Binder and electrochemical device including the same

By using polymer binders containing specific structural units in lithium-ion batteries, the problem of insufficient amount of binders for lithium-ion batteries is solved, the adhesion and kinetic performance of the battery is improved, and the cycle life of the battery is extended.

CN114207883BActive Publication Date: 2024-11-12NINGDE AMPEREX TECHNOLOGY LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180003987.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-03-24
Publication Date
2024-11-12
Estimated Expiration
2041-03-24

AI Technical Summary

Technical Problem

Inadequate amount of adhesive used in lithium-ion batteries leads to a decrease in bonding effect and cannot withstand the stress of changes in the volume of the main material, resulting in a decrease in the cell cycle life and a deterioration in the kinetic performance.

Method used

Develop a polymer binder containing specific structural units, forming a π-π conjugated force with graphite through the benzene ring structure, the phenolic hydroxyl group and the metal current collector have a polar force, and the salting of anionic groups helps desolvate lithium ions , improve the dynamic performance of electrochemical devices.

Benefits of technology

It improves the adhesion and dynamic performance of lithium-ion batteries, alleviates the obstruction of lithium-ion embedding, extends the battery cycle life and improves capacity retention.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114207883B_ABST
    Figure CN114207883B_ABST
Patent Text Reader

Abstract

A binder and an electrochemical device comprising the binder, wherein the binder is a polymer containing structural units shown in formula I, formula II and formula III, wherein R 1 is independently selected from any one of substituted or unsubstituted C1-C10 alkyl, substituted or unsubstituted C2-C10 alkenyl, substituted or unsubstituted C2-C10 alkynyl, and substituted or unsubstituted C6-C20 aryl; R 2 is selected from phenolic hydroxyl groups, and the number of phenolic hydroxyl groups is 2 to 5; R 3 is selected from any one of C, S, N, and P; X is selected from any one of Li, Na, and K; R 4 , R 5 Each is independently selected from any one of a hydrogen atom, a substituted or unsubstituted C1-C10 alkyl group, a substituted or unsubstituted C2-C10 alkenyl group, a substituted or unsubstituted C2-C10 alkynyl group, and a substituted or unsubstituted C6-C20 aryl group; n1, n2, and n3 are each independently an integer greater than zero. The binder has a high bonding force, helps to desolvate lithium ions, alleviates the obstruction of lithium ion insertion, and improves the kinetic performance of electrochemical devices. #imgabs0#
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present application relates to the field of secondary batteries, and in particular, to a binder and an electrochemical device comprising the binder. [Background technology]

[0002] At present, lithium-ion battery binders provide bonding effects in pole pieces. Since they do not participate in the deintercalation of lithium from the main material, the less they are used, the better. However, a decrease in the amount used will inevitably lead to a decrease in the bonding effect, causing the active main material to be delaminated from the current collector. In addition, some alloy-type main material particles (such as silicon) undergo huge volume changes when deintercalating lithium. Binders with low bonding effects cannot withstand the stress caused by the huge volume deformation, resulting in failure of bonding between particles and unrestricted slippage between particles, which reduces the cycle life of the battery cell and continuously increases the cycle thickness.

[0003] Conventional binders completely cover the particle surface, which hinders the insertion of lithium ions and causes poor charging and discharging dynamics of lithium batteries. [Summary of the invention]

[0004] In view of this, the present application proposes a binder and an electrochemical device comprising the binder, wherein the binder has a high bonding force, helps desolvation of lithium ions, alleviates the obstruction of lithium ion insertion, and improves the kinetic performance of the electrochemical device. In a first aspect, the present application provides a binder, wherein the binder is a polymer containing structural units shown in Formula I, Formula II, and Formula III:

[0005]

[0006] Wherein, R1 is independently selected from any one of substituted or unsubstituted C1-C10 alkyl, substituted or unsubstituted C2-C10 alkenyl, substituted or unsubstituted C2-C10 alkynyl, substituted or unsubstituted C6-C20 aryl;

[0007] R2 is selected from phenolic hydroxyl groups, and the number of the phenolic hydroxyl groups is 2 to 5;

[0008] R3 is selected from any one of C, S, N, and P; X is selected from any one of Li, Na, and K;

[0009] R4 and R5 are each independently selected from any one of a hydrogen atom, a substituted or unsubstituted C1-C10 alkyl group, a substituted or unsubstituted C2-C10 alkenyl group, a substituted or unsubstituted C2-C10 alkynyl group, and a substituted or unsubstituted C6-C20 aryl group;

[0010] n1, n2, and n3 are each independently an integer greater than zero.

[0011] In combination with the first aspect, in a feasible embodiment, R2 in the structural unit shown in Formula I is selected from any one of the following groups:

[0012]

[0013] in, Indicates the binding site with the neighboring atoms.

