Laminated glass for projection image display and image display system
By using a heat-sealing layer and a hybrid layer in laminated glass, the problems of wrinkles and insufficient sealing of semi-reflective films in laminated glass are solved, achieving high sealing and clear projection image display.
Patent Information
- Application Number
- CN202111608138.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-05-16
- Filing Date
- 2018-09-07
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2038-09-07
AI Technical Summary
When manufacturing wide-area laminated glass, the semi-reflective film is prone to wrinkles, which leads to a decrease in yield and affects the visibility of the projected image. At the same time, the seal is insufficient, and the problem is more pronounced when using curved glass.
A semi-reflective mirror film with a heat-sealing layer on a transparent support is used. By setting a specific heat-sealing layer in the laminated glass, the airtightness is improved, and a hybrid layer is formed between the transparent support and the heat-sealing layer to suppress wrinkles in the semi-reflective mirror film.
The improved sealing of the semi-reflective mirror film prevents wrinkles and ensures the high quality of the laminated glass and the clarity of the projected image.
Smart Images

Figure CN114236845B_ABST
Abstract
Description
[0001] This application is a divisional application of Chinese patent application No. 201880057540.X filed on March 5, 2020 (international application number is PCT / JP2018 / 033307, invention name: semi-reflective mirror film for projection image display, laminated glass for projection image display and image display system). Technical Field
[0002] The present invention relates to a half mirror film for projected image display, a laminated glass for projected image display, and an image display system using the laminated glass for projected image display. Background Art
[0003] By embedding a half-mirror film in a laminated glass used in a windshield of an automobile, the laminated glass can also be used as a projection image display component of a head-up display system. Patent Document 1 discloses that a half-mirror film including a phase difference layer and a plurality of cholesteric liquid crystal layers is used as a projection image display component. Patent Document 1 describes that a half-mirror film is provided on an intermediate film in a windshield having a laminated glass structure.
[0004] Generally, laminated glass has an interlayer film between two glass sheets.
[0005] Previous technical literature
[0006] Patent Literature
[0007] Patent Document 1: International Publication No. 2016 / 052367 Summary of the invention
[0008] Technical issues to be solved by the invention
[0009] The inventors of the present invention have conducted research and found that when manufacturing a wide laminated glass such as a windshield of an automobile, wrinkles are easily generated in the half mirror film if an intermediate film and a half mirror film are laminated at the same time. The generation of wrinkles is particularly noticeable when using a glass plate with a curved surface.
[0010] If a wrinkle occurs at one point, the laminated glass including the glass sheet will become a defective product, so this is a problem that directly affects the yield rate. In addition, there is a problem that fine wrinkles will cause optical distortion and adversely affect the visibility of the projected image.
[0011] Furthermore, in a half mirror film formed by laminating a plurality of layers, there may be a problem of low adhesion.
[0012] The object of the present invention is to provide a laminated half-mirror film for projection image display with high adhesion, a laminated glass for projection image display using the half-mirror film, a laminated glass for projection image display with high adhesion, a laminated glass for projection image display that suppresses the generation of wrinkles in the half-mirror film, and an image display system using the laminated glass.
[0013] Organization for solving technical problems
[0014] The inventors of the present invention have conducted in-depth research and found that, by providing a semi-mirror film with a heat-sealing layer on a transparent support, the adhesion of the semi-mirror film can be improved, and by providing a specific heat-sealing layer on a laminated glass using the semi-mirror film, it is possible to obtain a laminated glass that suppresses the formation of wrinkles in the semi-mirror film or has higher adhesion.
[0015] [1] A half mirror film for projected image display, comprising a transparent support and a selective reflection layer that reflects light in a wavelength-selective manner, wherein:
[0016] The absolute value of the in-plane phase difference of the transparent support at a wavelength of 550 nm is 10 nm or less.
[0017] The transparent support has a heat seal layer on the opposite side of the surface having the selective reflection layer, the heat seal layer contains a thermoplastic resin, and
[0018] A mixed layer in which a component of the transparent support and a component of the heat seal layer are mixed is formed between the transparent support and the heat seal layer.
[0019] [2] The half mirror film for projected image display according to [1], wherein a phase difference layer is provided between the transparent support and the selective reflection layer, and the in-plane phase difference of the phase difference layer at a wavelength of 550 nm is 250 to 450 nm or 50 to 180 nm.
[0020] [3] The half mirror film for projected image display according to [1] or [2], wherein the surface of the heat seal layer is roughened.
[0021] [4] A semi-reflective mirror film for projected image display according to any one of [1] to [3], wherein at least one of the transparent support and the heat seal layer contains a component derived from a compound having a plurality of groups selected from the group consisting of a polymerizable group and a group capable of forming a bond with a resin contained in the transparent support.
[0022] [5] A laminated glass for projected image display, wherein the half mirror film for projected image display according to any one of [1] to [4] and an intermediate film adjacent to the selective reflection layer of the half mirror film for projected image display are sandwiched between two glass plates.
[0023] [6] A laminated glass for projected image display, wherein a half mirror film and an intermediate film are sandwiched between a glass plate on the half mirror film side and a glass plate on the intermediate film side,
[0024] A heat seal layer containing a thermoplastic resin and having a thickness of 0.1 to 50 μm is provided between the half mirror film and the glass plate on the half mirror side.
[0025] [7] The laminated glass for projected image display according to [6], wherein the half mirror film has a selective reflection layer and a phase difference layer for reflecting light in a selective wavelength manner, and the heat seal layer is adjacent to the selective reflection layer or the phase difference layer.
[0026] [8] The laminated glass for projected image display according to [7], wherein the heat seal layer is adjacent to the selective reflection layer.
[0027] [9] The laminated glass for projected image display according to any one of [6] to [8], wherein the heat seal layer contains inorganic particles forming secondary particles, and the secondary particles are formed by aggregation of primary particles having an average primary particle diameter of 5 to 50 nm.
[0028]
[10] An image display system, wherein an image is projected from a p-linearly polarized light source onto the laminated glass for image display described in any one of [5] to [9].
[0029] Effects of the Invention
[0030] According to the present invention, it is possible to provide a half mirror film for projected image display with high adhesion, a laminated glass for projected image display with suppressed wrinkles of the half mirror film or with higher adhesion, and an image display system using the laminated glass. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is a diagram conceptually showing an example of the half mirror film for projected image display of the present invention.
[0032] Figure 2 This is a diagram conceptually showing an example of the first embodiment of the laminated glass for projected image display of the present invention.
[0033] Figure 3 This is a diagram conceptually showing an example of the second embodiment of the laminated glass for projected image display of the present invention.
[0034] Figure 4 This is a diagram conceptually showing another example of the second embodiment of the laminated glass for projected image display of the present invention.
[0035] Figure 5This is a diagram conceptually showing another example of the second embodiment of the laminated glass for projected image display of the present invention.
[0036] Figure 6 This is a diagram conceptually showing another example of the second embodiment of the laminated glass for projected image display of the present invention.
[0037] Figure 7 It conceptually represents projection Figure 2 The diagram shown is a diagram of how a projection image is viewed when an image is displayed using laminated glass. DETAILED DESCRIPTION
[0038] Hereinafter, the present invention will be described in detail.
[0039] In this specification, "to" is used to mean that the numerical values described before and after it are inclusive as the lower limit and the upper limit.
[0040] Furthermore, in this specification, angles (e.g., angles of 90°) and their relationships (e.g., parallel, horizontal, vertical, etc.) include the permissible error range in the technical field to which the present invention belongs. For example, it refers to the range of ±10° less than the exact angle, and the error between the exact angle and the angle is preferably 5° or less, and more preferably 3° or less.
[0041] In this specification, when "selectivity" is mentioned for circularly polarized light, it means that the amount of light of either the right circularly polarized light component or the left circularly polarized light component of the light is greater than the amount of light of the other circularly polarized light component. Specifically, when "selectivity" is mentioned, the circular polarization intensity of the light is preferably 0.3 or more, more preferably 0.6 or more, and even more preferably 0.8 or more. In fact, it is even more preferably 1.0. Here, the circular polarization intensity refers to the intensity of the right circularly polarized light component of the light when the intensity is set to I R , set the intensity of the left circularly polarized light component to I L Time use |I R -I L | / (I R +I L ) represents the value.
[0042] In this specification, when the "sense" of circularly polarized light is mentioned, it means right circularly polarized light or left circularly polarized light. Regarding the sense of circularly polarized light, when the light is viewed in a direction toward the near front, the case where the front end of the electric field vector rotates clockwise with time is defined as right circularly polarized light, and the case where it rotates counterclockwise is defined as left circularly polarized light.
[0043] In this specification, the term "handedness" is sometimes used to refer to the twisting direction of the helix of cholesteric liquid crystal. When the twisting direction (handedness) of the helix of cholesteric liquid crystal is right, right circularly polarized light is reflected and left circularly polarized light is transmitted, and when the handedness is left, left circularly polarized light is reflected and right circularly polarized light is transmitted.
[0044] In this specification, "light" refers to visible light and natural light (non-polarized light) unless otherwise specified. Visible light is electromagnetic light with wavelengths observable to the human eye, and generally refers to light in the wavelength range of 380 to 780 nm.
[0045] In this specification, when simply expressed as "reflected light" or "transmitted light", it is used to mean including scattered light and diffracted light.
[0046] In addition, the polarization state of each wavelength of light can be measured using a spectroradiometer or a spectrometer equipped with a circular polarizer. In this case, the intensity of light measured by the right circular polarizer is equivalent to I R The intensity of light measured by the left circular polarizer is equivalent to I L Furthermore, even if the circular polarizing plate is attached to a photometer or a spectrometer, measurement can be performed. By attaching a right circularly polarized light transmission plate to measure the right circularly polarized light amount, and attaching a left circularly polarized light transmission plate to measure the left circularly polarized light amount, the ratio can be measured.
[0047] In this specification, p-polarized light refers to polarized light that vibrates in a direction parallel to the incident plane of the light. The incident plane is a plane perpendicular to the reflection plane (windshield surface, etc.) and contains the incident light and the reflected light. The vibration plane of the electric field vector of p-polarized light is parallel to the incident plane.
[0048] In this specification, the in-plane phase difference (in-plane phase difference Re) is a value measured by AxoScan manufactured by Axometrics Inc. Unless otherwise specified, the measurement wavelength is 550 nm.
[0049] In this specification, "projection image" does not refer to the surrounding scenery such as the front, but refers to the image projected by the light from the projector used. From the observer's perspective, the projection image is observed as a virtual image that appears at the front end of the projection image display part of the windshield.
[0050] In this specification, "screen image" refers to an image displayed on a rendering device of a projector or an image rendered on an intermediate image screen by a rendering device. A screen image is a real image as opposed to a virtual image.
[0051] Both the image and the projected image may be a monochrome image, a multi-color image of two or more colors, or a full-color image.
[0052] In this specification, "visible light transmittance" is defined as the visible light transmittance of light source A specified in JIS R3212:2015 (Test methods for automotive safety glass). That is, it is the transmittance obtained by measuring the transmittance of each wavelength in the range of 380 to 780 nm using a spectrophotometer using light source A, and multiplying the transmittance at each wavelength by a weighted coefficient obtained from the wavelength distribution and wavelength interval of the illumination adaptation standard of CIE (International Commission on Illumination) to perform a weighted average.
