Positive electrode material for self-supporting film type lithium secondary battery, preparation method thereof and lithium secondary battery containing the same
The carbon-containing sulfur melt independent film cathode material was prepared by dry method, which solved the problems of low positive electrode loading and complex process in lithium-sulfur secondary batteries, and achieved the effect of high loading and simplified process.
Patent Information
- Application Number
- CN202180004710.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-05-18
- Filing Date
- 2021-05-24
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2041-05-24
AI Technical Summary
In the existing lithium-sulfur secondary batteries, since the slurry process of the sulfur-carbon composite requires conductive materials and adhesives, the positive electrode load volume is reduced, the energy density is reduced, and the process time and cost are increased.
A carbon-containing sulfur melt independent film cathode material is prepared by dry method. By mixing sulfur with porous carbon material, heat treatment and pressurizing, a carbon-containing sulfur melt is formed to achieve a high load positive electrode material.
The self-reliable film-type positive electrode material prepared by the dry method can increase load capacity, simplify processes, reduce costs and time, avoid battery performance deterioration caused by adhesives, and improve formability and durability.
Smart Images

Figure CN114207875B_ABST
Abstract
Description
Technical Field
[0001] This application claims the benefit of priority to Korean Patent Application No. 2020-0063882, filed on May 27, 2020, and Korean Patent Application No. 2021-0064083, filed on May 18, 2021, which are hereby incorporated by reference in their entirety.
[0002] One aspect of the present disclosure relates to a positive electrode material for a self-standing film type lithium secondary battery, a preparation method thereof, and a lithium secondary battery including the same. Background Art
[0003] Recently, with the rapid development of the fields of electronic devices and electric vehicles, the demand for secondary batteries is increasing. In particular, with the trend of miniaturization and weight reduction of portable electronic devices, the demand for secondary batteries with high energy density that can cope with these is growing.
[0004] Among the secondary batteries, the lithium-sulfur secondary battery is a secondary battery that uses a sulfur-based compound having a sulfur-sulfur bond as a positive electrode active material, and uses an alkali metal such as lithium, a carbon-based material in which metal ions such as lithium ions are intercalated and deintercalated, or silicon or tin that forms an alloy with lithium as a negative electrode active material. Specifically, in the case of a lithium-sulfur secondary battery, during discharge as a reduction reaction, as the sulfur-sulfur bond is cut, the oxidation value of sulfur decreases, and during charging as an oxidation reaction, as the oxidation value of sulfur increases, the sulfur-sulfur bond is reformed. Through this oxidation-reduction reaction, electrical energy is stored and generated.
[0005] In particular, sulfur used as a positive electrode active material in a lithium-sulfur secondary battery has a theoretical energy density of 1.675 mAh / g, and thus has a theoretical energy density of about four times that of a positive electrode active material used in a conventional lithium secondary battery, thereby enabling the battery to exhibit high power and high energy density. In addition, since sulfur has the advantages of being cheap and abundant in resources, it is easily available and environmentally friendly, and sulfur has attracted attention as an energy source not only for portable electronic devices but also for medium and large devices such as electric vehicles.
[0006] In lithium-sulfur batteries, the conductivity of sulfur used as the positive electrode active material is 5×10 -30 S / cm, so it is a non-conductor with no conductivity, and there is a problem that electrons generated by electrochemical reactions have difficulty in moving. Therefore, it is used as a sulfur-carbon composite combined with a conductive material such as carbon, which can provide an electrochemical reaction site.
[0007] In order to use the sulfur-carbon composite as a positive electrode material, a method of manufacturing a positive electrode through a slurry process of preparing a slurry together with a conductive material and a binder and then applying the slurry to a current collector is generally used.
[0008] However, the problem with the positive electrode manufactured by the slurry process is that the loading amount of the positive electrode is reduced due to the conductive material and binder used in the slurry preparation, so that the energy density is also reduced. In addition, the problem with the slurry process is that a series of detailed processes including mixing, coating, drying and calendering require time and cost increases.
[0009] Therefore, there is a need to develop a technology capable of producing a positive electrode for a lithium secondary battery having a high loading amount through a simple process.
[0010] [Prior art literature]
[0011] [Patent Document]
[0012] (Patent Document 1) Korean Patent Publication No. 2019-0100152
[0013] (Patent Document 2) Chinese Patent Publication No. 109873120
[0014] (Patent Document 3) U.S. Patent Publication No. 2018-0212252 Summary of the invention
[0015]
Technical issues
[0016] In one aspect of the present disclosure, the inventors conducted various studies to solve the above-mentioned problems, and as a result, confirmed that a self-supporting film-type positive electrode material made of a carbon-containing sulfur melt can be prepared by a dry method, in which the sulfur-carbon composite is subjected to pressurized conditions by using the property of melting sulfur formed on the surface of the sulfur-carbon composite under pressurized conditions and aggregating with the surrounding sulfur and the flexibility of the carbon material; and confirmed that the self-supporting film-type positive electrode material itself can be used as a positive electrode of a lithium secondary battery.
[0017] Therefore, an object of one aspect of the present disclosure is to provide a positive electrode material for a self-standing film type lithium secondary battery containing a sulfur melt containing carbon and a method for preparing the same.
[0018] Another object of another aspect of the present disclosure is to provide a lithium secondary battery including a positive electrode material for a self-standing film type lithium secondary battery.