[0014] In combination with the first aspect, in a feasible implementation manner,

[0015] The molar proportion of the structural unit represented by formula I in the binder is 5 mol% to 30 mol%;

[0016] The molar proportion of the structural unit represented by formula II in the binder is 10 mol% to 60 mol%;

[0017] The molar proportion of the structural unit represented by formula III in the binder is 35 mol % to 55 mol %.

[0018] In combination with the first aspect, in a feasible implementation, the binder further includes a functional monomer with a mass percentage of 0 wt % to 1 wt %, and the functional monomer includes at least one of an acrylamide derivative monomer and an acrylic acid derivative monomer.

[0019] In combination with the first aspect, in a feasible implementation, the acrylamide derivative monomer includes at least one of acrylamide, N-methylacrylamide, N-ethylacrylamide, N-butylacrylamide or NN-methylenebisacrylamide.

[0020] In combination with the first aspect, in a feasible embodiment, the acrylic derivative monomer includes at least one of methyl acrylate, ethyl acrylate, n-butyl acrylate, tert-butyl acrylate, 2-ethylhexyl acrylate, cyclohexyl acrylate, isobornyl acrylate, hydroxyethyl acrylate, hydroxypropyl acrylate, vinyl acetate, methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, 2-ethylhexyl methacrylate, cyclohexyl methacrylate, isobornyl methacrylate, hydroxyethyl methacrylate, hydroxypropyl methacrylate, glycidyl methacrylate or polyoxyethylene diacrylate.

[0021] In combination with the first aspect, in a feasible implementation manner, the pH value of the binder is 3 to 12.

[0022] In combination with the first aspect, in a feasible implementation manner, the adhesive satisfies at least one of the following features a to c:

[0023] a. The glass transition temperature of the binder is 80°C to 200°C;

[0024] b. When the solid content of the binder is 4%, the viscosity of the binder is 1000mPa·s to 20000mPa·s;

[0025] c. The molecular weight of the binder is between 1,000 and 5,000,000.

[0026] In combination with the first aspect, in a feasible embodiment, the binder further includes a solvent, and the solvent is an organic solvent or water. In combination with the first aspect, in a feasible embodiment, the binder further includes an additive, and the additive includes at least one of a dispersant, a leveling agent, a wetting agent, a defoaming agent, and a softener.

[0027] In combination with the first aspect, in a feasible implementation manner, the binder is applied to the negative electrode and / or positive electrode of a lithium-ion battery.

[0028] In a second aspect, an embodiment of the present application provides an electrochemical device, comprising a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein at least one of the positive electrode sheet, the negative electrode sheet and the separator contains the binder described in the first aspect above.

[0029] In combination with the second aspect, in a feasible implementation manner, the negative electrode plate includes a negative electrode current collector and a negative electrode active material layer, and the binder accounts for 3.0 wt % to 6.0 wt % of the negative electrode active material layer.

[0030] Compared with the prior art, this application has at least the following beneficial effects:

[0031] The binder provided by the present application has a benzene ring structure that can form a ππ conjugated force with graphite, a phenolic hydroxyl group and a cyano group that can have a strong polar force with the metal current collector, and a salted anionic group that can provide more lithium ion migration and compete with the solvent around the lithium ions to help lithium ions desolvate, alleviate the obstruction of lithium ion embedding, and improve the kinetic performance of the electrochemical device.

Brief Description of the Drawings

[0032] Figure 1a This is a schematic diagram of the bonding strength test of the adhesive of Example 3 of the present application;

[0033] Figure 1b This is a schematic diagram of the bonding force test of the adhesive of Comparative Example 1 of the present application;

[0034] Figure 2 Schematic diagram of battery charge and discharge test results of Example 3 and Comparative Example 1 of the present application. [Specific implementation method]

[0035] The following is a preferred implementation of the embodiments of the present application. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the embodiments of the present application. These improvements and modifications are also considered to be within the scope of protection of the embodiments of the present application.

[0036] For simplicity, only some numerical ranges are explicitly disclosed herein. However, any lower limit can be combined with any upper limit to form an unambiguous range; and any lower limit can be combined with other lower limits to form an unambiguous range, and any upper limit can be combined with any other upper limit to form an unambiguous range. In addition, although not explicitly stated, each point or single value between the range endpoints is included in the range. Thus, each point or single value can be combined with any other point or single value as its own lower limit or upper limit or with other lower limits or upper limits to form an unambiguous range.

[0037] In the description of this article, it should be noted that, unless otherwise specified, “above” and “below” are inclusive of the number itself, and “multiple” in “one or more” means more than two.

[0038] The above application content of the present application is not intended to describe each disclosed embodiment or each implementation in the present application. The following description more specifically illustrates exemplary embodiments. In many places throughout the application, guidance is provided by a series of examples, which can be used in various combinations. In each example, enumeration is only used as a representative group and should not be interpreted as exhaustive.