[0053] Furthermore, in this specification, the concepts of liquid crystal composition and liquid crystal compound also include compositions and compounds that no longer show liquid crystal properties due to curing or the like.
[0054] Hereinafter, the half mirror film for projected image display, the laminated glass for projected image display, and the image display system of the present invention will be described with reference to the accompanying drawings. Figure 1 to Figure 7 In the drawings, the same components are denoted by the same symbols.
[0055] Figure 1 1 and 2 conceptually show an example of the half mirror film for projected image display of the present invention.
[0056] like Figure 1 As shown, the half mirror film for projected image display of the present invention comprises a heat seal layer 4, a transparent support 1, a phase difference layer 2 and a selective reflection layer 3 from the bottom of the figure.
[0057] In the half mirror film for projected image display of the present invention, the heat seal layer 4 is provided on the surface of the transparent support 1 on the opposite side to the selective reflection layer 3. Moreover, a mixed layer M in which the components of the transparent support 1 and the components of the heat seal layer 4 are mixed is formed between the transparent support 1 and the heat seal layer 4. As will be shown in the examples later, the half mirror film for projected image display of the present invention and the first embodiment of the laminated glass of the present invention described later achieve high adhesion between the transparent support 1 and the heat seal layer 4 by having the mixed layer.
[0058] In the half mirror film for projected image display of the present invention, the phase difference layer 2 is a layer provided as a preferred embodiment, and is provided between the transparent support 1 and the selective reflection layer 3 .
[0059] Figure 2 An example of the first embodiment of the laminated glass for projected image display of the present invention is conceptually shown in FIG. In the following description, the "laminated glass for projected image display" is also simply referred to as "laminated glass".
[0060] In a first aspect of the laminated glass of the present invention, the above-mentioned half mirror film for projected image display of the present invention and an intermediate film adjacent to the selective reflection layer of the half mirror film for projected image display are sandwiched between two glass plates.
[0061] Figure 2 The laminated glass shown in the figure has a first glass 6, a heat seal layer 4, a transparent support 1, a phase difference layer 2, a selective reflection layer 3, an intermediate film 5 and a second glass 7 from the bottom of the figure. As described above, the half mirror film for projected image display of the present invention is composed of a heat seal layer 4, a transparent support 1, a phase difference layer 2 and a selective reflection layer 3, and a mixed layer M is formed between the heat seal layer 4 and the transparent support 1.
[0062] With the first aspect of the laminated glass of the present invention, by having such a structure, a laminated glass is realized in which the adhesion of the half mirror film for projected image display is high and the generation of wrinkles of the half mirror film for projected image display is suppressed.
[0063] Figure 3 An example of the second embodiment of the laminated glass of the present invention is conceptually shown in FIG.
[0064] In the second embodiment of the laminated glass of the present invention, the half mirror film and the intermediate film are sandwiched by a glass plate on the half mirror film side and a glass plate on the intermediate film side, and a heat seal layer containing a thermoplastic resin and having a thickness of 0.1 to 50 μm is provided between the half mirror film and the glass plate on the half mirror film side. The second embodiment of the laminated glass of the present invention prevents wrinkles of the half mirror film in the laminated glass for projected image display using the half mirror film by providing such a heat seal layer.
[0065] Figure 3 The laminated glass shown in the figure has a first glass 6, an intermediate film 5, a transparent support 1, a phase difference layer 2, a selective reflection layer 3, a heat sealing layer 4 and a second glass 7 from the bottom. In this example, as a preferred embodiment, the transparent support 1, the phase difference layer 2 and the selective reflection layer 3 constitute a half mirror film 10.
[0066] Figure 4 Another example of the second embodiment of the laminated glass of the present invention is shown in FIG. Figure 4 The laminated glass shown in the figure has, from the bottom, a first glass 6, a heat seal layer 4, a phase difference layer 2, a selective reflection layer 3, a transparent support 1, an intermediate film 5 and a second glass 7. In this example, as a preferred embodiment, the phase difference layer 2, the selective reflection layer 3 and the transparent support 1 also constitute a half mirror film 10.
[0067] Figure 3 and Figure 4 In the laminated glass shown, as a preferred embodiment, the heat sealing layer 4 is adjacent to the phase difference layer 2 or the selective reflection layer 3. Figure 3In the laminated glass shown, as a more preferred embodiment, the heat sealing layer 4 is adjacent to the selective reflection layer 3 .
[0068] Figure 5 Another example of the second embodiment of the laminated glass of the present invention is shown in FIG. Figure 5 The laminated glass shown in the figure has a first glass 6, an intermediate film 5, a phase difference layer 2, a selective reflection layer 3, a transparent support 1, a heat seal layer 4 and a second glass 7 from the bottom. In this example, as a preferred embodiment, a half mirror film 10 is also formed by the phase difference layer 2, the selective reflection layer 3 and the transparent support 1. In addition, a mixed layer M is formed between the heat seal layer 4 and the transparent support 1.
[0069] In the second embodiment of the laminated glass of the present invention, when the transparent support 1 is adjacent to the heat seal layer 4, Figure 5 As shown, a mixed layer M in which components of the transparent support 1 and components of the heat seal layer 4 are mixed may be provided between the transparent support 1 and the heat seal layer 4 .
[0070] However, the second embodiment of the laminated glass of the present invention is not limited thereto, and even when the transparent support 1 is adjacent to the heat seal layer 4, it is not necessary to have the mixed layer M. Furthermore, when the transparent support 1 is adjacent to the heat seal layer 4 and does not have the mixed layer M, the heat seal layer 4 may be provided with a close adhesion enhancer described later.
[0071] Furthermore, in the laminated glass of the present invention, in both the first aspect and the second aspect, it is preferred that the heat seal layer 4 is in contact with either the first glass 6 or the second glass 7 .
[0072] Figure 3 to Figure 5 In the second embodiment of the laminated glass of the present invention shown above, each of them has the transparent support 1 , but the laminated glass of the second embodiment of the present invention is not limited thereto. That is, the second embodiment of the laminated glass of the present invention may not have the transparent support 1 .
[0073] For example, if Figure 3 The laminated glass shown in Figure 6 , the structure may be as follows: the transparent support 1 is not provided, but the first glass 6, the intermediate film 5, the phase difference layer 2, the selective reflection layer 3, the heat sealing layer 4 and the second glass 7 are provided from the bottom of the figure.
[0074] And, if Figure 5 The laminated glass shown may have the following structure: it does not have the transparent support 1, but has the first glass 6, the intermediate film 5, the phase difference layer 2, the selective reflection layer 3, the heat sealing layer 4 and the second glass 7 from the bottom of the figure.
[0075] That is, in the second embodiment of the laminated glass of the present invention, if the half mirror film 10 and the intermediate film 5 are sandwiched by the first glass plate 6 and the second glass plate 7, and a heat seal layer 4 with a thickness of 0.1 to 50 μm is provided between the half mirror film 10 and any of the glass plates, various layer structures can be used.
[0076] Hereinafter, the half mirror film for projected image display and the laminated glass of the present invention having such a layer structure and each layer constituting the half mirror film for projected image display and the laminated glass of the present invention will be described in more detail.
[0077] 《Half mirror film for projected image display》
[0078] In this specification, the half mirror film for projected image display refers to a half mirror film that can display a projected image using reflected light.
[0079] The half mirror film for projected image display of the present invention is visible light transmissive. Specifically, the visible light transmittance of the half mirror film for projected image display of the present invention is preferably 85% or more, more preferably 86% or more, and even more preferably 87% or more.
[0080] By having such a high visible light transmittance, even when the laminated glass is combined with glass having a low visible light transmittance, the visible light transmittance that satisfies the standards of a vehicle windshield can be achieved.
[0081] The half-mirror film for projected image display of the present invention preferably does not show actual reflection in the wavelength region with high luminous efficiency. Specifically, when comparing the usual laminated glass and the laminated glass assembled with the half-mirror film for projected image display of the present invention with respect to the light from the normal direction, it is preferred to show practically equivalent reflection near the wavelength of 550nm. In particular, it is more preferred to show practically equivalent reflection in the visible light wavelength region of 490 to 620nm. "Practically equivalent reflection" means that the difference in reflectivity of natural light (unpolarized light) in the target wavelength measured from the normal direction by a spectrophotometer such as the spectrophotometer "V-670" manufactured by JASCO Corporation is 10% or less. In the above-mentioned wavelength region, the difference in reflectivity is preferably 5% or less, more preferably 3% or less, further preferably 2% or less, and particularly preferably 1% or less. By showing practically equivalent reflection in the wavelength region with high luminous efficiency, when it is combined with glass with low visible light transmittance to be laminated glass, it is also possible to achieve a visible light transmittance that meets the standard of vehicle windshield.
[0082] The half mirror film for projected image display of the present invention may be in the form of a thin film, a sheet, or the like.
[0083] The half mirror film for projected image display of the present invention may be formed into a roll shape as a thin film before being used on a windshield.
[0084] The half mirror film for projected image display of the present invention only needs to function as a half mirror for at least a portion of the projected light, for example, it does not need to function as a half mirror for the entire visible light region. Furthermore, the half mirror film for projected image display of the present invention may function as the above-mentioned half mirror for light of all incident angles, but it only needs to function as the above-mentioned half mirror for light of at least a portion of the incident angles.
[0085] As described above, the half mirror film for projected image display of the present invention includes a transparent support, a selective reflection layer, and a heat seal layer.
[0086] In the first aspect of the laminated glass (for projected image display) of the present invention, the half mirror film for projected image display and the intermediate film of the present invention are sandwiched between two glass plates, and the intermediate film is adjacent to the selective reflection layer.
[0087] Furthermore, in the second aspect of the laminated glass (for projected image display) of the present invention, the half mirror film and the intermediate film are sandwiched between two glass plates, and a heat seal layer is provided between the half mirror film and the glass plates.
[0088] Furthermore, the half mirror film for projected image display and the laminated glass of the present invention may further include layers such as a phase difference layer, an orientation layer, and an adhesive layer in addition to these components as necessary.
[0089] <Select Reflection Layer>
[0090] The selective reflection layer is a layer that reflects light in a wavelength-selective manner. The selective reflection layer preferably shows selective reflection in a part of the visible light wavelength region. The selective reflection layer may just reflect light for projecting an image.
[0091] In the present invention, the center wavelength of selective reflection of the selective reflection layer having a center wavelength of selective reflection at the shortest wavelength is preferably 650 to 780 nm. In this specification, the center wavelength λ of selective reflection of the selective reflection layer represents the wavelength located at the center of gravity of the reflection peak of the reflection spectrum measured from the normal direction of the selective reflection layer. Such a structure can be realized, for example, by a structure in which the half mirror for projected image display includes a selective reflection layer having a center wavelength of selective reflection of 650 to 780 nm and does not include a selective reflection layer having a center wavelength of selective reflection in the visible light wavelength region of less than 650 nm.