[0019]
Technical solution
[0020] To achieve the above object, one aspect of the present disclosure provides a positive electrode material for a lithium secondary battery in the form of a self-standing film, wherein the positive electrode material comprises a carbon-containing sulfur melt.
[0021] The present invention also provides a method for manufacturing a positive electrode material for a lithium secondary battery, comprising the following steps:
[0022] (S1) mixing sulfur with a porous carbon material;
[0023] (S2) heat-treating the mixture formed in step (S1); and
[0024] (S3) The sulfur-carbon composite formed in step (S2) is filled in a container and then pressurized to form a sulfur melt containing carbon.
[0025] The present invention also provides a lithium secondary battery, comprising: a positive electrode comprising the positive electrode material; a negative electrode comprising lithium metal or a lithium alloy; a separator placed between the positive electrode and the negative electrode; and an electrolyte impregnating the positive electrode, the negative electrode and the separator.
[0026]
Beneficial Effects
[0027] The positive electrode material according to the present invention includes a carbon-containing sulfur melt made of only sulfur and a porous carbon material to achieve a high loading amount of the positive electrode.
[0028] In addition, the cathode material itself can be used as a self-standing film type cathode, rather than a method of using a slurry coating a current collector.
[0029] In addition, the positive electrode material can be prepared by a simple dry process (rather than a slurry process including a series of detailed processes of mixing, coating, drying and calendering), in which sulfur and a porous carbon material are mixed, then heat-treated, and then pressurized, thereby improving process efficiency in terms of cost and time. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 is a schematic diagram showing changes in physical properties and moldability when sulfur, carbon, and a sulfur-carbon composite that can be used as a positive electrode material for a lithium secondary battery are pressed.
[0031] Figure 2 is a photograph of the self-standing film type positive electrode material prepared in Example 1.
[0032] Figure 3 is a photograph of the positive electrode material prepared in Comparative Example 3.
[0033] Figures 4a to 4e is a graph showing the measurement results of the initial discharge capacity of coin cells to which the positive electrode materials prepared in Examples and Comparative Examples were applied.
[0034] Figure 5 is a graph showing the measurement results of the life characteristics of coin cells to which the positive electrode materials prepared in Example 2 and Comparative Example 2 were applied.
[0035] Figure 6 1 is a SEM photograph of the carbon nanotube (CNT) and the sulfur-carbon composite (S-CNT) of Preparation Example 1. DETAILED DESCRIPTION
[0036] Hereinafter, in order to facilitate understanding of the present invention, the present invention will be described in more detail.
[0037] The terms and words used in this specification and claims should not be construed as limited to general terms or terms in dictionaries, but should be interpreted with meanings and concepts consistent with the technical concept of the present invention based on the principle that the inventor can appropriately define the concepts of the terms and thus interpret his invention in the best possible manner.
[0038] As used herein, the term "self-standing film" refers to a film that is capable of maintaining the shape of the film by itself without additional support at room temperature and atmospheric pressure.
[0039] As used herein, the term "carbon-containing sulfur melt" refers to a material in which a porous carbon material is dispersed inside the sulfur melt, which can be prepared by heat treatment and pressurization using sulfur and carbon as raw materials.
[0040] Positive electrode materials for lithium secondary batteries
[0041] One aspect of the present disclosure provides a positive electrode material for a lithium secondary battery in the form of a self-supporting film, wherein the positive electrode material contains a carbonaceous sulfur melt. The positive electrode material may be in a form in which a porous carbon material is dispersed in the sulfur melt. In addition, as will be described later, since the positive electrode material is prepared by a dry method using only sulfur and porous carbon materials as raw materials, it may consist only of sulfur and porous carbon materials.
[0042] Generally, the sulfur-carbon composite used as the positive electrode material of the lithium secondary battery refers to a composite in which sulfur is loaded on a porous carbon material. For example, sulfur can be uniformly attached or coated on the surface of the porous carbon material. In addition, sulfur can be attached, filled or coated in the internal pores of the porous carbon material.
[0043] However, in one aspect of the present disclosure, the positive electrode material may include a carbon-containing sulfur melt, wherein the porous carbon material is dispersed inside the sulfur melt, and due to the property of sulfur melting and agglomerating under pressurized conditions, it can be easily formed, and due to the flexibility of the porous carbon material, it can be prepared in the form of a self-supporting film.
[0044] The positive electrode material in the form of a self-standing film may not be coated on a current collector, but the positive electrode material in the form of a self-standing film itself may be used as a positive electrode.
[0045] Since the positive electrode material is prepared by a dry method using sulfur and porous carbon material as raw materials, it contains only sulfur and porous carbon material, so it has the advantage of high loading when used as a positive electrode. In addition, the dry method can omit a series of processes such as mixing, defoaming, coating, drying and calendering required in the conventional slurry process, thereby reducing the process cost. In addition, since the dry method does not use slurry, the carbonaceous sulfur melt prepared by the dry method does not contain any adhesive, so that the battery performance degradation caused by the resistance of the adhesive can be fundamentally eliminated. In addition, since the carbonaceous sulfur melt prepared by the dry method does not contain conductive materials at all, it is possible to minimize the problem of deteriorated formability caused by conductive materials lacking cohesion.
[0046] In addition, in a state where the carbon material forms the skeleton of the positive electrode material, the positive electrode material is connected by the sulfur melt formed on the surface of the porous carbon material or surrounding the porous carbon material, thereby showing the form of a self-standing film.
