Preparation method and application of passive vacuum maintenance alloy
By activating the adsorption capacity of elemental alloy materials such as Ti and Zr at low activation temperatures, a passive vacuum maintaining alloy film is prepared, which solves the problem of high vacuum maintenance in a passive vacuum environment and achieves high adsorption at room temperature and low pressure. Gas and carbon monoxide absorption performance, suitable for high vacuum applications under no power supply conditions.
Patent Information
- Application Number
- CN202111585980.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-17
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2041-12-17
AI Technical Summary
Existing technology is difficult to maintain a high vacuum environment under passive conditions, especially in space or aerospace applications. Traditional active vacuum pumps cannot be used, resulting in vacuum devices unable to achieve high vacuum performance.
A passive vacuum-maintaining alloy material is used to activate its adsorption capacity at low activation temperature. The alloy film is prepared using alloy formulas of Ti, Zr and other elements, combined with vacuum evaporation and physical vapor deposition processes, to achieve room temperature and low temperature. High air and carbon monoxide suction performance at ambient pressure.
It effectively maintains the vacuum environment of the device, reduces the suction balance pressure, and improves the passive vacuum maintenance capability. It is suitable for high vacuum applications under no power supply conditions.
Smart Images

Figure CN114231819B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a sensor device, and in particular to a preparation method of a passive vacuum maintaining alloy and application thereof. Background Art
[0002] Various chip devices and nuclear medicine, hydrogen atomic clocks, ion accelerators, etc. require a high vacuum environment. Some vacuum can be maintained by external vacuum, such as dry pumps, molecular pumps, ion pumps, etc. to maintain the vacuum of the device, but these pumps require a power system, and their application must be completed under power. For some portable vacuum devices or devices used in space or aerospace that are strongly related to vacuum, active vacuum cannot be achieved, and passive vacuum materials need to be relied on to maintain the high vacuum of the device. The preparation method of the passive vacuum maintenance alloy of the present invention and its application can absorb excess gas in the device and maintain the vacuum of the device. Summary of the invention
[0003] The purpose of the present invention is to propose a preparation method and application of a passive vacuum maintaining alloy. This alloy material can be activated at a relatively low activation temperature, has a high ability to absorb hydrogen and carbon monoxide at room temperature and low ambient pressure, and can maintain the vacuum environment of the device in a passive vacuum environment.
[0004] The object of the present invention is achieved by: a preparation method of a passive vacuum maintenance alloy and its application, the alloy formula of the material is as follows:
[0005]
[0006]
[0007] Wherein, the main element is one or two of Ti and Zr.
[0008] Preferably, the main elements of the alloy formula are 52wt%-63wt%, the Y is 5wt%-30wt%, the Mo is 18-22wt%, the W is 0.1wt%-5wt%, the Re is 0.1wt%-4wt%, the Hf is 0-1.8wt%, the Nb is 0-1.8wt%, and the Ni is 0.1wt%-1.8wt%.
[0009] Preferably, the alloy formula is:
[0010] (Ti x Zr y ) 50-64 Y 4-32 Mo 18-22 W 0.01-20 Re 0-20 Hf 0-2Nb 0-2 Ni 0-2 (wt%);
[0011] 0≤x≤1, 0≤y≤1, x+y=1.
[0012] Preferably, the alloy formula is:
[0013] (Ti x Zr y ) 52-63 Y 5-30 Mo 18-22 W 0.01-5 Re 0.1-4 Hf 0-1.8 Nb 0-1.8 Ni 0-1.8 (wt%);
[0014] 0≤x≤1, 0≤y≤1, x+y=1.
[0015] Preferably, the alloy formula is selected from:
[0016] Ti 60 Y 20 Mo 20 (wt%),
[0017] Ti 63 Y6 19 W8Re4 (wt%),
[0018] Ti 51 Y 10 Mo 18 W 14 Re5Hf1Nb1(wt%),
[0019] Zr 54 Y8 19 W 15 Re4Hf1Nb1(wt%)
[0020] Ti 50 Y 10 Mo 19 W 13 Re5Hf1Nb1Ni1(wt%),
[0021] Ti 34 Zr 33 Y8Mo5W4Re3Hf1Nb1Ni1) (wt%).
[0022] Preferably, the method for preparing the alloy target material of the passive vacuum maintenance alloy by vacuum evaporation method is as follows:
[0023] Raw materials with a purity of 99.5 to 99.95% are prepared according to the above alloy formula, wherein the raw materials are Ti, Zr, Y, Mo, W, Re, Hf, Nb and Ni respectively, and the ingredients are melted to obtain an alloy target blank of a passive vacuum maintaining alloy; or an alloy target blank is prepared by a powder metallurgy sintering method, and the alloy target blank is machined to obtain the 2-inch to 12-inch alloy target material.