[0092] In the present invention, the central wavelength of selective reflection of the selective reflection layer having a central wavelength of selective reflection at the shortest wavelength is preferably 750 nm or less, more preferably 720 nm or less, and further preferably 700 nm or less.
[0093] The half mirror film for projected image display and the laminated glass of the present invention may include two or more selective reflection layers.
[0094] The central wavelengths of the selective reflection of more than two selective reflection layers may be the same or different, but are preferably different. By including more than two selective reflection layers with different central wavelengths of the selective reflection, ghosting can be reduced. For example, when two selective reflection layers are included, the central wavelengths of the selective reflection of the two layers preferably differ by more than 60 nm, more preferably by more than 80 nm, and further preferably by more than 100 nm. The central wavelengths of the selective reflection of more than two selective reflection layers may all be between 650 and 780 nm, or at least one of them may be between 650 and 780 nm and the other may be at a wavelength exceeding 780 nm, but are preferably both between 650 and 780 nm.
[0095] The selective reflection layer is preferably a polarized light reflection layer. The polarized light reflection layer is a layer that reflects linearly polarized light, circularly polarized light, or elliptically polarized light.
[0096] The polarized light reflecting layer is preferably a circularly polarized light reflecting layer or a linearly polarized light reflecting layer. The circularly polarized light reflecting layer is a layer that reflects circularly polarized light of any one hand in the wavelength region of selective reflection and transmits circularly polarized light of another hand. Furthermore, the linearly polarized light reflecting layer is a layer that reflects linearly polarized light of one polarization direction in the wavelength region of selective reflection and transmits linearly polarized light of a polarization direction orthogonal to the reflected polarization direction.
[0097] The polarized light reflecting layer can transmit polarized light that is not reflected, and can also transmit a portion of light in the wavelength region where the selective reflection layer reflects. Therefore, the color tone of light that has passed through the half mirror for projected image display is not easily degraded, and the visible light transmittance is not easily reduced, so it is preferred.
[0098] As the circularly polarized light reflecting layer, that is, the selective reflecting layer, a cholesteric liquid crystal layer is preferable.
[0099] [Cholesteric Liquid Crystal Layer]
[0100] In this specification, the cholesteric liquid crystal layer refers to a layer in which a cholesteric liquid crystal phase is fixed.
[0101] The cholesteric liquid crystal layer is a layer that maintains the orientation of the liquid crystal compound that has become the cholesteric liquid crystal phase. A representative layer is as follows: after the polymerizable liquid crystal compound is set to the orientation state of the cholesteric liquid crystal phase, it is polymerized and cured by ultraviolet irradiation, heating, etc., thereby forming a layer without fluidity, and at the same time, it becomes a state in which the orientation morphology will not change due to external fields and external forces.
[0102] In addition, in the cholesteric liquid crystal layer, it is sufficient as long as the optical properties of the cholesteric liquid crystal phase are maintained in the layer, and the liquid crystal compound in the layer no longer needs to exhibit liquid crystal properties. For example, the polymerizable liquid crystal compound can be made high molecular weight by a curing reaction, thereby no longer having liquid crystal properties.
[0103] It is known that a cholesteric liquid crystal layer exhibits circularly polarized light selective reflection, which selectively reflects circularly polarized light of one of right-handed circularly polarized light and left-handed circularly polarized light and transmits circularly polarized light of the other direction.
[0104] As a film including a layer in which a cholesteric liquid crystal phase showing circularly polarized light selective reflectivity is fixed, various films formed from a composition including a polymerizable liquid crystal compound have been known in the past, and reference can be made to these prior arts regarding the cholesteric liquid crystal layer.
[0105] The selective reflection center wavelength λ of the cholesteric liquid crystal layer depends on the pitch P (= period of the spiral) of the spiral structure in the cholesteric phase, and follows the relationship between the average refractive index n of the cholesteric liquid crystal layer and λ=n×P. From this formula, it can be seen that by adjusting the n value and the P value, the central wavelength of the selective reflection can be adjusted to 650-780nm.
[0106] The selective reflection central wavelength and half-value width of the cholesteric liquid crystal layer can be obtained as follows.
[0107] When the transmission spectrum of the cholesteric liquid crystal layer is measured using a spectrophotometer UV3150 (SHIMADZU CORPORATION) (measured from the normal direction of the cholesteric liquid crystal layer), a peak of transmittance decrease can be observed in the selective reflection band. Of the two wavelengths of transmittance that are intermediate (average) between the minimum transmittance of the peak and the transmittance before the decrease, if the value of the wavelength on the short wavelength side is λ1 (nm) and the value of the wavelength on the long wavelength side is λ h (nm), the central wavelength λ and half-value width Δλ of the selective reflection can be expressed by the following formulas.
[0108] λ=(λ l +λ h ) / 2Δλ=(λ h -λ l )
[0109] The selective reflection center wavelength determined as described above substantially coincides with the wavelength located at the center of gravity of the reflection peak of the circularly polarized light reflection spectrum measured in the normal direction of the cholesteric liquid crystal layer.
[0110] As described later, in a head-up display system, by using light that is incident at an angle relative to the windshield, the reflectivity in the glass plate surface on the projection light incident side can be lowered. At this time, the light is also incident at an angle relative to the cholesteric liquid crystal layer. For example, light incident at an angle of 45° to 70° relative to the normal to the projection image display portion in air with a refractive index of 1 transmits a cholesteric liquid crystal layer with a refractive index of about 1.61 at an angle of about 26° to 36°. In this case, the reflected wavelength is shifted to the short wavelength side. In a cholesteric liquid crystal layer whose central wavelength of selective reflection is λ, the central wavelength of selective reflection when the light is transmitted at an angle of θ2 relative to the normal direction of the cholesteric liquid crystal layer (the helical axis direction of the cholesteric liquid crystal layer) is set to λ d When d It is expressed by the following formula.
[0111] λ d =λ×cosθ2
[0112] Therefore, the cholesteric liquid crystal layer having a central wavelength of selective reflection in the range of 650 to 780 nm when θ2 is 26° to 36° can reflect projection light in the range of 520 to 695 nm.
[0113] This wavelength range is a wavelength region with a high luminous efficiency and therefore has a high contribution to the brightness of the projected image. As a result, a high-brightness projected image can be achieved.
[0114] Since the pitch of the cholesteric liquid crystal phase depends on the type of chiral reagent used together with the polymerizable liquid crystal compound or its added concentration, the desired pitch can be obtained by adjusting these. In addition, the method for measuring the handedness and pitch of the spiral can be adopted in "Introduction to Liquid Crystal Chemistry Experiments" (edited by the Liquid Crystal Society of Japan, published by Sigma, published in 2007, 46 pages) and "Liquid Crystal Handbook" (Liquid Crystal Handbook Editorial Committee, Maruzen, 196 pages).
[0115] Furthermore, in the half mirror film and laminated glass for projected image display of the present invention, the cholesteric liquid crystal layers are preferably arranged in order from the layer having the shortest center wavelength of selective reflection when viewed from the viewing side (interior side).
[0116] As each cholesteric liquid crystal layer, a cholesteric liquid crystal layer whose handedness of the spiral is either right or left is used. The handedness of the reflected circularly polarized light of the cholesteric liquid crystal layer is consistent with the handedness of the spiral. The handedness of the spirals of the cholesteric liquid crystal layers with different central wavelengths for selective reflection may be the same, or may include different handednesses, but are preferably the same.
[0117] Furthermore, in the half mirror film and laminated glass for projected image display of the present invention, as the cholesteric liquid crystal layer showing selective reflection in the same or repeated wavelength region, it is preferred that the cholesteric liquid crystal layer not include a cholesteric liquid crystal layer of different helical handedness. This is to prevent the transmittance in a specific wavelength region from being reduced to, for example, less than 50%.
[0118] As for the half-value width Δλ (nm) of the selective reflection band showing the selective reflection, Δλ depends on the birefringence Δn of the liquid crystal compound and the above-mentioned pitch P, and follows the relationship of Δλ=Δn×P. Therefore, the width of the selective reflection band can be controlled by adjusting Δn. The adjustment of Δn can be performed by adjusting the type of polymerizable liquid crystal compound and its mixing ratio, or controlling the temperature when the alignment is fixed.
[0119] In order to form a cholesteric liquid crystal layer with the same central wavelength of selective reflection, a plurality of cholesteric liquid crystal layers with the same pitch P and the same handedness of the helix can be stacked. By stacking cholesteric liquid crystal layers with the same pitch P and the same handedness of the helix, the selectivity of circularly polarized light can be improved at a specific wavelength.
[0120] When stacking multiple cholesteric liquid crystal layers, you can either stack separately made cholesteric liquid crystal layers using an adhesive or the like, or directly apply a liquid crystal composition containing a polymerizable liquid crystal compound or the like on the surface of a previous cholesteric liquid crystal layer formed using the method described later, and repeat the alignment and fixing steps, but the latter is preferred.
[0121] This is because, by directly forming the next cholesteric liquid crystal layer on the surface of the previously formed cholesteric liquid crystal layer, the orientation of the liquid crystal molecules on the air interface side of the previously formed cholesteric liquid crystal layer is consistent with the orientation of the liquid crystal molecules on the lower side of the cholesteric liquid crystal layer formed thereon, and the polarization characteristics of the stacked body of the cholesteric liquid crystal layer become good. In addition, the interference unevenness that may be caused by the uneven thickness of the adhesive layer is not observed.
[0122] The thickness of the cholesteric liquid crystal layer is preferably 0.5 to 10 μm, more preferably 1.0 to 8.0 μm, and further preferably 1.5 to 6.0 μm. Furthermore, the total thickness of the cholesteric liquid crystal layer in the projection image display half mirror is preferably 2.0 to 30 μm, more preferably 2.5 to 25 μm, and further preferably 3.0 to 20 μm.
[0123] In the present invention, by setting the thickness of the cholesteric liquid crystal layer to the above range, the visible light transmittance can be maintained high without reducing the thickness of the cholesteric liquid crystal layer.
[0124] (Method for producing a cholesteric liquid crystal layer)
[0125] Hereinafter, the materials and the method for producing the cholesteric liquid crystal layer will be described.
[0126] As materials for forming the above-mentioned cholesteric liquid crystal layer, there can be cited liquid crystal compositions containing polymerizable liquid crystal compounds and chiral agents (optically active compounds), etc. As needed, the above-mentioned liquid crystal composition further mixed with a surfactant and a polymerization initiator, etc. and dissolved in a solvent, etc., is applied to a support, an alignment layer, a cholesteric liquid crystal layer that becomes a bottom layer, etc., and after the cholesteric alignment is matured, it is fixed by curing the liquid crystal composition, thereby forming a cholesteric liquid crystal layer.
[0127] (Polymerizable Liquid Crystal Compound)
[0128] The polymerizable liquid crystal compound may be a rod-like liquid crystal compound or a disc-like liquid crystal compound, but is preferably a rod-like liquid crystal compound.