[0039] In a first aspect, an embodiment of the present application provides a binder, the structure of which is shown in Formula A:

[0040]

[0041] Specifically, the binder is a polymer containing structural units shown in Formula I, Formula II and Formula III:

[0042]

[0043] Wherein, R1 is independently selected from any one of substituted or unsubstituted C1-C10 alkyl, substituted or unsubstituted C2-C10 alkenyl, substituted or unsubstituted C2-C10 alkynyl, substituted or unsubstituted C6-C20 aryl;

[0044] R2 is selected from phenolic hydroxyl groups, and the number of the phenolic hydroxyl groups is 2 to 5;

[0045] R3 is selected from any one of C, S, N, and P; X is selected from any one of Li, Na, and K;

[0046] R4 and R5 are each independently selected from any one of a hydrogen atom, a substituted or unsubstituted C1-C10 alkyl group, a substituted or unsubstituted C2-C10 alkenyl group, a substituted or unsubstituted C2-C10 alkynyl group, and a substituted or unsubstituted C6-C20 aryl group;

[0047] n1, n2, and n3 are each independently an integer greater than zero.

[0048] The binder provided by the present application has a benzene ring structure that can form a ππ conjugated force with graphite, a phenolic hydroxyl group and a cyano group that can have a strong polar force with the metal current collector, and a salted anionic group that can provide more lithium ion migration and compete with the solvent around the lithium ions to help lithium ions desolvate, alleviate the obstruction of lithium ion embedding, and improve the kinetic performance of the electrochemical device.

[0049] Optionally, the C1-C10 alkyl group may be a chain alkyl group or a cyclic alkyl group, and the chain alkyl group may be a straight chain alkyl group or a branched chain alkyl group, and the hydrogen on the ring of the cyclic alkyl group may be further substituted by an alkyl group. The preferred lower limit of the number of carbon atoms in the C1-C10 alkyl group is 1, 2, 3, or 4, and the preferred upper limit is 5, 6, 8, or 10. Examples of C1-C10 alkyl groups include: methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, isopentyl, neopentyl, hexyl, 2-methyl-pentyl, 3-methyl-pentyl, 1,1,2-trimethylpropyl, 3,3-dimethyl-butyl, heptyl, 2-heptyl, 3-heptyl, 2-methylhexyl, 3-methylhexyl, isoheptyl, octyl, nonyl, and decyl.

[0050] When the aforementioned C1-C10 alkyl group contains an oxygen atom, it may be a C1-C10 alkoxy group. Preferably, a C1-C6 alkoxy group is selected; more preferably, a C1-C4 alkoxy group is selected. Examples of C1-C10 alkoxy groups include: methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy, sec-butoxy, tert-butoxy, n-pentoxy, isopentyloxy, cyclopentyloxy, and cyclohexyloxy.

[0051] The C2-C10 alkenyl group may be a cyclic alkenyl group or a chain alkenyl group, and the chain alkenyl group may be a straight chain alkenyl group or a branched chain alkenyl group. In addition, the number of double bonds in the C2-C10 alkenyl group is preferably 1. The preferred lower limit of the number of carbon atoms in the C2-C10 alkenyl group is 2, 3, 4, and 5, and the preferred upper limit is 3, 4, 5, 6, 8, and 10. Preferably, a C2-C6 alkenyl group is selected; more preferably, a C2-C5 alkenyl group is selected. Examples of C2-C10 alkenyl groups include: vinyl, allyl, isopropenyl, pentenyl, cyclohexenyl, cycloheptenyl, and cyclooctenyl.

[0052] The C2-C10 alkynyl group may be a cyclic alkynyl group or a chain alkynyl group, and the chain alkynyl group may be a straight chain alkynyl group or a branched chain alkynyl group. In addition, the number of triple bonds in the C2-C10 alkynyl group is preferably 1. The preferred lower limit of the number of carbon atoms in the C2-C10 alkynyl group is 2, 3, 4, and 5, and the preferred upper limit is 3, 4, 5, 6, 8, and 10. Examples of C2-C10 alkynyl groups include: ethynyl, propargyl, isopropynyl, pentynyl, cyclohexynyl, and cycloheptynyl.

[0053] The C6-C20 aryl group may be a phenyl group, a phenylalkyl group, a biphenyl group, or a condensed aromatic hydrocarbon group (e.g., a naphthyl group, anthracenyl group, or a phenanthryl group), and the biphenyl group and the condensed aromatic hydrocarbon group may be further substituted by an alkyl group or an alkenyl group. Examples of the C6-C20 aryl group include: a phenyl group, a benzyl group, a biphenyl group, a p-tolyl group, an o-tolyl group, an m-tolyl group, and a naphthyl group.

[0054] The substituent is selected from one or more halogen atoms, and preferably, the substituent is selected from fluorine atoms, chlorine atoms and bromine atoms.

[0055] As an optional technical solution of the present application, the structural unit shown in Formula I is a phenolic hydroxyl group-containing structure, wherein R2 is selected from phenolic hydroxyl groups, and the number of the phenolic hydroxyl groups is 2 to 5. Optionally, R2 is selected from any one of the following groups:

[0056]

[0057] in, Indicates the binding site with the neighboring atoms.