[0047] In addition, the positive electrode material may be a positive electrode material having an adhesive strength of more than 10gf / cm in the positive electrode material after the electrode is pressed and formed. The adhesive strength is generated due to the nature of sulfur that melts and aggregates with the surrounding sulfur during the pressing process. If the adhesive strength of the positive electrode material is less than 10gf / cm, it may be difficult to form an electrode due to the lack of adhesive strength between the positive electrodes. Specifically, the adhesive strength may be more than 10gf / cm, more than 15gf / cm, more than 20gf / cm, more than 25gf / cm, more than 30gf / cm or more than 35gf / cm. In addition, the upper limit of the adhesive strength may be but is not limited to less than 50gf / cm, less than 60gf / cm, less than 70gf / cm, less than 80gf / cm, less than 90gf / cm or less than 100gf / cm. As the adhesive strength in the positive electrode material increases, it can be good in terms of formability, durability and battery performance.
[0048] In addition, the porosity of the positive electrode material may be 68% or less, 65% or less, 60% or less, or 55% or less, and 45% or more, or 50% or more. If the porosity of the positive electrode material exceeds 68%, the durability of the positive electrode may be reduced. If the porosity of the positive electrode material is less than 45%, the battery may have difficulty in operating normally because the space for electrochemical reactions to occur in the pores is narrowed.
[0049] In one aspect of the present disclosure, sulfur can be selected from inorganic sulfur (S8), Li2S n (n ≥ 1, where n is an integer), organic sulfur compounds and carbon-sulfur polymers [(C2S x ) n , 2.5≤x≤50, n≥2, where x and n are integers].
[0050] In addition, based on the total weight of the carbon-containing sulfur melt, the sulfur content may be 50% by weight or more, 55% by weight or more, or 60% by weight or more, 70% by weight or less, 75% by weight or less, or 80% by weight or less. If the sulfur content is less than 50% by weight, as the ratio of sulfur as an electrochemically active material decreases, the thickness of the sulfur melt formed on the surface of the porous carbon material becomes thinner, so that it may be difficult to properly form the carbon-containing sulfur melt, or the amount of sulfur may decrease, and thus the capacity of the battery may decrease. In addition, if the sulfur content is greater than 80% by weight, since the non-conductive sulfur blocks the conductive structure of the porous carbon material, the electrochemical activity is blocked, which may limit the operation of the battery.
[0051] When 50 wt % to 80 wt % of sulfur is contained in the carbon-containing sulfur melt, the positive electrode material can exhibit strong self-aggregation, and the porous carbon material can be well dispersed in the sulfur melt, thereby being able to well form a positive electrode in a self-supporting form.
[0052] In one aspect of the present disclosure, the porous carbon material may have a structure in which pores or voids are formed, or may be a porous carbon material having a high specific surface area, and any material commonly used in the art may be used.
[0053] The porous carbon material may be, but is not limited to, at least one selected from the following: graphite; graphene; carbon black selected from Denka black, acetylene black, Ketjen black, channel black, furnace black, lamp black and thermal black; carbon nanotubes (CNTs) selected from single-walled carbon nanotubes (SWCNTs) and multi-walled carbon nanotubes (MWCNTs); carbon fibers selected from graphite nanofibers (GNFs), carbon nanofibers (CNFs) and activated carbon fibers (ACFs); and activated carbon. Preferably, the porous carbon material may be a carbon nanotube.
[0054] The carbon nanotubes may have more connection points due to structural characteristics, and thus may be more advantageous when forming a self-standing film. Specifically, since the carbon nanotubes have a shape with an aspect ratio greater than 1, they may be advantageously connected to each other to form a self-standing film.
[0055] In addition, graphene refers to a single layer form in which carbon atoms are arranged in a two-dimensional honeycomb shape, is a material having a thin, wide cross-sectional area and excellent conductive properties, and exhibits excellent physical properties such as bending properties and high sensitivity to light. In the present invention, graphene includes at least one selected from reduced graphene formed by reducing graphene oxide and physically exfoliated graphene. The graphene film may be included in the form of surrounding the outer surface of the carbon nanotube, and can suppress sulfur dissolution into the electrolyte during operation of the battery while enhancing the conductive path.
[0056] In addition, based on the total weight of the carbon-containing sulfur melt, the content of the porous carbon material can be more than 20 weight %, more than 25 weight %, more than 30 weight % or more than 35 weight %, and can be less than 40 weight %, less than 45 weight % or less than 50 weight %. If the content of the porous carbon material is less than 20 weight %, the surface area and space that the molten sulfur can fill, adhere to or apply cannot be fully provided, thereby possibly reducing the electrochemical availability (reactivity) of sulfur. If the carbon material is greater than 50 weight %, the sulfur content is relatively low, so that when applied to a lithium secondary battery, the energy density of the battery may be excessively reduced.
[0057] Method for preparing positive electrode material for lithium secondary battery
[0058] Figure 1 is a schematic diagram showing changes in physical properties and moldability when sulfur, carbon, and a sulfur-carbon composite that can be used as a positive electrode material for a lithium secondary battery are pressed.
[0059] Sulfur can be shaped because its surface melts under pressure and exhibits a property of aggregating with surrounding sulfur, but since sulfur has no flexibility, a positive electrode material (positive electrode) in the form of a self-standing film cannot be prepared only from sulfur.