[0129] As examples of rod-shaped polymerizable liquid crystal compounds forming a cholesteric liquid crystal layer, rod-shaped nematic liquid crystal compounds can be cited. As rod-shaped nematic liquid crystal compounds, preferably used are azomethines, azoxyls, cyanobiphenyls, cyanophenyl esters, benzoates, cyclohexanecarboxylic acid phenyl esters, cyanophenylcyclohexanes, cyano-substituted phenylpyrimidines, alkoxy-substituted phenylpyrimidines, phenyldioxanes, tolans, and cyclohexenylbenzonitrile. Not only low molecular weight liquid crystal compounds but also high molecular weight liquid crystal compounds can be used.
[0130] The polymerizable liquid crystal compound is obtained by introducing a polymerizable group into a liquid crystal compound. Examples of polymerizable groups include unsaturated polymerizable groups, epoxy groups, and aziridine groups, preferably unsaturated polymerizable groups, and particularly preferably ethylenically unsaturated polymerizable groups. The polymerizable group can be introduced into the molecules of the liquid crystal compound by various methods. The number of polymerizable groups possessed by the polymerizable liquid crystal compound is preferably 1 to 6 in one molecule, more preferably 1 to 3.
[0131] Examples of superimposable liquid crystal compounds include Makromol.Chem., Vol. 190, p. 2255 (1989), Advanced Materials Vol. 5, p. 107 (1993), U.S. Pat. No. 4,683,327, U.S. Pat. No. 5,622,648, U.S. Pat. No. 5,770,107, International Publication WO95 / 022586, International Publication WO95 / 024455, WO97 / 000600, WO98 / 023580, WO98 / 052905, Japanese Patent Laid-Open No. 1-272551, Japanese Patent Laid-Open No. 6-016616, Japanese Patent Laid-Open No. 7-110469, Japanese Patent Laid-Open No. 11-080081, and Japanese Patent Laid-Open No. 2001-328973. Two or more polymerizable liquid crystal compounds may also be used simultaneously. When two or more polymerizable liquid crystal compounds are used simultaneously, the alignment temperature can be lowered.
[0132] The amount of the polymerizable liquid crystal compound added to the liquid crystal composition is preferably 80 to 99.9% by mass, more preferably 85 to 99.5% by mass, and particularly preferably 90 to 99% by mass, relative to the solid content mass of the liquid crystal composition (mass excluding the solvent).
[0133] (Chiral reagent: optically active compound)
[0134] The chiral agent has the function of inducing a helical structure of a cholesteric liquid crystal phase. Since the handedness or helical pitch of the helix induced by the compound is different, the chiral agent can be selected according to the purpose.
[0135] As chiral reagent, there is no particular limitation, known compounds can be used. As the example of chiral reagent, the compound recorded in each bulletin of Liquid Crystal Device Handbook (Chapter 3, 4-3, TN, STN use chiral reagent, 199 pages, Japan Society for the Promotion of Science 142nd Committee compilation, 1989), Japanese Patent Publication No. 2003-287623, Japanese Patent Publication No. 2002-302487, Japanese Patent Publication No. 2002-080478, Japanese Patent Publication No. 2002-080851, Japanese Patent Publication No. 2010-181852 and Japanese Patent Publication No. 2014-034581 etc. can be enumerated.
[0136] The chiral agent generally contains an asymmetric carbon atom, but an axially asymmetric compound or a surface asymmetric compound not containing an asymmetric carbon atom can also be used as a chiral agent. Examples of the axially asymmetric compound or the surface asymmetric compound include binaphthyl, helicene, p-xylene dimer and their derivatives.
[0137] The chiral agent may also have a polymerizable group. In the case where both the chiral agent and the liquid crystal compound have a polymerizable group, a polymer having a repeating unit derived from the polymerizable liquid crystal compound and a repeating unit derived from the chiral agent can be formed by the polymerization reaction of the polymerizable chiral agent and the polymerizable liquid crystal compound. In this manner, the polymerizable group possessed by the polymerizable chiral agent is preferably a group of the same type as the polymerizable group possessed by the polymerizable liquid crystal compound. Thus, the polymerizable group of the chiral agent is also preferably an unsaturated polymerizable group, an epoxy group or an aziridine group, more preferably an unsaturated polymerizable group, and further preferably an ethylenically unsaturated polymerizable group.
[0138] Furthermore, the chiral agent may also be a liquid crystal compound.
[0139] As the chiral reagent, it is preferable to use an isosorbide derivative, an isomannide derivative, a binaphthyl derivative, etc. As the isosorbide derivative, a commercially available product such as LC-756 manufactured by BASF Corporation can also be used.
[0140] The content of the chiral agent in the liquid crystal composition is preferably 0.01 to 200 mol %, more preferably 1 to 30 mol %, based on the amount of the polymerizable liquid crystal compound.
[0141] (Polymerization initiator)
[0142] It is preferred that the liquid crystal composition contains a polymerization initiator. In the method of conducting the polymerization reaction by ultraviolet irradiation, the polymerization initiator used is preferably a photopolymerization initiator that can start the polymerization reaction by ultraviolet irradiation. Examples of photopolymerization initiators include α-carbonyl compounds (described in the specifications of U.S. Patent No. 2367661 and U.S. Patent No. 2367670), acyloin ethers (described in the specification of U.S. Patent No. 2448828), α-hydrocarbon substituted aromatic acyloin compounds (described in the specification of U.S. Patent No. 2722512), polynuclear quinone compounds (described in the specifications of U.S. Patent No. 3046127 and U.S. Patent No. 2951758), a combination of triaryl imidazole dimer and para-aminophenyl ketone (described in the specification of U.S. Patent No. 3549367), acridine and phenazine compounds (described in Japanese Patent Publication No. 60-105667 and U.S. Patent No. 4239850), acylphosphine oxide compounds (described in Japanese Patent Publication No. 63-040799, Japanese Patent Publication No. 5-029234, Japanese Patent Application Publication No. 10-095788, Japanese Patent Application Publication No. 10-029997, Japanese Patent Application Publication No. 2001-233842, Japanese Patent Application Publication No. 2000-080068, Japanese Patent Application Publication No. 2006-342166, Japanese Patent Application Publication No. 2013-114249, Japanese Patent Application Publication No. 2014-1 37466, Japanese Patent No. 4223071, Japanese Patent Publication No. 2010-262028, Japanese Patent Publication No. 2014-500852), oxime compounds (Japanese Patent Publication No. 2000-066385, Japanese Patent No. 4454067), and oxadiazole compounds (U.S. Patent No. 4212970). For example, reference can also be made to paragraphs
[0500] to
[0547] of Japanese Patent Publication No. 2012-208494.
[0143] As the polymerization initiator, an acylphosphine oxide compound or an oxime compound is preferably used.
[0144] As the acylphosphine oxide compound, for example, IRGACURE 810 (compound name: bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide) manufactured by BASF JAPAN LTD. can be used. As the oxime compound, commercially available products such as IRGACURE OXE01 (manufactured by BASF), IRGACURE OXE02 (manufactured by BASF), TR-PBG-304 (manufactured by Changzhou Qiangli Electronic New Materials Co., Ltd.), ADEKA ARKLS NCI-831, ADEKA ARKLS NCI-930 (manufactured by ADEKA CORPORATION), and ADEKA ARKLS NCI-831 (manufactured by ADEKA CORPORATION) can be used.
[0145] The polymerization initiator may be used alone or in combination of two or more.
[0146] The content of the photopolymerization initiator in the liquid crystal composition is preferably 0.1 to 20% by mass, more preferably 0.5 to 5% by mass, based on the content of the polymerizable liquid crystal compound.
[0147] (Crosslinking agent)
[0148] The liquid crystal composition may optionally contain a crosslinking agent in order to increase the film strength after curing and improve durability. As the crosslinking agent, a crosslinking agent that is cured by ultraviolet rays, heat, moisture, etc. can be appropriately used.
[0149] As a cross-linking agent, there is no particular limitation, and it can be suitably selected according to the purpose, for example, multifunctional acrylate compounds such as trimethylolpropane tri(meth)acrylate and pentaerythritol tri(meth)acrylate can be cited; epoxy compounds such as (meth) acrylic acid glycidyl ester and ethylene glycol diglycidyl ether; 2,2-bishydroxymethylbutanol-tri[3-(1-aziridine) propionate], 4,4-bis(ethylene iminocarbonylamino) diphenylmethane and other aziridine compounds; isocyanate compounds such as hexamethylene diisocyanate and biuret type isocyanate; polyoxazoline compounds with oxazoline groups in the side chain; alkoxysilane compounds such as vinyl trimethoxysilane and N-(2-aminoethyl) 3-aminopropyl trimethoxysilane, etc. In addition, it is possible to use a known catalyst according to the reactivity of the cross-linking agent, in addition to being able to improve film strength and durability, it is also possible to improve productivity. These can be used alone or in combination of two or more.
[0150] The content of the crosslinking agent is preferably 3 to 20% by mass, more preferably 5 to 15% by mass, relative to the content of the polymerizable liquid crystal compound. By setting the content of the crosslinking agent to 3% by mass or more, the effect of increasing the crosslinking density can be obtained, and by setting the content of the crosslinking agent to 20% by mass or less, the stability of the cholesteric liquid crystal layer can be prevented from decreasing.
[0151] (Orientation Control Agent)
[0152] An alignment control agent that helps to stably or quickly form a planar oriented cholesteric liquid crystal layer may also be added to the liquid crystal composition. Examples of alignment control agents include fluoro(meth)acrylate polymers described in paragraphs
[0018] to
[0043] of Japanese Patent Application Publication No. 2007-272185, compounds represented by formulas (I) to (IV) described in paragraphs
[0031] to
[0034] of Japanese Patent Application Publication No. 2012-203237, and compounds described in Japanese Patent Application Publication No. 2013-113913.
[0153] Furthermore, as the alignment control agent, one kind may be used alone, or two or more kinds may be used in combination.
[0154] The amount of the alignment control agent added to the liquid crystal composition is preferably 0.01 to 10% by mass, more preferably 0.01 to 5% by mass, and particularly preferably 0.02 to 1% by mass, based on the total mass of the polymerizable liquid crystal compound.
[0155] (Other additives)
[0156] In addition, the liquid crystal composition may also contain at least one selected from various additives such as surfactants and polymerizable monomers for adjusting the surface tension of the coating film to make the thickness uniform. In addition, the liquid crystal composition may further contain polymerization inhibitors, antioxidants, ultraviolet absorbers, light stabilizers, colorants, metal oxide particles, etc. as needed within a range that does not reduce the optical properties.
[0157] As for the cholesteric liquid crystal layer, a liquid crystal composition obtained by dissolving a polymerizable liquid crystal compound and a polymerization initiator, and further, as needed, a chiral agent, a surfactant, etc., in a solvent is applied to a support, an orientation layer, or a previously prepared cholesteric liquid crystal layer, etc., and dried to obtain a coating film, and the coating film is irradiated with active light to polymerize the cholesteric liquid crystal composition, thereby forming a cholesteric liquid crystal layer in which the cholesterol regularity is fixed.
[0158] In addition, a stacked film including a plurality of cholesteric liquid crystal layers can be formed by repeatedly performing the above-mentioned production steps of the cholesteric liquid crystal layers.