[0024] Preferably, the getter film is prepared from the alloy target by a physical vapor deposition process.
[0025] Preferably, the method comprises the following steps:
[0026] Providing an alloy target material prepared by the above preparation method;
[0027] The alloy target is used as a cathode and deposited on an anode substrate by a vacuum evaporation process to obtain a passive vacuum-maintaining alloy film.
[0028] Preferably, the adhesion between the film and the substrate is 1-3.5 N / cm; and / or the thickness of the film is 1-10 μm; and / or the substrate is a wafer, a metal film, a ceramic film or an inorganic metal film.
[0029] Preferably, the getter film needs to be activated under vacuum conditions before getting air, and then tested; the test process is: evacuate the test cavity, and when the back vacuum of the cavity is higher than 3×10 -8 Pa, the sample was activated by external heating method, the activation temperature was 210℃~500℃, the activation time was 10min-4h, after the activation was completed, the sample was cooled to room temperature, and the gas absorption performance and carbon monoxide absorption performance were tested; the flow conductance during the test was 4~5×10 -4 Pa, when the hydrogen absorption performance of the sample was tested, the initial hydrogen absorption rate at room temperature was 20.7~58.6cm 3 / s.cm 2 After 2 hours, the total hydrogen absorption capacity at room temperature is 43~109Pa.cm 3 / cm 2 When the sample was tested for carbon monoxide absorption performance, the initial rate of carbon monoxide absorption at room temperature was 16-65.9 cm 3 / s.cm 2 After 2 hours, the total hydrogen absorption capacity at room temperature is 23-89Pa.cm 3 / cm 2 .
[0030] Compared with the prior art, the invention is beneficial in that the alloy prepared by the invention patent has a high specific surface area and a large porosity, which is due to the addition of W, Mo, Re, Nb elements with d electron orbits, such as Ti60 Y 20 Mo 20 (wt%), Ti 63 Y6 19 W8Re4、Ti 51 Y 10 Mo 18 W 14 Re5Hf1Nb1、Zr 54 Y8 19 W 15 Re4Hf1Nb1、Ti 50 Y 10 Mo 19 W 13 Re5Hf1Nb1Ni1、Ti 34 Zr 33 Y8Mo5W4Re3Hf1Nb1Ni1, which reduces the alloy's intake balance pressure, is beneficial to the alloy's intake performance, and can effectively maintain passivity. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is the hydrogen absorption performance curve of the alloy at room temperature at different activation temperatures for the samples of the present invention.
[0032] Figure 2 This is the carbon monoxide absorption performance curve of the alloy at room temperature under different activation temperatures of the samples of the present invention. DETAILED DESCRIPTION
[0033] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0034] Example 1
[0035] like Figure 1 Sample 1 in the curve is deposited on a 2-12 inch wafer using room temperature ultra-high vacuum electron beam co-evaporation method. 60 Y 20 Mo 20 (wt%) thin film, the specific method is: first use three evaporation tables to evaporate Ti, Y, and Mo. The first evaporation table is for Ti alloy, with a weight of 60g. The second evaporation table is for Y alloy, with a weight of 20g. The third evaporation table is for Mo, with a weight of 20g. First, vacuum is drawn. When the vacuum reaches 1.0×10 -6 Pa, three evaporation tables evaporated onto the substrate at the same time, and the substrate was a 2-inch diameter wafer. The evaporation rates of Ti, Y, and Mo were After 3 hours of vacuum enrichment, a film with a thickness of 2.1 microns was obtained. The air absorption performance was tested on a constant pressure test instrument, and the test method adopted the national standard GB / T 25497-2010. The test process is: evacuate the test chamber, and when the vacuum degree of the back of the chamber reaches 10 -8 Pa, the sample was activated by external heating method, and the activation process was 450℃×30min. After activation, the sample was cooled to room temperature and tested. The conductance during the test was 4×10 -4 Pa, the test results show that the initial hydrogen absorption rate of the sample at room temperature is 58.6 cm 3 / s.cm 2 After 2 hours, the total hydrogen absorption capacity at room temperature is 100 Pa.cm 3 / cm 2 .