[0060] Since carbon has flexibility but lacks cohesive strength, it cannot be formed independently when pressed, and thus a positive electrode material (positive electrode) in the form of a self-standing film cannot be prepared.
[0061] The sulfur-carbon composite is a composite of sulfur and a porous carbon material. In the case of the sulfur-carbon composite, since sulfur is also present on the outer surface of the porous carbon material, and when pressed, the sulfur present on the outer surface of the porous carbon material melts, whereby the porous carbon material is present in a dispersed form in the sulfur melt and the sulfur-carbon composite can be formed, and since the porous carbon material is flexible, a positive electrode material (positive electrode) in the form of a self-supporting film can also be formed by stamping.
[0062] Therefore, another aspect of the present disclosure provides a method of preparing a positive electrode material for a lithium secondary battery by applying a sulfur-carbon composite to a dry process to form a carbon-containing sulfur melt using the characteristics of the sulfur-carbon composite as described above during pressurization.
[0063] The method for preparing the positive electrode material for a lithium secondary battery comprises the following steps (S1) to (S3):
[0064] (S1) mixing sulfur with a porous carbon material;
[0065] (S2) heat-treating the mixture formed in step (S1); and
[0066] (S3) The sulfur-carbon composite formed in step (S2) is filled in a container and then pressurized to form a sulfur melt containing carbon.
[0067] Hereinafter, each step of the method for preparing the positive electrode material for a lithium secondary battery of the present invention will be described in more detail.
[0068] In step (S1), a mixture of sulfur and porous carbon material, which is a raw material for manufacturing a positive electrode material made of a sulfur melt containing carbon, may be formed. In this case, the types and appropriate weight ranges of sulfur and porous carbon material are the same as above.
[0069] In step (S2), the mixture formed in step (S1) may be heat-treated.
[0070] If the mixture of sulfur and porous carbon material is heated, the sulfur becomes liquid, and then the liquid sulfur enters the interior of the porous carbon material or is coated or adhered to the surface, so that the porous carbon material is dispersed in the liquid sulfur. For example, if the porous carbon material is a carbon nanotube, the liquid sulfur is sucked into the carbon nanotube by capillary action, the sulfur is loaded on the carbon nanotube, and the carbon nanotube is dispersed in the liquid sulfur.
[0071] The heat treatment may be performed above the melting point of sulfur. For example, the heat treatment temperature may be above 130°C, above 140°C, or above 150°C, and below 160°C, below 165°C, or below 170°C. If the heat treatment temperature is lower than 130°C, sulfur will not melt, and thus it is difficult to form a form in which the sulfur is loaded or coated on the carbon material, and it is also difficult to form a form in which the carbon material is dispersed in sulfur. If the heat treatment temperature is higher than 170°C, sulfur volatilization may occur, and thus sulfur loss and degradation of manufacturing equipment may be induced.
[0072] In addition, the heat treatment time only needs to melt sulfur by heat treatment and be supported on the porous carbon material or the porous carbon material can be dispersed in sulfur, and it can be 25 minutes or more, 30 minutes or more, and 40 minutes or less, 45 minutes or less, or 50 minutes or less.
[0073] In step (S3), the carbon-containing sulfur melt formed in step (S2) is filled in a container and pressurized to prepare a positive electrode material in the form of a self-standing film.
[0074] The composite of sulfur and carbon has the property of showing strong self-cohesion under pressure. Specifically, under pressure, the sulfur on the surface of the sulfur-carbon composite partially melts to provide connectivity, thereby showing strong self-cohesion. Therefore, if pressure is applied to the sulfur-carbon composite, a sulfur melt in which carbon is dispersed is formed, and cohesive force is generated between carbon particles, and also because the carbon material acts as a skeleton and has flexibility itself, a self-supporting film is formed.
[0075] The pressure during pressurization may be a pressure at which cohesion is sufficiently generated between the sulfur-carbon composite to form a self-supporting film. For example, the pressure during pressurization may be 0.8 MPa or more, 0.9 MPa or more, or 1 MPa or more, and 5 MPa or less, 8 MPa or less, 10 MPa or less, 13 MPa or less, or 15 MPa or less. If the pressure during pressurization is less than 0.8 MPa, the cohesion between the sulfur-carbon composite is weak, and a self-supporting film may not be formed. If the pressure during pressurization exceeds 15 MPa, the porosity of the positive electrode material is too low, and the structure of the electrode may collapse.
[0076] Lithium secondary battery
[0077] Another aspect of the present disclosure also relates to a lithium secondary battery including the self-standing film type positive electrode material containing the carbon-containing sulfur melt as described above as a positive electrode.
[0078] If the self-supporting film type positive electrode material is used as a positive electrode, the loading amount of the positive electrode active material in the positive electrode can be 3.0 mAh / cm 2 Up to 5.0mAh / cm 2 , which may be due to the fact that the cathode materials are prepared by a dry process without the need for binders or conductive materials.
[0079] The lithium secondary battery according to the present invention comprises a positive electrode, a negative electrode and an electrolyte interposed therebetween, wherein the positive electrode material in the form of a self-standing film as described above as the positive electrode itself can be used as the positive electrode.
[0080] In addition, in the lithium secondary battery according to the present invention, the negative electrode is manufactured by forming a negative electrode active material layer having a negative electrode active material on a negative electrode current collector, or may be only a negative electrode active material layer (eg, lithium foil).