[0159] (Solvent)
[0160] The solvent used for preparing the liquid crystal composition is not particularly limited and can be appropriately selected according to the purpose, but an organic solvent is preferably used.
[0161] As the organic solvent, there is no particular limitation and it can be appropriately selected according to the purpose, for example, ketones, alkyl halides, amides, sulfoxides, heterocyclic compounds, hydrocarbons, esters and ethers can be mentioned. These can be used alone or in combination of two or more. Among these, ketones are particularly preferred in consideration of the load on the environment.
[0162] (Coating, Orientation, Polymerization)
[0163] The coating method of the liquid crystal composition is not particularly limited and can be appropriately selected according to the purpose, for example, a wire rod coating method, a curtain coating method, an extrusion coating method, a direct gravure coating method, a reverse gravure coating method, a die coating method, a spin coating method, a dip coating method, a spray coating method and a slide coating method can be cited. In addition, it can also be implemented by transferring a liquid crystal composition that is separately coated on a support. The liquid crystal molecules are oriented by heating the coated liquid crystal composition. The heating temperature is preferably below 200°C, and more preferably below 130°C. Through this orientation treatment, an optical film in which the polymerizable liquid crystal compound is twisted and oriented in a manner having a helical axis in a direction substantially perpendicular to the film surface can be obtained.
[0164] The liquid crystal composition can be cured by further polymerizing the aligned liquid crystal compound. The polymerization may be either thermal polymerization or photopolymerization by light irradiation, but photopolymerization is preferred. Ultraviolet rays are preferably used for light irradiation. The irradiation energy is preferably 20 mJ / cm 2 ~50J / cm 2 , more preferably 100 to 1,500 mJ / cm 2 .
[0165] In order to promote the photopolymerization reaction, light irradiation can also be carried out under heating conditions and / or in a nitrogen atmosphere. The wavelength of the irradiated ultraviolet light is preferably 350 to 430 nm. From the viewpoint of stability, the polymerization reaction rate is preferably higher, preferably 70% or more, more preferably 80% or more. The polymerization reaction rate can be determined by measuring the consumption ratio of polymerizable functional groups using IR absorption spectroscopy.
[0166] [Linearly polarized light reflecting layer]
[0167] As the selective reflection layer, a linearly polarized light reflection layer can be used. As the linearly polarized light reflection layer, for example, a polarizer formed by laminating thin films having different refractive index anisotropies can be mentioned.
[0168] This polarizer can be configured to have a high visible light transmittance and a central wavelength of selective reflection in a specific wavelength range of 650 to 780 nm, similar to the cholesteric liquid crystal layer. In addition, it can reflect obliquely incident projection light at a wavelength with high luminous efficiency when used in a head-up display system.
[0169] As a polarizer formed by laminating thin films having different refractive index anisotropies, for example, a polarizer described in JP-A-9-506837 can be used. Specifically, a polarizer can be formed using a wide variety of materials if processing is performed under conditions selected to obtain a refractive index relationship.
[0170] Typically, one of the first materials will have a different refractive index than the second material in the selected direction. This difference in refractive index can be achieved by a variety of methods including stretching, extrusion or coating during or after film formation. Furthermore, it is preferred to have similar rheological properties (e.g., melt viscosity) so that the two materials can be extruded simultaneously.
[0171] As a polarizer formed by stacking thin films with different refractive index anisotropy, a commercial product can be used. As a commercial product, a commercial product that is a laminate of a reflective polarizer and a pseudo support can be used. As a commercial product, for example, DBEF (manufactured by 3M Company) and APF (Advanced Polarizing Film (manufactured by 3M Company)) can be cited.
[0172] The thickness of the reflective polarizer is preferably in the range of 2.0 to 50 μm, more preferably in the range of 8.0 to 30 μm.
[0173] <Phase difference layer>
[0174] The half mirror film for projected image display (ie, the first embodiment of laminated glass) and the second embodiment of laminated glass of the present invention may include a phase difference layer. In particular, the half mirror film for projected image display and laminated glass including a cholesteric liquid crystal layer preferably include a phase difference layer.
[0175] By combining the phase difference layer with the cholesteric liquid crystal layer, a clear projection image can be displayed. By adjusting the in-plane phase difference and the slow axis direction, a half mirror for projected image display that provides high brightness and prevents ghosting in a head-up display system can be provided.
[0176] In the half mirror for projected image display, the phase difference layer is provided so as to be located on the visual recognition side with respect to all the selective reflection layers (cholesteric liquid crystal layers) when in use.
[0177] Even when the half mirror film and laminated glass for projected image display include a cholesteric liquid crystal layer, for example, when a projector of a head-up display system (image display system) irradiates a projection image of circularly polarized light, the half mirror film and laminated glass for projected image display may not include a phase difference layer.
[0178] There is no particular limitation on the phase difference layer, and it can be appropriately selected according to the purpose. For example, there can be mentioned a stretched polycarbonate film, a stretched norbornene polymer film, a transparent film oriented with inorganic particles having birefringence such as strontium carbonate, a film formed by obliquely vapor-depositing an inorganic dielectric on a support, a film oriented and fixed by uniaxially orienting a liquid crystal compound, etc.
[0179] As the phase difference layer, it is preferably a film that is oriented and fixed by uniaxially orienting the polymerizable liquid crystal compound. For example, the phase difference layer can be formed by coating a liquid crystal composition containing a polymerizable liquid crystal compound on the surface of a pseudo support or an orientation layer, and after the polymerizable liquid crystal compound in the liquid crystal composition is formed into a nematic orientation in a liquid crystal state, it is fixed by curing. In the formation of the phase difference layer at this time, no chiral agent is added to the liquid crystal composition. Otherwise, it can be carried out in the same manner as the formation of the above-mentioned cholesteric liquid crystal layer. Among them, when the nematic orientation is performed after the liquid crystal composition is applied, the heating temperature is preferably 50 to 120°C, and more preferably 60 to 100°C.
[0180] The retardation layer may be a layer obtained by applying a composition containing a polymer liquid crystal compound on the surface of a dummy support or an alignment layer, forming a nematic alignment in a liquid crystal state, and then cooling to fix the alignment.
[0181] The thickness of the phase difference layer is preferably 0.2 to 300 μm, more preferably 0.5 to 150 μm, and further preferably 1.0 to 80 μm. The thickness of the phase difference layer formed of the liquid crystal composition is not particularly limited, but is preferably 0.2 to 10 μm, more preferably 0.5 to 5.0 μm, and further preferably 1.0 to 2.0 μm.
[0182] It is preferable that the slow axis direction of the phase difference layer be determined based on the incident direction of incident light for displaying a projection image and the handedness of the helix of the cholesteric liquid crystal layer in the case of a head-up display system.
[0183] For example, in the first embodiment (half-mirror film for projected image display) and the second embodiment of the laminated glass of the present invention, when the direction for use in a head-up display system is determined, and the incident light is incident from the lower (vertically lower) direction of the laminated glass (half-mirror film for projected image display) and from the phase difference layer side relative to the cholesteric liquid crystal layer, the direction of the slow axis can be determined within the following range based on the in-plane phase difference.
[0184] For example, when a phase difference layer having an in-plane phase difference of 250 to 450 nm at a wavelength of 550 nm is used, the slow axis of the phase difference layer is preferably in the range of +30° to +85° or -30° to -85° relative to the vertical direction of the laminated glass (half mirror for projected image display). Furthermore, when a phase difference layer having an in-plane phase difference of 50 to 180 nm at a wavelength of 550 nm is used, the slow axis of the phase difference layer is preferably in the range of +120° to +175° or -120° to -175° relative to the vertical direction of the laminated glass.
[0185] It is installed in the windshield (stacked image mirror) of a vehicle such as an automobile. When normally used, it is possible to determine the direction within the surface of the windshield (stacked image mirror) and the up and down directions (up and down directions in the vertical direction) based on the driver and the surface that becomes the visual recognition side (observer side, driver side, inside the vehicle).
[0186] In this specification, when the vertical upward direction is referred to as for a windshield, a laminated glass, or a semi-reflective mirror film for displaying a projected image, it means the direction along the vertical direction when in use that can be determined as described above on the surface of the visual recognition side of the windshield, the laminated glass, or the semi-reflective mirror film for displaying a projected image that can be determined as described above.
[0187] When a retardation layer having an in-plane retardation of 250 to 450 nm at a wavelength of 550 nm is used, the slow axis of the retardation layer is more preferably in the range of -35° to +70° or -35° to -70° relative to the vertical direction of the laminated glass.
[0188] When a retardation layer having an in-plane retardation of 50 to 180 nm at a wavelength of 550 nm is used, the slow axis of the retardation layer is more preferably in the range of +125° to +160° or -125° to -160° relative to the vertical direction of the laminated glass.
[0189] The slow axis is defined as + and - in the above description, which indicates the clockwise direction and the counterclockwise direction when the visual recognition position is fixed. The preferred direction depends on the handedness of the helix of the cholesteric liquid crystal layer of the laminated glass (half mirror film for projected image display).
[0190] For example, when the handedness of the spiral of all cholesteric liquid crystal layers included in the laminated glass is right, when the phase difference layer is observed from the phase difference layer side relative to the cholesteric liquid crystal layer, the direction of the slow axis of the phase difference layer relative to the vertical direction in the clockwise direction is 30° to 85° or 120° to 175°. When the handedness of the spiral of all cholesteric liquid crystal layers included in the laminated glass is left, when the phase difference layer is observed from the phase difference layer side relative to the cholesteric liquid crystal layer, the direction of the slow axis of the phase difference layer in the counterclockwise direction is 30° to 85° or 120° to 175°.
[0191] [Second phase difference layer]
[0192] The half mirror film for projected image display and the laminated glass of the present invention may include a second retardation layer in addition to the retardation layer described above.
[0193] When the second phase difference layer is provided, the above phase difference layer (hereinafter also referred to as the "first phase difference layer"), all cholesteric liquid crystal layers and the second phase difference layer may be provided in this order. In particular, the first phase difference layer, the selective reflection layer and the second phase difference layer may be provided in this order from the visual recognition side.
[0194] By including a second phase difference layer at the above position in addition to the first phase difference layer, ghosting can be further prevented. In particular, ghosting can be further prevented when a projected image is formed by incident p-polarized light. The reason why ghosting can be further prevented by using the second phase difference layer is presumed to be because ghosting caused by light of a wavelength not existing in the selective reflection band of the cholesteric liquid crystal layer undergoing polarization conversion in the cholesteric liquid crystal layer and being reflected by the back side of the windshield can be prevented.
[0195] The in-plane retardation of the second retardation layer may be appropriately adjusted within the range of 160 to 460 nm, preferably within the range of 240 to 420 nm at a wavelength of 550 nm.
[0196] The material, thickness, etc. of the second retardation layer can be selected within the same range as those of the first retardation layer.
[0197] The slow axis direction of the second retardation layer is preferably determined based on the incident direction of incident light for displaying a projected image and the handedness of the helix of the cholesteric liquid crystal layer.