[0058] As an optional technical solution of the present application, the molar proportion of the structural unit shown in Formula I in the binder is 5mol% to 30mol%, which can be 5mol%, 7mol%, 9mol%, 10mol%, 12mol%, 15mol%, 18mol%, 20mol%, 25mol%, 28mol% or 30mol%, etc., and of course it can be other values ​​within the above range, which are not limited here. It can be understood that when the molar proportion of the structural unit shown in Formula I is less than 5mol% or greater than 30mol%, the viscosity of the binder decreases, and the negative electrode active material or the positive electrode active material easily falls off the current collector during the battery cycle, and the capacity retention rate of the battery decreases. Preferably, the molar proportion of the structural unit shown in Formula I in the binder is 10mol% to 25mol%, and further preferably, the molar proportion of the structural unit shown in Formula I in the binder is 15mol% to 20mol%.

[0059] As an optional technical solution of the present application, the structural unit shown in Formula II is an anionic group XO mR3 structure, wherein R3 can be any one of C, S, N, P elements; the number of oxygen m can be 1, 2, 3 or 4, and X can be an element such as Li, Na, K, etc. Preferably, the anion group can be lithium carboxylate, lithium sulfonate, lithium phosphate, etc. It can be understood that the anion group can not only carry more lithium ions and increase the number of lithium ion migration, but also compete with the solvent around the lithium ions to help lithium ions desolvate, alleviate the obstruction of lithium ion embedding, and improve the kinetic performance of the electrochemical device.

[0060] As an optional technical solution of the present application, the molar proportion of the structural unit shown in Formula II in the binder is 10mol% to 60mol%, which can be specifically 10mol%, 15mol%, 20mol%, 25mol%, 30mol%, 35mol%, 40mol%, 45mol%, 50mol%, 55mol% or 60mol%, etc., and of course it can also be other values ​​within the above range, which are not limited here. It can be understood that with the increase of the structural unit shown in Formula II in the binder, that is, the increase of the salted anionic groups in the binder, the binder can provide more lithium ions during the battery cycle, and can compete with the solvent around the lithium ions to help lithium ions desolvate, alleviate the obstruction of lithium ion embedding, and improve the kinetic performance of the electrochemical device. Preferably, the molar proportion of the structural unit shown in Formula II in the binder is 15mol% to 45mol%, and further preferably, the molar proportion of the structural unit shown in Formula II in the binder is 20mol% to 30mol%.

[0061] As an optional technical solution of the present application, the structural unit shown in formula III is a cyano-containing structure, and the structural unit shown in formula III is selected from at least one of the following structural units:

[0062]

[0063] As an optional technical solution of the present application, the molar proportion of the structural unit shown in Formula III in the binder is 35 mol% to 55 mol%, specifically 35 mol%, 40 mol%, 45 mol%, 50 mol% or 55 mol%, etc., and of course it can also be other values ​​within the above range, which are not limited here. It can be understood that with the increase of the structural unit shown in Formula III in the binder, that is, the increase of cyano groups in the binder, the viscosity of the binder gradually increases, the structural stability of the active material layer on the current collector increases, and the capacity retention rate of the battery can be improved. However, when the molar proportion of the structural unit shown in Formula III in the binder is greater than 60%, the viscosity of the binder is too large and cannot be water-soluble, reducing its ease of use. Preferably, the molar proportion of the structural unit shown in Formula III in the binder is 40 mol% to 55 mol%, and further preferably, the molar proportion of the structural unit shown in Formula III in the binder is 50 mol% to 55 mol%.

[0064] As an optional technical solution of the present application, the binder further comprises a functional monomer with a mass percentage of 0wt% to 1wt%, wherein the functional monomer comprises at least one of an acrylamide derivative monomer and an acrylic acid derivative monomer. The functional monomer can improve the mechanical properties of the binder, and improve the solvent resistance, water resistance, gloss retention, color retention, and acid and alkali resistance of the binder.

[0065] As an optional technical solution of the present application, the acrylamide derivative monomer includes at least one of acrylamide, N-methyl acrylamide, N-ethyl acrylamide, N-butyl acrylamide or NN-methylenebisacrylamide.

[0066] As an optional technical solution of the present application, the acrylic acid derivative monomer includes at least one of methyl acrylate, ethyl acrylate, n-butyl acrylate, tert-butyl acrylate, 2-ethylhexyl acrylate, cyclohexyl acrylate, isobornyl acrylate, hydroxyethyl acrylate, hydroxypropyl acrylate, vinyl acetate, methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, 2-ethylhexyl methacrylate, cyclohexyl methacrylate, isobornyl methacrylate, hydroxyethyl methacrylate, hydroxypropyl methacrylate, glycidyl methacrylate or polyoxyethylene diacrylate.