[0081] At this time, the types of the negative electrode current collector and the negative electrode active material layer are not particularly limited in the present invention, and known materials may be used.
[0082] In addition, the negative electrode current collector is not particularly limited as long as it has conductivity and does not cause chemical changes in the battery. For example, as the negative electrode current collector, copper, stainless steel, aluminum, nickel, titanium, sintered carbon; copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc.; aluminum-cadmium alloy, etc. can be used. In addition, like the positive electrode current collector, the shape of the negative electrode current collector can be various forms, such as a film, sheet, foil, net, porous body, foam, non-woven fabric, etc. having fine concavoconvex on the surface.
[0083] In addition, the negative electrode active material may include, but is not limited to: at least one carbon-based material selected from crystalline artificial graphite, crystalline natural graphite, amorphous hard carbon, low-crystalline soft carbon, carbon black, acetylene black, Ketjen black, Super-P, graphene and fibrous carbon; Si-based materials; metal composite oxides such as Li x Fe2O3(0≤x≤1), Li x WO2(0≤x≤1), Sn x Me 1-x Me' y O z (Me: Mn, Fe, Pb, Ge; Me': Al, B, P, Si, elements of Group 1, Group 2 and Group 3 of the periodic table, halogen; 0<x≤1; 1≤y≤3; 1≤z≤8); lithium metal; lithium alloy; silicon alloy; tin alloy; metal oxides, such as SnO, SnO2, PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4, Bi2O5; conductive polymers, such as polyacetylene; Li-Co-Ni materials; titanium oxide; lithium titanium oxide.
[0084] In addition, the negative electrode active material can be a metal composite oxide, such as Sn x Me 1-x Me' y O z (Me: Mn, Fe, Pb, Ge; Me': Al, B, P, Si, elements of Group 1, Group 2 and Group 3 of the periodic table, halogen; 0<x≤1; 1≤y≤3; 1≤z≤8); oxides, such as SnO, SnO2, PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4 and Bi2O5, and carbon-based negative electrode active materials such as crystalline carbon, amorphous carbon or carbon composites can be used alone or in combination of two or more.
[0085] In addition, in the lithium secondary battery according to the present invention, any of those electrolytes conventionally used in the manufacture of lithium secondary batteries can be used as the electrolyte.
[0086] For example, a lithium salt that can be contained as an electrolyte in an electrolyte solution can be used without limitation as long as it is generally used in an electrolyte solution for a lithium secondary battery. For example, the anion of the lithium salt can be any one selected from the following: - , Cl - Br - ,I - 、NO3 - 、N(CN)2 - 、BF4- 、ClO4 - PF6 - 、(CF3)2PF4 - 、(CF3)3PF3 - 、(CF3)4PF2 - 、(CF3)5PF - 、(CF3)6P - CF3SO3 - CF3CF2SO3 - 、(CF3SO2)2N - 、(FSO2)2N - CF3CF2(CF3)2CO - 、(CF3SO2)2CH - 、(SF5)3C - 、(CF3SO2)3C - CF3(CF2)7SO3 - CF3CO2 - 、CH3CO2 - 、SCN - and (CF3CF2SO2)2N - Specifically, the lithium salt may be LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2(bis(perfluoroethylsulfonyl)imide lithium, BETI), LiN(CF3SO2)2(bis(trifluoromethanesulfonyl)imide lithium, LiTFSI), LiN(C a F 2a+1 SO2)(C b F 2b+1 SO2) (wherein a and b are natural numbers, preferably 1≤a≤20, 1≤b≤20), poly[4,4'-(hexafluoroisopropylidene)diphenoxy]sulfonyl imide lithium (LiPHFIPSI), LiCl, LiI, LiB(C2O4)2, LiNO3, etc. Among them, sulfonyl-containing lithium imide compounds such as LiTFSI, BETI or LiPHFIPSI can be more preferred.
[0087] In the electrolyte used in the present invention, the organic solvent contained in the electrolyte can be used without restriction, as long as it is commonly used in lithium secondary battery electrolyte. Usually, representatively, it can be selected from propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), methyl propyl carbonate, dipropyl carbonate, tetraethylene glycol dimethyl ether (TEGDME), dioxolane (DOL), dimethyl sulfoxide, acetonitrile, dimethoxyethane, diethoxyethane, vinylene carbonate, cyclopentane, gamma-butyrolactone, propylene sulfite and tetrahydrofuran at least one, and a mixture of two or more thereof. In particular, ethylene carbonate and propylene carbonate as cyclic carbonates among carbonate organic solvents are high viscosity organic solvents, which can be preferably used due to having a high dielectric constant and dissociating lithium salts well in the electrolyte. If such a cyclic carbonate is mixed with a linear carbonate having low viscosity and low dielectric constant such as dimethyl carbonate and diethyl carbonate at an appropriate ratio, an electrolyte having high conductivity can be prepared, and thus it can be more preferably used.
[0088] In addition, in the lithium secondary battery according to the present invention, the separator can be a conventional porous polymer film conventionally used as a separator. For example, as a separator, a porous polymer film made of a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer and an ethylene / methacrylate copolymer can be used alone, or they can be laminated and used, or a conventional porous non-woven fabric can be used, such as a non-woven fabric made of a high melting point glass fiber, a polyethylene terephthalate fiber, etc., but is not limited thereto.