[0198] For example, if the second phase difference layer has an in-plane phase difference in the range of 160 to 400 nm in a wavelength of 550 nm, it is preferred that the slow axis be in the range of +10° to +35° or -10° to -35° relative to the vertical direction of the laminated glass (half-mirror film for projected image display). If the second phase difference layer has an in-plane phase difference in the range of 200 to 400 nm in a wavelength of 550 nm, it is preferred that the slow axis be in the range of +100° to +140° or -100° to -140° relative to the vertical direction of the laminated glass.
[0199] [Other layers]
[0200] The half mirror film for projected image display and the laminated glass may include other layers in addition to the essential components. It is preferred that all other layers are transparent in the visible light region.
[0201] Furthermore, it is preferred that all other layers have low birefringence. In this specification, low birefringence means that the in-plane phase difference in the wavelength region where the projection image display semi-reflective lens for the windshield of the present invention shows reflection is less than 10nm, and the in-plane phase difference is preferably less than 5nm. Furthermore, it is preferred that the difference in refractive index between the average refractive index (in-plane average refractive index) of the other layers and the cholesteric liquid crystal layer is small. As other layers, a support, an orientation layer, an adhesive layer, etc. can be cited.
[0202] (Transparent support)
[0203] In the first embodiment of the half mirror film and laminated glass for projected image display of the present invention, the transparent support is an essential component. In contrast, in the second embodiment of the laminated glass of the present invention, as described above, the transparent support can be omitted, and the phase difference layer can also serve as the transparent support. Alternatively, the transparent support can also serve as the phase difference layer.
[0204] In the transparent support body that preferably uses in the present invention, the absolute value of the in-plane phase difference in the wavelength 550nm is below 10nm, and the absolute value of the preferred in-plane phase difference is below 5nm.And, the absolute value of the phase difference Rth in the thickness direction is preferably below 40nm, more preferably below 30nm.It is little by phase difference, and the disorder of the polarized light that the transparent support body causes tapers down, and it is little by the physical characteristic in the plane, has improved the effect of the present invention.
[0205] The transparent support is preferably composed of a resin such as cellulose acylate or acrylic acid, and is particularly preferably composed of a cellulose acylate resin, and particularly preferably composed of a triacetyl cellulose resin or a cellulose acetate butyrate resin.
[0206] In the present invention, it is preferred that the two glass plates, the half mirror film, and the intermediate film are bonded together while the transparent support is heated so that the storage elastic modulus of the transparent support becomes 2.0 GPa or less.
[0207] Furthermore, it is also preferred that the two glass plates, the half mirror film, and the intermediate film are bonded together while heating the transparent support so that the storage elastic modulus of the half mirror film (laminate) including the transparent support becomes 2.0 GPa or less.
[0208] Furthermore, in the second aspect of the laminated glass of the present invention, Figure 4 In the example shown, when the heat seal layer is adjacent to the phase difference layer, the transparent support 1 is disposed on the outdoor side relative to the selective reflection layer 3. Therefore, an ultraviolet absorber can be added to the transparent support 1 to impart an ultraviolet cutoff function.
[0209] The thickness of the transparent support may be about 5.0 to 1000 μm, preferably 10 to 250 μm, and more preferably 15 to 90 μm.
[0210] (Heat seal layer)
[0211] In the first aspect of the half mirror film for projected image display and the laminated glass of the present invention, the transparent support for the half mirror film for projected image display has a heat seal layer on the side opposite to the side having the selective reflection layer.
[0212] Furthermore, in the second embodiment of the laminated glass of the present invention, the half-mirror film and the intermediate film are sandwiched by a glass plate on the half-mirror film side and a glass plate on the intermediate film side, and a heat-sealing layer having a thickness of 0.1 to 50 μm and containing a thermoplastic resin is provided between the half-mirror film and the glass plate on the half-mirror film side.
[0213] In the first embodiment of the half mirror film for projected image display and the laminated glass of the present invention, the "heat sealing layer" is a layer for physically joining the transparent support body of the half mirror film for projected image display and the glass plate, and has the function of melting the thermoplastic resin contained in the heat sealing layer by heating when making the laminated glass. In addition, in the second embodiment of the laminated glass of the present invention, the "heat sealing layer" is a layer for physically joining the glass plate and the adjacent layer, and has the function of melting the thermoplastic resin contained in the heat sealing layer by heating when making the laminated glass.
[0214] In the present invention, a heat-sealing layer is provided to ensure the sliding property between the half-mirror film and the glass plates of the laminated glass, so that when the laminated glass can be heated while the two glass plates, the half-mirror film and the intermediate film are tightly bonded together, wrinkles generated during production can be suppressed and the half-mirror film and the glass plates can be firmly bonded together.
[0215] In particular, in the first embodiment of the semi-reflective mirror film for projected image display and laminated glass of the present invention, by forming a mixed layer containing components of the transparent support and components of the heat-sealing layer between the transparent support and the heat-sealing layer, the adhesion between the transparent support and the heat-sealing layer becomes strong, thereby preventing peeling failure inside the laminated glass.
[0216] Furthermore, in the second embodiment of the laminated glass of the present invention, when the transparent support and the heat seal layer are adjacent to each other, it is preferred that the same mixed layer is formed between the transparent support and the heat seal layer, so that the adhesion between the transparent support and the heat seal layer becomes strong, and the peeling failure inside the laminated glass can be prevented (refer to Figure 5 ).
[0217] In the second embodiment of the laminated glass of the present invention, the half mirror film has a selective reflection layer and a phase difference layer that reflect light in a wavelength-selective manner, and the heat seal layer is preferably adjacent to the selective reflection layer or the phase difference layer, and the heat seal layer is more preferably adjacent to the selective reflection layer. In particular, when the selective reflection layer and the phase difference layer are composed of a solidified liquid crystal layer, the surface of the heat seal layer adjacent to them is smoothed, so it is less likely to cause wrinkles when manufacturing the laminated glass, which is more preferred.
[0218] Here, when the heat seal layer is adjacent to the selective reflection layer or the phase difference layer, the heat seal layer and the selective reflection layer or the phase difference layer may be in direct contact or may be in indirect contact with each other via an adhesive layer or the like.
[0219] In the second aspect of the laminated glass of the present invention, the thickness of the heat seal layer is 0.1 to 50 μm, preferably 0.1 to 25 μm, more preferably 0.1 to 10 μm, further preferably 0.1 to 5.0 μm, and particularly preferably 0.1 to 3.0 μm.
[0220] Furthermore, in the second embodiment of the laminated glass of the present invention, as described above, the transparent support body adjacent to the heat-sealing layer or the phase difference layer or the mixed layer between the selective reflection layer and the heat-sealing layer is not necessary. In this case, by using a chemically bonded adhesion enhancer at the interface between the heat-sealing layer and the layer adjacent to the heat-sealing layer, or by the action of a cross-linking agent contained in the heat-sealing layer and / or the layer adjacent to the heat-sealing layer, good adhesion between the two can be obtained.
[0221] Moreover, as described above, in the second embodiment of the laminated glass of the present invention, the transparent support can be omitted. In this case, for example, the phase difference layer can also serve as the transparent support. In the second embodiment of the laminated glass of the present invention, when the phase difference layer also serves as the transparent support, it is preferred that the phase difference within the above-mentioned preferred range can be exhibited by stretching a film containing a birefringent thermoplastic resin such as cellulose acylate, acrylic acid, and cyclic olefin, among which the phase difference layer composed of cellulose acylate resin is particularly preferred, and the phase difference layer composed of triacetyl cellulose resin or acetyl cellulose resin is particularly preferred.
[0222] [Thermoplastic resin contained in heat seal layer]
[0223] The heat seal layer contains a thermoplastic resin. The heat seal layer is preferably transparent. Furthermore, the thermoplastic resin is preferably an amorphous resin.
[0224] As such thermoplastic resin, a resin having good affinity and adhesion to the glass plate is preferred, and a resin selected from the group consisting of polyvinyl acetal resin represented by polyvinyl butyral (PVB) resin, ethylene-vinyl acetate copolymer and chlorine-containing resin can be used. The main component of the heat seal layer is preferably the above resin. In addition, the main component refers to a component accounting for 50% by mass or more of the total mass of the heat seal layer.
[0225] Among the above resins, polyvinyl acetal resins represented by polyvinyl butyral resins or ethylene-vinyl acetate copolymers are preferred, and polyvinyl acetal resins represented by polyvinyl butyral resins (also referred to as alkyl acetalized polyvinyl alcohol) are more preferred. The resin is preferably a synthetic resin.
[0226] Polyvinyl butyral can be obtained by acetalizing polyvinyl alcohol with butyraldehyde. The preferred lower limit of the acetalization degree of the polyvinyl acetal resin represented by the polyvinyl butyral resin is 40%, the preferred upper limit is 85%, the more preferred lower limit is 60%, and the more preferred upper limit is 80%.
[0227] Polyvinyl alcohol used as a raw material of these resins is generally obtained by saponifying polyvinyl acetate, and polyvinyl alcohol having a saponification degree of 80 to 99.8 mol % is generally used.
[0228] Furthermore, the preferred lower limit of the degree of polymerization of the polyvinyl alcohol is 200, and the preferred upper limit is 10000. If the degree of polymerization of the polyvinyl alcohol is 200 or more, the penetration resistance of the obtained laminated glass is not easy to decrease, and if it is 10000 or less, the formability of the resin film is good, and the rigidity of the resin film does not become too large, and the processability is good. A more preferred lower limit is 500, and a more preferred upper limit is 5000. The degree of polymerization mentioned here means the average degree of polymerization.
[0229] As the polyvinyl acetal resin that is preferably used for heat seal layer, for example, KS-10, KS-1, KS-3 and KS-5 etc. manufactured by SEKISUI CHEMI CAL CO., LTD can be enumerated. These polyvinyl acetal resins are easy to form a mixed layer with the transparent support when coated on the transparent support. Especially, from the perspective of excellent adhesion with the transparent support, it is possible to preferably use KS-3 and KS-5 with a calculated molecular weight of more than 100,000.
[0230] In addition, in order to apply the heat seal layer as a thin layer, it is important that the coating liquid has low viscosity. From this viewpoint, the calculated molecular weight is preferably more than 10,000 and less than 50,000, preferably KS-10 and KS-1. In the present invention, the calculated molecular weight is defined as the average degree of polymerization of the polyvinyl alcohol used as the raw material multiplied by the molecular weight of the acetalized unit.
[0231] It is also a preferred embodiment that the heat seal layer contains, in addition to the polyvinyl acetal resin, a crosslinking agent for crosslinking the polyvinyl alcohol units in the structure of the polyvinyl acetal resin.
[0232] Examples of the crosslinking agent include epoxy-based additives, and particularly preferred are compounds having two or more epoxy groups in one molecule, and preferred are compounds represented by the following general formula (EP1).
[0233] Ep-CH2-O-(RO) n -CH2-Ep(EP1)
[0234] In the above general formula (EP1), Ep is an epoxy group, R is an alkylene group having 2 to 4 carbon atoms, and n is 1 to 30. However, when n is 2 or more, a plurality of Rs may be the same or different.
[0235] Specific examples of the compound represented by the general formula (EP1) include Denacol EX-810, 811, 821, 830, 832, 841, 850, 851, 861, 911, 920, 931, and 941 manufactured by Nagase ChemteX Corporation.