[0067] As an optional technical solution of the present application, the pH value of the binder is 3 to 12, specifically 3, 4, 5, 6, 7, 8, 9, 10, 11 or 12, etc., and of course, it can also be other values ​​within the above range, which is not limited here. Preferably, the pH value of the binder is 6 to 10.

[0068] As an optional technical solution of the present application, the glass transition temperature of the binder is 80°C to 200°C, specifically 80°C, 90°C, 100°C, 110°C, 120°C, 140°C, 150°C, 160°C, 180°C or 200°C, etc. Of course, it can also be other values ​​within the above range, which are not limited here. If the glass transition temperature of the binder is too high, the binder will be hard and brittle, and the pole piece will be cold pressed and demolded; if the glass transition temperature of the binder is too low, it will be in a rubbery state at room temperature, and it will be difficult to maintain the bonding effect of the material particles in the pole piece.

[0069] As an optional technical solution of the present application, when the solid content of the binder is 4%, the viscosity of the binder is 1000mPa·s to 20000mPa·s, specifically 1000mPa·s, 3000mPa·s, 5000mPa·s, 8000mPa·s, 10000mPa·s, 13000mPa·s, 15000mPa·s, 18000mPa·s or 20000mPa·s, etc., of course, it can also be other values ​​within the above range, which are not limited here. The adjustment of monomer components will affect the viscosity of the binder, and the viscosity will affect the slurry stirring and coating process. If the viscosity is too high, the stirring power consumption is large, and the slurry is difficult to level during the coating process; if the viscosity is too low, the coating slurry has good fluidity. Difficulty in leveling and excessive fluidity will lead to coating differentiation, severe fluctuations in coating weight, and the pole piece cannot be used normally.

[0070] As an optional technical solution of the present application, the molecular weight of the binder is between 1000 and 5 million, specifically 1000, 5000, 10,000, 100,000, 500,000, 1 million, 3 million or 5 million, etc., and of course other values ​​within the above range, which are not limited here. The molecular weight of the binder will affect the viscosity of the binder, and the viscosity will affect the slurry stirring and coating process. If the viscosity is too high, the stirring power consumption is large, and the slurry is difficult to level during the coating process; if the viscosity is too low, the coating slurry has good fluidity. Difficulty in leveling and excessive fluidity will lead to coating differentiation, severe fluctuations in coating weight, and the electrode cannot be used normally.

[0071] As an optional technical solution of the present application, the binder also includes a solvent, and the solvent is an organic solvent or water.

[0072] The present invention also relates to a method for preparing the adhesive: the adhesive is prepared by subjecting monomers of formula I, II and III to emulsion polymerization.

[0073] As an optional technical solution of the present application, the binder further includes an additive, and the additive includes at least one of a dispersant, a leveling agent, a wetting agent, a defoaming agent, and a softener.

[0074] As an optional technical solution of the present application, the binder is applied to the negative electrode and / or positive electrode of the lithium-ion battery.

[0075] In a second aspect, an embodiment of the present application further provides an electrochemical device, comprising a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein at least one of the positive electrode sheet, the negative electrode sheet and the separator contains the binder described in the first aspect above.

[0076] As an optional technical solution of the present application, the negative electrode plate includes a negative electrode current collector and a negative electrode active material layer, and the binder accounts for 3.0wt% to 6.0wt% of the negative electrode active material layer, preferably 4.5wt% to 5.5wt%, and more preferably 5wt%.

[0077] As an optional technical solution of the present application, the above-mentioned positive electrode plate includes a positive electrode current collector and a positive electrode active material layer located on the positive electrode current collector.

[0078] As an optional technical solution of the present application, the positive electrode active material includes at least one of lithium cobalt oxide (LiCoO2), lithium nickel manganese cobalt ternary material, lithium iron phosphate, lithium manganese iron phosphate, and lithium manganese oxide.

[0079] As an optional technical solution of the present application, the positive electrode current collector includes, but is not limited to: aluminum foil.

[0080] As an optional technical solution of the present application, the above-mentioned negative electrode plate includes a negative electrode current collector and a negative electrode active material layer located on the negative electrode current collector.

[0081] As an optional technical solution of the present application, the negative electrode active material includes at least one of a silicon negative electrode material, a silicon-oxygen negative electrode material, a silicon-carbon negative electrode material, and a graphite negative electrode material.

[0082] As an optional technical solution of the present application, the negative electrode current collector includes, but is not limited to: copper foil, nickel foil, stainless steel foil, titanium foil, foam nickel, foam copper or a polymer substrate coated with a conductive metal.

[0083] As an optional technical solution of the present application, the electrochemical device further includes an electrolyte, which includes an organic solvent, a lithium salt and an additive.

[0084] The organic solvent of the electrolyte according to the present application can be any organic solvent known in the prior art that can be used as a solvent for the electrolyte. The electrolyte used in the electrolyte according to the present application is not limited, and it can be any electrolyte known in the prior art. The additive of the electrolyte according to the present application can be any additive known in the prior art that can be used as an electrolyte additive.