[0036] Example 2
[0037] like Figure 2 Sample 2 in the curve is a mixture of various raw materials with a purity of 99.95%, and its composition ratio is Ti 63 Y6 19 The mixture was melted twice by vacuum electromagnetic induction, and the vacuum degree during melting was 2×10 -1 Pa to obtain an alloy target blank; the target blank is machined to obtain an alloy target with a size of 2 inches. The physical vapor deposition process used is a magnetron sputtering process. The parameters of the magnetron sputtering process are: the cavity sputtering pressure is 0.08Pa; the base substrate sample is a 2-inch wafer, and the base substrate sample temperature is 30°C; the sputtering power is 80W; the distance between the target material and the base substrate is 75mm. After sputtering for 1h, the final sputtered film thickness is 1 micron. The carbon monoxide gas absorption performance is tested on a constant pressure test instrument, and the test method adopts the national standard GB / T 25497-2010. The test process is: evacuate the test cavity, and when the back vacuum of the cavity reaches 10 -8 Pa, the sample was activated by external heating method, and the activation process was 250℃×2h. After the activation was completed, the sample was cooled to room temperature and tested for carbon monoxide. The conductance during the test was 4×10 -4 Pa, the test results show that the initial rate of carbon monoxide absorption by the sample at room temperature is 37.5cm 3 / s.cm 2 After 2 hours, the total capacity of carbon monoxide absorption at room temperature is 89.6Pa.cm 3 / cm 2 .
[0038] Example 3
[0039] like Figure 1 Sample 3 in the curve is a mixture of various raw materials with a purity of 99.95%, and its composition ratio is Ti 51 Y 10 Mo 18 W 14 The mixture was melted twice by vacuum electromagnetic induction, and the vacuum degree during melting was 1×10 -1 Pa to obtain an alloy target blank; the target blank is machined to obtain an alloy target material with a size of 8 inches. The physical vapor deposition process used is a magnetron sputtering process. The parameters of the magnetron sputtering process are: the cavity sputtering pressure is 1.2Pa; the base substrate sample is an 8-inch wafer, and the base substrate sample temperature is 60°C; the sputtering power is 130W; the distance between the target material and the base substrate is 45mm. After sputtering for 1.2h, the final sputtered film thickness is 1.3 microns. The air absorption performance is tested on a constant pressure test instrument, and the test method adopts the national standard GB / T 25497-2010. The test process is: evacuate the test cavity, and when the back vacuum of the cavity reaches 10 -8 Pa, the sample was activated by external heating method, and the activation process was 500℃×15min. After the activation was completed, the sample was cooled to room temperature and tested. The conductance during the test was 4×10 -4 Pa, the test results show that the initial hydrogen absorption rate of the sample at room temperature is 65.9 cm 3 / s.cm 2 After 2 hours, the total hydrogen absorption capacity at room temperature is 109.8 Pa.cm 3 / cm 2 .
[0040] Example 4
[0041] like Figure 2 Sample 4 in the curve is a mixture of various raw materials with a purity of 99.95%, and its composition ratio is Zr 54 Y8 19 W 15 The mixture was melted twice by vacuum electromagnetic induction, and the vacuum degree during melting was 2×10 -2Pa to obtain an alloy target blank; the target blank is machined to obtain an alloy target material with a size of 12 inches. The physical vapor deposition process used is a magnetron sputtering process. The parameters of the magnetron sputtering process are: the cavity sputtering pressure is 2.0Pa; the base substrate sample is a 12-inch wafer, and the base substrate sample temperature is 100°C; the sputtering power is 280W; the distance between the target material and the base substrate is 48mm. After sputtering for 1.8 hours, the final sputtered film thickness is 1.9 microns. The air absorption performance is tested on a constant pressure test instrument, and the test method adopts the national standard GB / T 25497-2010. The test process is: evacuate the test cavity, and when the back vacuum of the cavity reaches 10 -8 Pa, the sample was activated by external heating method, and the activation process was 250℃×1h. After the activation was completed, the sample was cooled to room temperature and the carbon monoxide test was performed. The conductance during the test was 4×10 -4 Pa, the test results show that the initial absorption rate of carbon monoxide by the sample at room temperature is 28.3cm 3 / s.cm 2 After 2 hours, the total carbon monoxide absorption capacity is 55Pa.cm 3 / cm 2 .