[0089] The type of the lithium secondary battery as described above is not particularly limited, and may be, for example, a jelly-roll type, a stack type, a stack-folding type (including a stack-Z-folding type), or a layer-stack type, preferably a stack-folding type.
[0090] The negative electrode, separator, and positive electrode as described above are sequentially stacked, and an electrolyte is injected to prepare an electrode assembly, and then the electrode assembly is placed in a battery case and sealed with a cap plate and a gasket to manufacture a lithium secondary battery.
[0091] In this case, lithium secondary batteries can be divided into various types of batteries according to the materials of the positive / negative electrodes used, such as lithium-sulfur secondary batteries, lithium-air batteries, lithium-oxide batteries, and lithium all-solid-state batteries, and can be divided into cylindrical, rectangular, coin-shaped, and bag-shaped according to the type, and can be divided into block and film types according to the size. The structures and preparation methods of these batteries are well known in the art, so their detailed description is omitted.
[0092] In the present invention, since the lithium secondary battery uses a positive electrode material in the form of a self-supporting film containing a carbonaceous sulfur melt as a positive electrode, it can be a lithium-sulfur secondary battery. The lithium-sulfur secondary battery can use lithium metal as a negative electrode active material. During the discharge of the lithium-sulfur secondary battery, an oxidation reaction of lithium occurs at the negative electrode, and a reduction reaction of sulfur occurs at the positive electrode. At this time, the reduced sulfur combines with the lithium ions moved from the negative electrode, thereby converting into lithium polysulfide, and finally forming lithium sulfide with the reaction.
[0093] In addition, the present invention relates to a battery module including a lithium secondary battery, which can be used as a power source for devices requiring high capacity and high rate characteristics, etc. Specific examples of the device may include, but are not limited to, electric tools powered by electric motors; electric vehicles, including electric vehicles (EVs), hybrid electric vehicles (HEVs), plug-in hybrid electric vehicles (PHEVs), etc.; electric two-wheeled vehicles, including electric bicycles (E-bikes) and electric scooters (Escooters); electric golf carts; and power storage systems.
[0094] Example
[0095] Hereinafter, preferred embodiments are provided to facilitate understanding of the present invention. However, it will be apparent to those skilled in the art that the following embodiments are merely examples of the present invention, and various changes and modifications may be made within the scope and spirit of the present invention, and such changes and modifications also fall within the scope of the appended claims.
[0096] Preparation Example 1: Preparation of sulfur-carbon composite
[0097] Sulfur (S) and carbon nanotubes (CNTs) were uniformly mixed in a solid state at a weight ratio of 65:35 and then ball-milled at 100 rpm for 1 hour to prepare a mixture.
[0098] The mixture was heat treated at 155° C. for 35 minutes to load sulfur into the pores of the CNTs and coat the surfaces thereof to prepare a sulfur-carbon composite (S-CNT). 2 / g of CNT specific surface area.
[0099] Example 1
[0100] (1) Preparation of self-standing film type positive electrode materials
[0101] The sulfur-carbon composite (S-CNT) of Preparation Example 1 was filled in a mold and pressurized at a pressure of 1 MPa using a hydraulic press to form a carbon-containing sulfur melt, thereby preparing a self-standing film-type positive electrode material, such as Figure 2 as shown in .
[0102] (2) Manufacturing of lithium-sulfur secondary batteries
[0103] The prepared self-standing film type positive electrode material was prepared as a positive electrode, and lithium metal having a thickness of 150 μm was prepared as a negative electrode.
[0104] Lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) having a concentration of 1 M and lithium nitrate (LiNO 3 ) having a concentration of 0.1 M were mixed in an organic solvent formed by mixing tetraethylene glycol dimethyl ether (TEGDME) / dioxolane (DOL) / dimethoxyethane (DME) in a volume ratio of 1:1:1 to prepare an electrolyte.
[0105] A porous polyethylene separator having a thickness of 20 μm and a porosity of 45% was interposed between the positive electrode and the negative electrode to prepare an electrode assembly, and the electrode assembly was placed inside the case, and then an electrolyte was injected into the case to prepare a lithium-sulfur secondary battery.
[0106] Example 2
[0107] The same method as in Example 1 was performed except that the pressure when the sulfur-carbon composite was pressurized was 1.5 MPa.
[0108] Example 3
[0109] The same method as in Example 1 was performed except that the pressure when the sulfur-carbon composite was pressurized was 3 MPa.
[0110] Comparative Example 1
[0111] A lithium-sulfur secondary battery was prepared in the same manner as in Example 1, except that the sulfur-carbon composite (S-CNT) of Preparation Example 1, a conductive material, and a binder were mixed in a weight ratio of 90:5:5 to prepare a slurry, which was then coated on an aluminum foil, dried and wound to prepare a positive electrode.
[0112] At this time, the conductive material is VGCF (vapor grown carbon fiber), and the binder is SBR (styrene butadiene rubber).
[0113] In addition, the porosity of the positive electrode was set to 68% by rolling.
[0114] Comparative Example 2
[0115] A lithium-sulfur secondary battery was prepared in the same manner as in Comparative Example 1, except that the thickness after rolling was reduced relative to Comparative Example 1 so that the porosity of the positive electrode was 65%.