[0085] In a specific embodiment, the organic solvent includes, but is not limited to, ethylene carbonate (EC), propylene carbonate (PC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), propylene carbonate or ethyl propionate.

[0086] In a specific embodiment, the lithium salt includes at least one of an organic lithium salt or an inorganic lithium salt. In a specific embodiment, the lithium salt includes, but is not limited to: lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium difluorophosphate (LiPO2F2), lithium bis(trifluoromethanesulfonyl)imide LiN(CF3SO2)2 (LiTFSI), lithium bis(fluorosulfonyl)imide Li(N(SO2F)2) (LiFSI), lithium bis(oxalatoborate) LiB(C2O4)2 (LiBOB) or lithium di(oxalatoborate) LiBF2(C2O4) (LiDFOB).

[0087] As an optional technical solution of the present application, the electrochemical device of the present application includes, but is not limited to: all kinds of primary batteries, secondary batteries, fuel cells, solar cells or capacitors.

[0088] In a specific embodiment, the electrochemical device is a lithium secondary battery, wherein the lithium secondary battery includes, but is not limited to: a lithium metal secondary battery, a lithium ion secondary battery, a lithium polymer secondary battery or a lithium ion polymer secondary battery.

[0089] The preparation of lithium-ion batteries is described below by taking lithium-ion batteries as an example and combining specific embodiments. Those skilled in the art will understand that the preparation method described in this application is only an example, and any other suitable preparation method is within the scope of this application.

[0090] 1. Preparation of Binder

[0091] 1.5 parts of ammonium persulfate, 15 parts of deionized water, and 15 parts of acrylonitrile were fully stirred to obtain a solution A, and the solution A was stored at 2°C to 8°C until use.

[0092] Add 30 parts of lithium acrylate, 40 parts of acrylonitrile, 15 parts of glycidyl methacrylate and 235 parts of deionized water into a three-necked flask and stir evenly; heat the water bath to 70°C, continue to introduce argon into the three-necked flask to exhaust the air, and after the temperature in the three-necked flask rises to 70°C, add solution A dropwise at a rate of 0.125 ml / min, stir at a rate of 400 rpm and react for 6 hours to obtain a colorless transparent solution;

[0093] Finally, 15 parts of dopamine hydrochloride were added to the colorless transparent solution, and stirred at 100 rpm for 5 hours at 80° C. under inert gas protection to obtain a binder having a molecular weight of 1,000 to 5,000,000.

[0094] The binders of Examples 1 to 33 (i.e., S1 to S33 in the table) and Comparative Examples 1 to 3 (i.e., D1 to D3 in the table) prepared according to the above method have mixing parameters as shown in Table 1.

[0095] Table 1

[0096]

[0097]

[0098]

[0099]

[0100]

[0101] “ / ” in the table means not added.

[0102] 2. Power-off test:

[0103] The negative electrode active material, conductive carbon black and polymer were mixed with deionized water in a mass ratio of 80:10:10 to form a slurry, and then coated with a 100um thick coating using a scraper. After drying in a vacuum oven at 85°C for 12 hours, the coating was cut into 1cm diameter discs using a punch in a dry environment. In a glove box, a metal lithium sheet was used as the counter electrode, and a ceglard composite membrane was selected as the isolation membrane. The electrolyte was added to assemble the button cell. The battery was charged and discharged using the LAND series battery test to test its charge and discharge performance.

[0104] 3. Performance test of lithium-ion battery:

[0105] (1) Electrode adhesion test method:

[0106] The negative electrode active material, conductive carbon black and polymer were added with deionized water in a mass ratio of 80:10:10 and stirred into a slurry. A 50um thick coating was applied with a scraper and dried in a vacuum oven at 85°C for 12 hours. The strips were cut into 2cm×10cm strips, and the coated surface of the strips was aligned and bonded on a 2cm wide double-sided adhesive (3MVBH4920), and rolled back and forth 3 to 4 times with a 2kg roller. The strips were passed through a universal material testing machine, 180° uniaxial tensile mode, a clamp speed of 50mm / min, and the average tensile force was calculated after stretching 50mm.

[0107] (2) 0.1C charging capacity test method:

[0108] The button cell made as above was tested by the blue battery test system. The process is as follows: stand for 2 hours, 0.05C to 0.05V, stand for 1 hour, 100uA constant current to 0.05V, stand for 10 minutes, 0.5C constant current to 2V. Calculate the gram capacity.

[0109] (3) 50-cycle capacity retention rate test method:

[0110] The button cell made as above was tested by the blue power test system. The process is as follows: stand for 30 minutes, 0.05C to 2V, stand for 10 minutes, 0.05C discharge to 0.005V, and repeat the above process 3 times. Stand for 10 minutes, 0.2C to 2V, stand for 10 minutes, 0.2C to 0.005V, and after 50 cycles of this step, calculate the ratio of the final capacity to the initial capacity.