[0236] When an epoxy additive is used as a crosslinking agent, an onium salt cationic polymerization initiator (photoacid generator) consisting of a light-absorbing cation part and an anion part as an acid generating source can be used, and a known sulfonium salt-based or iodonium salt-based cationic polymerization initiator can be used. An iodonium-based cationic polymerization initiator is particularly preferred.
[0237] [Solvent for coating composition of heat seal layer]
[0238] In the present invention, the coating composition for forming the heat seal layer contains 30 to 70% by mass of at least one solvent having permeability to the transparent support, based on the total amount of the solvent.
[0239] The "permeability" relative to the transparent support means that the solvent will penetrate into the transparent support when applied to the transparent support, and the solvent can also penetrate into the support, thereby the transparent support shows swelling. The permeable solvent penetrates into the transparent support, and when the heat seal layer is applied, a mixed layer containing components of the heat seal layer and components of the transparent support is formed between the heat seal layer and the transparent support.
[0240] As specific examples of solvents that are permeable to the transparent support, when the transparent support is triacetyl cellulose, ketones: acetone, methyl ethyl ketone, cyclohexanone, methyl isobutyl ketone and diacetone alcohol can be cited; esters: methyl formate, methyl acetate, ethyl acetate, butyl acetate and ethyl lactate; nitrogen-containing compounds: nitromethane, acetonitrile, N-methylpyrrolidone and N,N-dimethylformamide; glycols: methyl glycol and methyl glycol acetate; ethers: tetrahydrofuran, 1,4-dioxane, dioxolane and diisopropyl ether; halogenated hydrocarbons: dichloromethane, chloroform and tetrachloroethane; glycol ethers: methyl cellosolve, ethyl cellosolve, butyl cellosolve and cellosolve acetate; others: dimethyl sulfoxide and propylene carbonate, etc., and mixtures thereof can also be cited, and esters and ketones; methyl acetate, ethyl acetate, butyl acetate and methyl ethyl ketone can be preferably cited. Furthermore, alcohols such as methanol, ethanol, isopropanol, butanol, and isobutanol, and aromatic hydrocarbons such as toluene and xylene can also be used in a mixed state with the above-mentioned penetrating solvent.
[0241] As described above, in the laminated glass according to the second aspect of the present invention, the heat seal layer is preferably adjacent to the selective reflection layer or the phase difference layer.
[0242] In this case, the thermoplastic resin contained in the heat seal layer is preferably the above-mentioned resin.
[0243] Furthermore, the solvent of the coating composition of the heat seal layer is preferably a solvent that dissolves the thermoplastic resin contained in the heat seal layer. When polyvinyl butyral is used, alcohols such as methanol, ethanol, isopropanol, butanol, isobutanol and diacetone alcohol can be mentioned; aromatic hydrocarbons such as toluene and xylene; glycol ethers such as methyl cellosolve, ethyl cellosolve, butyl cellosolve and cellosolve acetate; ketones such as acetone, methyl ethyl ketone, cyclohexanone, methyl isobutyl ketone, diisobutyl ketone and isophorone; amides such as N,N-dimethylacetamide, N,N- dimethylformamide and N-methyl-2-pyrrolidone; esters: methyl formate, methyl acetate, ethyl acetate, butyl acetate and ethyl lactate; ethers: tetrahydrofuran, 1,4-dioxane, dioxolane, diisopropyl ether and ethyl ether; halogenated hydrocarbons: dichloromethane, chloroform and tetrachloroethane; nitrogen-containing compounds: nitromethane, acetonitrile, N-methylpyrrolidone and N,N-dimethylformamide; glycols: methyl glycol and methyl glycol acetate; others: dimethyl sulfoxide, propylene carbonate and water, or mixtures thereof.
[0244] In order to improve the close contact between the heat seal layer and any one of the selective reflection layer or the phase difference layer, the polymerization reaction rate when making any one of the selective reflection layer or the phase difference layer adjacent to the heat seal layer is adjusted to 70% or less, so that a part of the heat seal layer penetrates into the surface of any one of the selective reflection layer or the phase difference layer, which can improve the close contact. The polymerization reaction rate is preferably 5 to 60%, and more preferably 10 to 40%. That is, in the second embodiment of the laminated glass of the present invention, a mixed layer having components of two layers mixed therein can be provided between the heat seal layer and the phase difference layer or between the heat seal layer and the selective reflection layer.
[0245] Furthermore, in order to improve the close contact between the heat seal layer and any one of the selective reflection layer or the phase difference layer, in addition to adjusting the polymerization reaction rate of any one of the selective reflection layer or the phase difference layer in contact with the heat seal layer to 70% or less, a crosslinking agent may be added to the heat seal layer. As the crosslinking agent, the aforementioned crosslinking agent that can be added with a liquid crystal composition is preferred. At this time, a polymerization initiator that initiates and promotes crosslinking may also be added. In the method of performing polymerization reaction by ultraviolet irradiation, the polymerization initiator used is preferably the aforementioned photopolymerization initiator that can start polymerization reaction by ultraviolet irradiation.
[0246] Since too much amount of the crosslinking agent reduces the adhesion with the glass, it is preferably set within the range of 0.01 to 50%, more preferably 0.1 to 30%, based on the thermoplastic resin.
[0247] When the heat seal layer is produced, the adhesion can be further improved by promoting the reaction so as to crosslink the heat seal layer and the selective reflection layer or the phase difference layer.
[0248] When ultraviolet irradiation is used, it is preferred that the ultraviolet irradiation amount when forming the selective reflection layer in contact with the heat seal layer is set so that the polymerization reaction rate becomes 70% or less, and when the heat seal layer is formed, ultraviolet irradiation is performed again to promote crosslinking between the heat seal layer and the selective reflection layer. Here, regarding the polymerization reaction rate, the consumption ratio of the polymerizable functional group can be determined using the IR absorption spectrum.
[0249] [Roughening of heat seal layer]
[0250] In the present invention, in order to improve the sliding property between the half mirror film and the glass plate of the laminated glass, the surface of the heat seal layer is preferably roughened.
[0251] As a preferred method for roughening the surface of the heat seal layer, an appropriate amount of water can be used as a solvent of the coating composition forming the heat seal layer. It is believed that by using water, the surface of the heat seal layer is roughened by the action of water vapor when the heat seal layer is dried and cured. The preferred amount of water in the coating composition of the heat seal layer is 2 to 8% by mass relative to all solvents.
[0252] In addition, as another preferred method for roughening the surface of the heat seal layer, there is a method of adding an appropriate amount of inorganic particles to the heat seal layer, wherein the inorganic particles include at least one of silicon dioxide, aluminum oxide, titanium dioxide, zirconium oxide, calcium carbonate, talc, clay, calcined kaolin, calcined calcium silicate, hydrated calcium silicate, aluminum silicate, magnesium silicate and calcium phosphate, etc. In this case, the added inorganic particles are distributed on the surface of the heat seal layer, and the surface is roughened.
[0253] As the inorganic fine particles added to the heat seal layer, inorganic oxide fine particles are preferred, and silica, alumina, titania or zirconia is more preferred.
[0254] The inorganic fine particles added to the heat seal layer are preferably composed of primary particles and form secondary particles formed by aggregation of the primary particles.
[0255] As inorganic particles added to the heat seal layer, preferably inorganic particles having an average primary particle size of 5 to 50 nm and an average secondary particle size of 100 to 500 nm are contained, and an average secondary particle size of 150 to 400 nm is particularly preferred. The inorganic particles added to the heat seal layer are preferably silica particles, for example, a commercially available composition containing silica particles (commercially available colloidal silica dispersion) can be used directly or arbitrarily by adding an organic solvent.
[0256] The preferred amount of the inorganic fine particles (solid content) in the coating composition of the heat seal layer is preferably 1 to 40% by mass, more preferably 3 to 30% by mass, based on the total solid content of the heat seal layer.
[0257] Furthermore, when forming a heat seal layer, from the viewpoint of adhesion and slip, it is preferred that the amount of residual solvent is small. As a method for reducing the amount of residual solvent, it is preferred to increase the temperature during drying or to extend the drying time. Regarding the drying temperature, it is preferably above the boiling point of the solvent used and below 200°C, and more preferably 80 to 150°C. Regarding the drying time, it is preferably 0.2 minutes to 300 minutes, and more preferably 0.5 minutes to 10 minutes. Furthermore, it is also preferred to place the heat seal layer under atmospheric pressure for more than 1 day after forming the heat seal layer.
[0258] The average primary particle size of the inorganic fine particles is a value obtained by measuring the inorganic fine particles contained in the dispersion composition or the inorganic fine particles contained in the heat seal layer.
[0259] The measurement is performed by transmission electron microscopy. Specifically, for 50 randomly selected primary particles, the diameter of the circle circumscribed to the primary particle is obtained, and the arithmetic average thereof is set as the average primary particle diameter. The observation magnification of the transmission electron microscope is set to an arbitrary magnification that can distinguish the primary particle diameter between 500,000 times and 5,000,000 times.
[0260] The average secondary particle size of the inorganic fine particles is a value measured by spherical fitting (refractive index: 1.46) using a laser diffraction / scattering particle size distribution measuring device. As a measuring device, for example, MicroTrac MT3000 manufactured by Microtrac BEL Corp. can be used.
[0261] (Seam Enhancer)
[0262] The compound (hereinafter, also referred to as a close fit enhancer) having a plurality of groups selected from the group consisting of a polymerizable group and a group that can form a key with the resin contained in the transparent support has the function of enhancing the close fit of the heat seal layer and the transparent support. And, at least one of the transparent support and the heat seal layer contains the above-mentioned component derived from the close fit enhancer is one of the preferred embodiments of the present invention. In addition, the above-mentioned component derived from the close fit enhancer represents a component obtained by reacting a group selected from the group consisting of a polymerizable group and a group that can form a key with the resin contained in the transparent support. For example, the close fit enhancer is included in the heat seal layer forming coating liquid, and the component derived from the close fit enhancer is included in the formed heat seal layer.
[0263] The polymerizable groups in the adhesion enhancer are defined as above. The number of polymerizable groups is not particularly limited and may be one or more (two or more). When the adhesion enhancer does not have a group capable of forming a bond with the resin contained in the transparent support, it has a plurality of polymerizable groups.
[0264] Specifically, the adhesion enhancer can be selected from commercially available monomers and oligomers having multiple polymerizable groups, and preferably has more than three polymerizable groups. Examples of such monomers or oligomers include U6HA (hexafunctional urethane acrylate oligomer) manufactured by Shin-Nakamura Chemical Co., Ltd. and PET-30 manufactured by Nippon Kayaku Co., Ltd.
[0265] When the adhesion enhancer has a polymerizable group, it is preferred to appropriately select and use the above-mentioned polymerization initiator.
[0266] The group capable of forming a bond with the resin contained in the transparent support (hereinafter also referred to as a reactive group) contained in the adhesion enhancer means a group capable of chemically adsorbing the resin contained in the transparent support by interacting with a group possessed by a material constituting the resin contained in the transparent support.