[0116] Comparative Example 3
[0117] A lithium-sulfur secondary battery was prepared in the same manner as in Comparative Example 1, except that the thickness after rolling was reduced relative to Comparative Example 2, so that the porosity of the positive electrode was 58%.
[0118] Comparative Example 4
[0119] The same method as in Example 1 was performed except that the pressure when the sulfur-carbon composite was pressurized was 0.5 MPa.
[0120] Comparative Example 5
[0121] The same method as in Example 1 was performed except that the pressure when the sulfur-carbon composite was pressurized was 20 MPa.
[0122] Comparative Example 6
[0123] A lithium-sulfur secondary battery was prepared in the same manner as in Example 1, except that 10 wt % of CNT as a conductive material was filled into a mold together with the sulfur-carbon composite and pressed. At this time, the content of the conductive material was based on the total weight of the sulfur-carbon composite and the conductive material.
[0124] Experimental Example 1: Comparison of process time
[0125] The time required for the process of preparing the positive electrode material in the examples and the comparative examples was measured and compared. The time required for the process is shown in Table 1 below.
[0126] Table 1:
[0127]
[0128] As shown in the above Table 1, it can be seen that in Examples 1, 2, and 3, since the positive electrode material was prepared using a dry process including only filling and pressing processes as detailed processes, the total process time was less than 1 hour.
[0129] In contrast, it can be seen that in Comparative Examples 1, 2, and 3, since the positive electrode material was prepared using a slurry process including mixing, coating, drying, and calendering processes as detailed processes, the total process time all exceeded 5 hours.
[0130] From these results, it was confirmed that the process efficiency can be improved if the positive electrode material is produced by a dry process.
[0131] Experimental Example 2: Measurement of Porosity of Positive Electrode Material and Adhesion Strength in Positive Electrode Material
[0132] The porosities of the positive electrodes prepared in Example and Comparative Example were measured and compared, and the results are shown in Table 2.
[0133] The porosity was calculated by calculating the density of the positive electrode based on the weight and thickness of the positive electrode and then back-calculating using the true densities of sulfur and carbon (true density of sulfur: 2.07 mg / cc, true density of carbon: 2.00 mg / cc).
[0134] The adhesive strength was measured using an adhesive strength measuring device (AMETEK Corporation, LS1).
[0135] Table 2:
[0136]
[0137] As shown in Table 2 above, it was confirmed that, in the case of Examples 1, 2, and 3 in which the positive electrode materials were produced by the dry method, as the pressure at the time of pressurization increased, the porosity decreased and the adhesive strength in the positive electrode material increased.
[0138] Furthermore, it was confirmed that in the case of Comparative Examples 1, 2, and 3 in which the positive electrode materials were prepared by the wet method, as the number of rolling times increased, the porosity decreased and the adhesive strength in the positive electrode material increased.
[0139] If the porosity of the positive electrode material is too high, durability is reduced, and if the porosity is too low, electrical conductivity or ion conductivity is reduced. Therefore, in order to express appropriate porosity, it is also necessary to appropriately control the pressure during pressurization.
[0140] Figure 3 is a photograph of the positive electrode material obtained in Comparative Example 4. It can be seen that in the case of Comparative Example 4, a carbon-containing sulfur melt was not formed due to low pressure during pressurization and thus lack of cohesion between sulfur-carbon composites, and thus a positive electrode material was not prepared.
[0141] It can be seen that in the case of Comparative Example 5, the porosity was significantly reduced due to the high pressure during pressurization, and in the case of Comparative Example 6, that is, in the case where a separate conductive material was externally added to the sulfur-carbon composite, the adhesive strength was significantly reduced.
[0142] Experimental Example 3: Measurement of Capacity and Charging Efficiency
[0143] For the batteries manufactured in the examples and comparative examples, the capacity (mAh) was measured by discharging at 0.1C and charging at 0.1C at 25°C, the capacity and the charging efficiency were measured by repeating charging and discharging to measure the capacity, and the results are shown in the following Tables 3 and Figures 4a to 4e As shown in Table 2 above, in the case of Comparative Example 4, due to the low pressurization pressure, there was a lack of cohesive force between the sulfur-carbon composites, and thus no electrode was produced. Therefore, Examples 1 to 3 and Comparative Examples 1 to 3, 5, and 6 were experimented.
[0144] Table 3:
[0145]
[0146] Refer to Table 3 above. Figure 4a , Figure 4b and Figure 4c, it was confirmed that Examples 1, 2 and 3, which were electrodes manufactured by a dry method, had improved overvoltage in an initial discharge curve and higher initial discharge capacity compared to Comparative Examples 1, 2 and 3 manufactured by a wet method.
[0147] Generally, porosity is an important factor in lithium-sulfur secondary batteries. This means that the lower the porosity, the more compact the battery. However, as the porosity decreases, the reaction space becomes narrower. Therefore, it may happen that the battery has difficulty in working properly at lower porosity.
[0148] However, it was confirmed that when Examples 1, 2, and 3 manufactured by the dry method had the same porosity as Comparative Examples 1, 2, and 3 manufactured by the wet method, they showed improvement in overvoltage and higher initial discharge capacity.
[0149] In addition, refer to Table 3 and Figure 4d , it was confirmed that in the case of Comparative Example 5, the pressure applied during the production of the positive electrode material was as high as 20 MPa, and the porosity was excessively reduced, so the battery could not function normally.