[0111] 4. Adhesive performance test:

[0112] (1) Test method for glass transition temperature of adhesive:

[0113] The adhesive solution was dried at 70°C for 24 hours to obtain an adhesive film, which was then tested. The test method was based on the national standard GB / T13464-2008. The test temperature range was -50 to 200°C, and the heating rate was 10°C / min.

[0114] (2) Test method for adhesive viscosity: The solid content of the prepared adhesive solution is 4%, and the adhesive solution is tested. The test method refers to the cone-plate type rotational viscometer in the national standard GB / T10247-2008, with a constant test temperature of 25°C and a constant shear rate of 0.11 / s.

[0115] The prepared Examples 1 to 33 (i.e., S1 to S33 in the table) and Comparative Examples 1 to 3 (i.e., D1 to D3 in the table) were subjected to performance tests, and the test results are shown in Table 2.

[0116] Table 2

[0117]

[0118]

[0119] According to the test data of Examples 1 to 6 in Table 1 and Table 2 above, when the molar ratio of the structural unit containing a cyano group shown in Formula III, the molar ratio of the structural unit containing an anionic group shown in Formula II, and the anionic group in Formula II in the binder remain unchanged, as the molar ratio of the structural unit shown in Formula I increases, that is, the proportion of phenolic hydroxyl groups increases, the viscosity of the binder first increases and then decreases.

[0120] like Figure 1a , Figure 1b and Figure 2 As shown, when the structural unit of formula I is not added to the binder of comparative example 1, the bonding force of the binder is low, the pole piece has the risk of demolding, and the 50-week cycle capacity retention rate is low. The cycle capacity retention rate of Example 3 is higher than that of comparative example 1.

[0121] According to the test data of Examples 7 to 10 and Example 3, when the molar ratio of the structural unit shown in Formula I in the binder, the molar ratio of the structural unit containing anionic groups shown in Formula II, and the anionic groups in Formula II remain unchanged, as the molar ratio of the structural unit shown in Formula III increases, that is, the cyano group ratio increases, the viscosity of the binder increases; however, when the molar ratio of the structural unit shown in Formula III is greater than 55mol%, the viscosity of the binder is too large and cannot be water-soluble, reducing its ease of use. Preferably, the molar ratio of the structural unit shown in Formula III in the binder is 40mol% to 55mol%, and further preferably, the molar ratio of the structural unit shown in Formula III in the binder is 50mol% to 55mol%.

[0122] Further combined with the test data of comparative example 2, it can be seen that when the structural unit of formula III is not added to the binder, the bonding force of the binder is low, the pole piece has the risk of demolding, and the 50-week cycle capacity retention rate is low. According to the test data of Examples 11 to 16 and Example 3, when the molar proportion of the structural unit shown in formula I, the molar proportion of the structural unit shown in formula III, and the anionic group in formula II in the binder remain unchanged, as the molar proportion of the structural unit shown in formula II increases, that is, the salted anionic groups in the binder increase, the binder can provide more lithium ions during the battery cycle, and can compete with the solvent around the lithium ions to help lithium ions desolvate, alleviate the obstruction of lithium ion embedding, and improve the kinetic performance of the electrochemical device. Preferably, the molar proportion of the structural unit shown in formula II in the binder is 15mol% to 45mol%, and further preferably, the molar proportion of the structural unit shown in formula II in the binder is 20mol% to 30mol%.

[0123] Further combined with the test data of Comparative Example 3, it can be seen that when the structural unit of Formula II is not added to the binder, the electrochemical device has poor kinetics and the specific capacity at high rate is low.

[0124] According to the test data of Examples 3, 17 to 18, when the anionic groups in Formula II in the binder are different, it has little effect on the viscosity of the binder and the battery capacity retention rate.

[0125] According to the test data of Examples 3, 19 to 21, as the binder content in the negative electrode plate increases, the bonding force of the plate increases, and the battery capacity retention rate increases.

[0126] According to the test data of Examples 3, 22 to 24, the negative electrode active materials in the negative electrode plates are different, but have little effect on the bonding strength of the plates. It can be seen that the binder is suitable for silicon-oxygen negative electrode materials, silicon-carbon negative electrode materials, silicon negative electrode materials or graphite negative electrode materials.

[0127] According to the test data of Examples 3, 25, and 26, different structural units of Formula I are added to the binder, namely, methacrylic acid modified catechol structure, acrylic acid modified catechol structure, and methacrylic acid modified benzylphenol structure. The structural units of Formula I with different structures have little effect on the electrode bonding force. Compared with Comparative Example 1, they can effectively improve the electrode bonding force and improve the battery capacity retention rate.

[0128] According to the test data of Examples 3, 27, 28, and 29, different structural units of Formula III are added to the binder, namely acrylonitrile, methacrylonitrile, 5-hexenenitrile, and allyl nitrile. The structural units of Formula III with different structures have little effect on the electrode bonding force. Compared with Comparative Example 2, they can effectively improve the electrode bonding force and increase the battery capacity retention rate.