[0042] Example 5
[0043] like Figure 1 Sample 5 in the curve is a mixture of various raw materials with a purity of 99.95%, and its composition ratio is Ti 50 Y 10 Mo 19 W 13 The mixture is melted twice by vacuum electromagnetic induction, and the vacuum degree during melting is 1×10 -2 Pa to obtain an alloy target blank; the target blank is machined to obtain an alloy target material with a size of 4 inches. The physical vapor deposition process is a magnetron sputtering process. The parameters of the magnetron sputtering process are: the cavity sputtering pressure is 2.1Pa; the base substrate sample is a 12-inch wafer, and the base substrate sample temperature is 80°C; the sputtering power is 110W; the distance between the target material and the base substrate is 55mm. After sputtering for 2.0h, the final sputtered film thickness is 2 microns. The air absorption performance is tested on a constant pressure test instrument, and the test method adopts the national standard GB / T 25497-2010. The test process is: evacuate the test cavity, and when the back vacuum of the cavity reaches 10 -8 Pa, the sample was activated by external heating method, and the activation process was 210℃×4h. After activation, the sample was cooled to room temperature and tested. The conductance during the test was 4×10 -4 Pa, the test results show that the initial hydrogen absorption rate of the sample at room temperature is 20.7 cm3 / s.cm 2 After 2 hours, the total hydrogen absorption capacity at room temperature is 43 Pa.cm 3 / cm 2 .
[0044] Implementation 6
[0045] like Figure 2 Sample 6 in the curve is a mixture of various raw materials with a purity of 99.95%, and its composition ratio is Ti 34 Zr 33 The mixture was melted twice by vacuum electromagnetic induction, and the vacuum degree during melting was 2×10 -1 Pa to obtain an alloy target blank; the target blank is machined to obtain an alloy target with a size of 4 inches. The physical vapor deposition process is a magnetron sputtering process. The parameters of the magnetron sputtering process are: the cavity sputtering pressure is 0.9Pa; the base substrate sample is 0.05 stainless steel film, and the base substrate sample temperature is 100℃; the sputtering power is 150W; the distance between the target material and the base substrate is 60mm. After sputtering for 2.5h, the final sputtered film thickness is 2.2 microns. The air absorption performance is tested on a constant pressure test instrument, and the test method adopts the national standard GB / T 25497-2010. The test process is: evacuate the test cavity, and when the back vacuum of the cavity reaches 10 -8 Pa, the sample was activated by external heating method, and the activation process was 210℃×4h. After activation, the sample was cooled to room temperature and tested. The conductance during the test was 4×10 -4 Pa, the test results show that the initial rate of carbon monoxide absorption of the sample at room temperature is 16cm 3 / s.cm 2 After 2 hours, the total carbon monoxide absorption capacity at room temperature is 23Pa.cm 3 / cm 2 .
[0046] The above-described embodiments are merely descriptions of preferred implementations of the present invention, and are not intended to limit the concept and scope of the present invention. Without departing from the design concept of the present invention, various modifications and improvements made by ordinary persons in the art to the technical solution of the present invention should fall within the protection scope of the present invention, and the technical contents for which protection is sought in the present invention have been fully recorded in the claims.
Claims
1. A passive vacuum-maintaining alloy getter film, characterized in that: The formula of the passive vacuum-maintaining alloy getter film is: You 50 Y 10 In 19 W 13 Re5Hf1Nb1Ni1(wt %) The preparation method of the passive vacuum-maintaining alloy getter film is as follows: Mix the mixture with a purity of 99.95%, and mix the mixture according to the following proportions: You 50 Y 10 In 19 W 13 Re5Hf1Nb1Ni1(wt %) The mixture is melted twice by vacuum electromagnetic induction, and the vacuum degree during melting is 1×10 -2 Pa, to obtain an alloy target blank; the alloy target blank is machined to obtain an alloy target material with a size of 4 inches, and a passive vacuum-maintained alloy gettering film is obtained by magnetron sputtering process. The parameters of the magnetron sputtering process are: the cavity sputtering pressure is 2.1Pa; the base substrate sample is a 12-inch wafer, and the base substrate sample temperature is 80°C; the sputtering power is 110W; the distance between the alloy target and the base substrate is 55mm.
2. A passive vacuum-maintaining alloy getter film according to claim 1, characterized in that: The getter film needs to be activated under vacuum conditions before getting air, and then tested; the test process is: evacuate the test cavity, and when the vacuum degree of the back of the cavity is higher than 10 -8 Pa, the sample was activated by external heating method, the activation temperature was 210℃, the activation time was 4h, after the activation was completed, the sample was cooled to room temperature and tested; the conductance during the test was 4×10 -4 Pa, the initial hydrogen absorption rate is 20.7 ml / s·cm 2 , the total air intake capacity after 2 hours is 43Pa·cm 3 / cm 2 .
Citation Information
Patent Citations
Target preparation method and getter film forming method
CN106591790A
Air suction alloy and application thereof, air suction target material and air suction film
CN113136504A
High-performance film getter and application thereof
CN113621851A