[0150] In addition, refer to Table 3 and Figure 4e It was confirmed that in the case of Comparative Example 6, when the positive electrode material was manufactured by a dry method by adding CNT as a conductive material in addition to the sulfur-carbon composite, it was difficult to form the positive electrode material during pressurization due to the lack of cohesion of the carbon itself, and the capacity of the positive electrode material was not as good as that of Example 1 in which no conductive material was added.
[0151] in addition, Figure 5 is a graph showing the results of measuring the life characteristics of coin cells using the positive electrode materials prepared in Example 2 and Comparative Example 2. It can be seen that the life characteristics of the cell including the electrode of Example 2 manufactured by the dry method are improved.
[0152] Experimental Example 4: Confirmation of the internal shape of the positive electrode material
[0153] The internal shape was confirmed after applying a pressing process to the carbon nanotubes (CNT) and the sulfur-carbon composite (S-CNT) used as raw materials in Preparation Example 1. The pressing process was applied as shown in Example 1 (1).
[0154] After carbon nanotubes (CNTs) and sulfur-carbon composites (S-CNTs) were filled in the mold, it was pressurized at a pressure of 1 MPa using a hydraulic press, and then the internal shape was confirmed using a scanning electron microscope (SEM).
[0155] Figure 6 1 is a SEM photograph of the carbon nanotube (CNT) and the sulfur-carbon composite (S-CNT) of Preparation Example 1.
[0156] like Figure 6As shown in , it was found that CNTs were not connected to each other due to lack of connectivity between CNTs, and were not connected to each other even after the pressing process.
[0157] In addition, it was found that by dispersing CNTs in a sulfur melt formed by melting sulfur, sulfur-carbon composites (S-CNTs) were connected as a whole. This is due to the fact that when the melting point of sulfur is lowered during the high pressure process and the melting of sulfur occurs instantaneously on the surface of the sulfur-carbon composite, CNTs are connected as a whole by the formed sulfur melt. That is, it can be seen that CNTs are dispersed in the sulfur melt.
[0158] Although the present invention has been described above with the aid of limited embodiments and drawings, the present invention is not limited thereto. Those skilled in the art may make various modifications and changes within the technical concept of the present invention and the equivalent scope of the appended claims.
Claims
1. A positive electrode material for a lithium secondary battery in the form of a self-supporting film, wherein the positive electrode material is a sulfur melt containing carbon, The carbon-containing sulfur melt is in the form of porous carbon material dispersed inside the sulfur melt, The porous carbon materials are not connected to each other. 2 . The positive electrode material for a lithium secondary battery according to claim 1 , wherein the carbon-containing sulfur melt consists of 50 to 80 wt % of sulfur and 20 to 50 wt % of a porous carbon material. 3 . The positive electrode material for a lithium secondary battery according to claim 1 , wherein the adhesive strength inside the positive electrode material is 10 gf / cm or more.
4. The positive electrode material for a lithium secondary battery according to claim 1, wherein the porous carbon material is at least one selected from the following: graphite; graphene; carbon black selected from Danka black, acetylene black, Ketjen black, channel black, furnace black, lamp black and thermal black; carbon nanotubes (CNTs) selected from single-walled carbon nanotubes (SWCNTs) and multi-walled carbon nanotubes (MWCNTs); carbon fibers selected from graphite nanofibers (GNFs), carbon nanofibers (CNFs) and activated carbon fibers (ACFs); and activated carbon. 5 . The positive electrode material for a lithium secondary battery according to claim 1 , wherein the porosity of the positive electrode material is 68% or less.
6. A method for preparing the positive electrode material for a lithium secondary battery according to claim 1, the method comprising the following steps: (S1) mixing sulfur with a porous carbon material; (S2) heat-treating the mixture formed in step (S1); and (S3) Forming a sulfur melt containing carbon by filling the sulfur-carbon composite formed in step (S2) in a container and then pressurizing it. 7 . The method for preparing a positive electrode material for a lithium secondary battery according to claim 6 , wherein the heat treatment is performed at 130° C. to 170° C. 8 . The method for preparing a positive electrode material for a lithium secondary battery according to claim 6 , wherein the pressurizing is performed at a pressure of 0.8 MPa to 15 MPa.
9. A lithium secondary battery, comprising: A positive electrode comprising the positive electrode material according to any one of claims 1 to 5; a negative electrode comprising lithium metal or a lithium alloy; a separator disposed between the positive electrode and the negative electrode; and The positive electrode, the negative electrode and the separator are impregnated with an electrolyte. 10 . The lithium secondary battery according to claim 9 , wherein the lithium secondary battery is a lithium-sulfur secondary battery.
11. The lithium secondary battery according to claim 9, wherein the positive electrode loading is 3.0 mAh / cm 2 Up to 5.0mAh / cm 2 .
Citation Information
Patent Citations
Preparation method of metal-free current collector and self-supported graphene-based lithium-sulfur battery anode
CN109873120A
Rapid sulfur melt diffusion into carbon host for making electrodes
US20180212252A1
Method for manufacturing carbon-sulfur composite, carbon-sulfur composite manufactured thereby, and lithium-sulfur battery including same
CN103828101A
Sulfur-carbon composite and method for manufacturing the same
KR1020150014793A
Freestanding type-cathode active material for lithium-sulfur battery and lithium-sulfur battery having the same
KR1020160051610A