[0129] According to the test data of Example 3 and Examples 30 to 32, different structural units of Formula II are added to the binder, namely lithium acrylate, lithium methacrylate, 2-acrylamide-2-methylpropane sulfonic acid, and p-styrene sulfonic acid. The structural units of Formula II with different structures have little effect on the electrode bonding force. Compared with Comparative Example 3, they can effectively improve the electrode bonding force and increase the battery capacity retention rate.

[0130] According to the test data of Example 3 and Example 33, different functional monomers are added to the adhesive, namely NN methylene bisacrylamide and polyethylene glycol diacrylate. Different functional monomers have little effect on the electrode bonding force, which can effectively improve the electrode bonding force and improve the battery capacity retention rate.

[0131] Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the claims. Any technical personnel in this field may make several possible changes and modifications without departing from the concept of the present application. Therefore, the scope of protection of the present application shall be based on the scope defined by the claims of the present application.

Claims

1. A binder, characterized in that: The binder is a polymer containing structural units shown in Formula I, Formula II and Formula III: Wherein, R1 is independently selected from any one of substituted or unsubstituted C1-C10 alkyl, substituted or unsubstituted C2-C10 alkenyl, substituted or unsubstituted C2-C10 alkynyl, substituted or unsubstituted C6-C20 aryl; R2 is selected from phenolic hydroxyl groups, and the number of the phenolic hydroxyl groups is 2 to 5; R3 is selected from any one of C, S, N, and P; X is selected from any one of Li, Na, and K; R4 and R5 are each independently selected from any one of a hydrogen atom, a substituted or unsubstituted C1-C10 alkyl group, a substituted or unsubstituted C2-C10 alkenyl group, a substituted or unsubstituted C2-C10 alkynyl group, and a substituted or unsubstituted C6-C20 aryl group; n1, n2, n3 are each independently an integer greater than zero; the oxygen quantity m is selected from 1, 2, 3 or 4; The molar proportion of the structural unit represented by formula I in the binder is 5 mol% to 30 mol%; The molar proportion of the structural unit represented by formula II in the binder is 10 mol% to 60 mol%; The molar proportion of the structural unit represented by formula III in the binder is 35 mol % to 55 mol %.

2. The adhesive according to claim 1, characterized in that R2 in the structural unit shown in Formula I is selected from any one of the following groups: in, Indicates the binding site with the neighboring atoms.

3. The adhesive according to claim 1, characterized in that The binder further includes a functional monomer with a mass percentage of 0wt% to 1wt%, and the functional monomer includes at least one of an acrylamide derivative monomer and an acrylic acid derivative monomer.

4. The adhesive according to claim 3, characterized in that The acrylamide derivative monomer includes at least one of acrylamide, N-methyl acrylamide, N-ethyl acrylamide, N-butyl acrylamide or N,N-methylenebisacrylamide.

5. The adhesive according to claim 3, characterized in that The acrylic acid derivative monomer includes at least one of methyl acrylate, ethyl acrylate, n-butyl acrylate, tert-butyl acrylate, 2-ethylhexyl acrylate, cyclohexyl acrylate, isobornyl acrylate, hydroxyethyl acrylate, hydroxypropyl acrylate, vinyl acetate, methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, 2-ethylhexyl methacrylate, cyclohexyl methacrylate, isobornyl methacrylate, hydroxyethyl methacrylate, hydroxypropyl methacrylate, glycidyl methacrylate or polyoxyethylene diacrylate.

6. The adhesive according to claim 1, characterized in that The pH value of the binder is 3 to 12.

7. The adhesive according to any one of claims 1 to 6, characterized in that: The binder satisfies at least one of the following characteristics a to c: a. The glass transition temperature of the binder is 80°C to 200°C; b. When the solid content of the binder is 4%, the viscosity of the binder is 1000mPa·s to 20000mPa·s; c. The molecular weight of the binder is between 1,000 and 5,000,000.

8. The adhesive according to claim 1, characterized in that The binder further includes a solvent, and the solvent is an organic solvent or water.

9. The adhesive according to claim 1, characterized in that The binder further comprises an additive, wherein the additive comprises at least one of a dispersant, a leveling agent, a wetting agent, a defoaming agent, and a softening agent.

10. The adhesive according to claim 1, characterized in that The binder is applied to the negative electrode and / or the positive electrode of a lithium ion battery.

11. An electrochemical device, comprising a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, characterized in that: At least one of the positive electrode sheet, the negative electrode sheet, and the separator contains the binder according to any one of claims 1 to 10.

12. The electrochemical device according to claim 11, characterized in that The negative electrode plate includes a negative electrode current collector and a negative electrode active material layer, and the binder accounts for 3.0 wt % to 6.0 wt % of the negative electrode active material layer.