhesion, and can effectively bond to inert substrates, meeting the requirements of related fields.
[0115] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A solvent-free UV light-curable biodegradable biomimetic adhesive, characterized in that: Its raw materials include: gallic acid analogs, polymers containing multiple carbon-carbon double bonds, tackifying composite resins and photoinitiators; In the adhesive, the weight percentages of the gallic acid analog, the polymer containing multiple carbon-carbon double bonds, and the tackifying composite resin are 25-50%, 45-70%, and 3-8%, respectively, and the total weight percentage of the gallic acid analog, the polymer containing multiple carbon-carbon double bonds, and the tackifying composite resin is 100%; The preparation method of the gallic acid analogue comprises the following steps: taking gallic acid and an allyl reagent, reacting in the presence of a catalyst, an antioxidant and an alkaline substance in an inert gas atmosphere to obtain the gallic acid analogue; The reaction temperature was 65°C and the reaction time was 18h; The molar ratio of gallic acid to the catalyst is 1:0.6, the molar ratio of gallic acid to the antioxidant is 1:2.3, the molar ratio of gallic acid to the alkaline substance is 1:12, and the molar ratio of gallic acid to the allyl reagent is 1:1; The catalyst is potassium iodide, the antioxidant is sodium sulfite, the allyl reagent is allyl chloride, the alkaline substance is potassium carbonate, and the reaction solvent is acetone; The polymer containing multiple carbon-carbon double bonds is a lactide polymer or / and a caprolactone polymer, wherein the structural formula of the lactide polymer is shown in formula (II), and the structural formula of the caprolactone polymer is shown in formula (III): Formula (II), Formula (III); Wherein, R is H or an alkyl group having 1 to 3 carbon atoms, and a, b, c, d, e, m, and n are all integers greater than 0; The tackifying composite resin comprises at least one of n-octylphenol-formaldehyde resin, p-tert-octylphenol-formaldehyde resin and alkylphenol-acetylene resin.
2. The solvent-free UV light-curable biodegradable biomimetic adhesive according to claim 1, characterized in that: The average molecular weight of the polymer containing multiple carbon-carbon double bonds is 500-6000.
3. The solvent-free UV light-curable biodegradable biomimetic adhesive according to claim 1 or 2, characterized in that: The weight of the photoinitiator accounts for 3-6% of the total weight of the gallic acid analogue and the polymer containing multiple carbon-carbon double bonds.
4. The solvent-free UV light-curable biodegradable biomimetic adhesive according to claim 1 or 2, characterized in that the photoinitiator include: At least one of 4-acryloyloxybenzophenone, 4-dimethylamino-ethyl benzoate, phenyl-(1-acryloyloxy)-cyclohexyl ketone, 2-hydroxy-2-methyl-1-phenyl-1-propanone, and 1-hydroxy-cyclohexyl phenyl ketone.
5. The solvent-free UV light-curable biodegradable biomimetic adhesive according to claim 1 or 2, characterized in that: After the reaction is carried out, the gallic acid analog is purified.
6. The solvent-free UV light-curable biodegradable biomimetic adhesive according to claim 5, characterized in that: The specific steps of purification are: after the reaction is completed, concentrate to obtain a concentrate, then dissolve it with water, adjust the pH to 3-4, extract it with an organic solution, take the organic phase, and concentrate it to obtain the gallic acid analogue.
7. The solvent-free UV light-curable biodegradable biomimetic adhesive according to claim 6, characterized in that: The organic solvent used for extraction is ethyl acetate.