[0267] As such reactive groups, for example, boric acid, borate, oxirane, oxetane, hydroxyl, carboxyl, isocyanate and -SiX3 (X represents halogen, alkoxy or alkyl, at least one of which is halogen or alkoxy) etc. can be cited. Wherein, when the resin contained in the above-mentioned transparent support is a partially saponified cellulose ester resin, as a reactive group, it is preferably a group (for example, boric acid, borate, isocyanate and -SiX3 etc.) among the exemplified groups that can form a bond with the hydroxyl group remaining in the cellulose ester resin, more preferably a boric acid, borate or isocyanate. The number of reactive groups is not particularly limited, and can be one or more (more than two).
[0268] As the close fit enhancer, it can be a compound having only a plurality of polymerizable groups or a compound having only a plurality of groups that can form a key with the resin contained in the transparent support. As the compound having only a plurality of polymerizable groups, a commercially available multifunctional monomer compound can be used. And, as the compound having only a plurality of groups that can form a key with the resin contained in the transparent support, for example, polyisocyanate can be cited, and as an example, CORONATE L manufactured by TOSOH CORPORATION can be cited.
[0269] The adhesion enhancer is preferably a compound having at least one polymerizable group in the molecule and at least one group capable of forming a bond with the resin contained in the transparent support, from the viewpoint of high adhesion between the transparent support and the heat seal layer.
[0270] Furthermore, when a mixed layer of these is formed between the transparent support and the heat seal layer, the adhesion-enhancing effect of the adhesion enhancer is greater. That is, when a mixed layer is formed and an adhesion enhancer is used, a synergistic effect is achieved, which is preferred.
[0271] As the most preferred embodiment of the adhesion enhancer, a compound represented by formula (A) can be mentioned from the viewpoint of further improving the adhesion between the transparent support and the heat seal layer.
[0272] Formula (A)(Z) n -XQ
[0273] In formula (A), Z represents a substituent having a polymerizable group. The definition of the polymerizable group is as described above. As a specific example of a substituent having the polymerizable group, preferably a substituent comprising a (meth)acryloyl group, a styryl group, a vinyl ketone group, a vinyl group, a butadienyl group, a vinyl ether group, an oxirane group, an aziridine group or an oxetane group, more preferably a substituent comprising a (meth)acryloyl group, a styryl group, a vinyl group, an oxirane group or an oxetane group, further preferably a substituent comprising a (meth)acryloyl group or a styryl group, and particularly preferably a substituent comprising a (meth)acryloyl group.
[0274] Among them, Z is preferably a substituent having a group represented by the following formula (II) or an oxiranyl group or an oxetaneyl group.
[0275] [Chemical formula 1]
[0276]
[0277] In formula (II), R 3 It is a hydrogen atom or a methyl group, and is preferably a hydrogen atom.
[0278] L 1 It is a single bond or a divalent linking group selected from -O-, -CO-, -NH-, -CO-NH-, -COO-, -O-COO-, an alkylene group, an arylene group, a heterocyclic group (heteroaryl group), and a combination thereof, preferably a single bond, -CO-NH-, or -COO-, and most preferably a single bond or -CO-NH-. * indicates a bonding position.
[0279] In formula (A), Q is a group capable of forming a bond with the resin contained in the transparent support. The definition of this group is as described above.
[0280] In formula (A), X represents an n+1-valent linking group.
[0281] n represents an integer of 1 to 4, and 1 is more preferred.
[0282] In addition, when n is 1, X represents a divalent linking group, for example, preferably a divalent linking group selected from -O-, -CO-, -NH-, -CO-NH-, -COO-, -O-COO-, an alkylene group, an arylene group, a heteroaryl group and a combination thereof, more preferably a substituted or unsubstituted arylene group.
[0283] X is preferably -COO-arylene-, -arylene-, or -CONH-arylene-, and more preferably -COO-arylene-.
[0284] The compound represented by formula (A) preferably contains at least one boron atom, and is preferably a compound represented by the following formula (I).
[0285] [Chemical formula 2]
[0286]
[0287] In formula (I), R 1 and R 2 Each independently represents a hydrogen atom, a substituted or unsubstituted aliphatic hydrocarbon group, an aryl group or a heteroaryl group.
[0288] And, R 1 With R 2 The groups may be linked to each other via a linking group consisting of an alkylene group, an arylene group, or a combination thereof.
[0289] In formula (I), Z and X 1 is defined as above.
[0290] In formula (I), R 1 and R 2 The substituted or unsubstituted aliphatic hydrocarbon groups respectively represented include substituted or unsubstituted alkyl groups, alkenyl groups and alkynyl groups.
[0291] Specific examples of the alkyl group include linear, branched or cyclic alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, undecyl, dodecyl, tridecyl, hexadecyl, octadecyl, eicosyl, isopropyl, isobutyl, sec-butyl, tert-butyl, isopentyl, neopentyl, 1-methylbutyl, isohexyl, 2-methylhexyl, cyclopentyl, cyclohexyl, 1-adamantyl and 2-norbornyl.
[0292] Specific examples of alkenyl include straight-chain, branched or cyclic alkenyls such as vinyl, 1-propenyl, 1-butenyl, 1-methyl-1-propenyl, 1-cyclopentenyl and 1-cyclohexenyl. Specific examples of alkynyl include ethynyl, 1-propynyl, 1-butynyl and 1-octynyl.
[0293] Specific examples of the aryl group include an aryl group formed by 1 to 4 benzene rings forming a condensed ring, and an aryl group formed by a benzene ring and an unsaturated five-membered ring forming a condensed ring. Specific examples include phenyl, naphthyl, anthracenyl, phenanthryl, indenyl, acenaphthenyl, fluorenyl and pyrenyl.
[0294] In addition, if possible, R 1 , R 2 and X 1 It may be further substituted with one or more substituents. The type of the substituent is not particularly limited, and examples thereof include the substituent group Y exemplified in paragraph 0054 of JP-A-2006-309120.
[0295] Specific examples of the adhesion enhancer are shown below, but the present invention is not limited thereto.
[0296] [Chemical formula 3]
[0297]
[0298] [Chemical formula 4]
[0299]
[0300] [Chemical formula 5]
[0301]
[0302] (Orientation Layer)
[0303] The half mirror for projected image display may include an alignment layer as a base layer to which a liquid crystal composition is applied when forming a cholesteric liquid crystal layer or a phase difference layer.
[0304] The alignment layer can be provided by the following methods: rubbing treatment of organic compounds such as polymers (resins such as polyimide, polyvinyl alcohol, polyester, polyarylate, polyamide-imide, polyetherimide, polyamide, and modified polyamide), oblique evaporation of inorganic compounds, formation of a layer with microgrooves, or accumulation of organic compounds (e.g., ω-tricosanoic acid, dioctadecylmethylammonium chloride, and methyl stearate) using the Langmuir-Blodgett method (LB film). In addition, an alignment layer that generates an alignment function by imparting an electric field, imparting a magnetic field, or irradiating light can also be used.
[0305] In particular, in an alignment layer composed of a polymer, it is preferred to apply a liquid crystal composition to the rubbed surface after rubbing treatment. The rubbing treatment can be performed by rubbing the surface of the polymer layer with paper or cloth in a predetermined direction.
[0306] The liquid crystal composition may be applied to the surface of the support or to the surface of the support subjected to a rubbing treatment without providing an alignment layer.
[0307] When the liquid crystal layer is formed using a dummy support, the alignment layer may be peeled off together with the dummy support without becoming a layer constituting the half mirror for projected image display.
[0308] The thickness of the alignment layer is preferably 0.01 to 5.0 μm, more preferably 0.05 to 2.0 μm.
[0309] (Adhesive layer)
[0310] The adhesive layer can be disposed, for example, between the cholesteric liquid crystal layers, between the selective reflection layer (cholesteric liquid crystal layer) and the phase difference layer, between the selective reflection layer and the second phase difference layer, and between the selective reflection layer and the transparent support. Furthermore, the adhesive layer can also be disposed between the selective reflection layer and the intermediate film, between the phase difference layer (the first or second) and the intermediate film, etc.
[0311] The adhesive layer may be formed of an adhesive.
[0312] As adhesives, from the viewpoint of curing mode, there are hot melt type, heat curing type, light curing type, reaction curing type, and pressure sensitive adhesive type that does not require curing, and as raw materials for each type, there can be used compounds such as acrylates, urethanes, urethane acrylates, epoxies, epoxy acrylates, polyolefins, modified olefins, polypropylenes, ethylene-vinyl alcohols, vinyl chlorides, chloroprene rubbers, cyanoacrylates, polyamides, polyimides, polystyrenes, and polyvinyl butyrals. From the viewpoint of operability and productivity, the curing mode is preferably a light curing type, and from the viewpoint of optical transparency and heat resistance, the raw materials are preferably acrylates, urethane acrylates, epoxy acrylates, etc.
[0313] The adhesive layer may be a layer formed by using a high-transparency adhesive transfer tape (OCA tape). As the high-transparency adhesive transfer tape, a commercial product for an image display device, especially a commercial product for the surface of the image display portion of the image display device, may be used. Examples of commercial products include adhesive sheets (PD-S1, etc.) manufactured by PANAC Co., Ltd. and adhesive sheets of the MHM series of NICHIEI KAKOH CO., LTD.
[0314] The thickness of the adhesive layer is preferably 0.5 to 10 μm, more preferably 1.0 to 5.0 μm. Furthermore, the thickness of the adhesive layer formed by the OCA tape can be 10 to 50 μm, preferably 15 to 30 μm. In order to reduce the color unevenness of the half mirror for projected image display, it is preferred to set it with a uniform thickness.
[0315] <Windshield>
[0316] The laminated glass of the present invention can be used to provide a windshield having a projected image display function.
[0317] In this specification, the windshield refers to a general window glass of a vehicle such as a car, a train, an airplane, a ship, an amusement ride, etc. The windshield is preferably a front windshield located in the direction of travel of the vehicle. The windshield is preferably a front windshield of a vehicle.
[0318] The visible light transmittance of the windshield is preferably 70% or more, more preferably more than 70%, further preferably 75% or more, and particularly preferably 80% or more. This visible light transmittance is preferably satisfied at any position of the windshield, and particularly preferably at the projection image display position.
[0319] As described above, the laminated glass (half mirror film for projected image display) of the present invention has high visible light transmittance in a wavelength region with high luminous efficiency, so when any glass generally used for windshields is used, it can be configured to satisfy the above-mentioned visible light transmittance.
[0320] The windshield (laminated glass of the present invention) may be flat and may be shaped for assembly to a vehicle to which it is applied, and may have a curved surface, for example.
[0321] The windshield may have a uniform thickness or a non-uniform thickness in the projection image display area. For example, the windshield may have a wedge-shaped cross-section as in the vehicle glass described in Japanese Patent Application Publication No. 2011-505330, and the thickness in the projection image display area may be non-uniform, but the thickness in the projection image display area is preferably uniform.
[0322] [Projected image display area]
[0323] The half mirror film for projected image display of the present invention and the half mirror film in the second embodiment of the laminated glass of the present invention can be provided at the projection image display portion of the windshield. Hereinafter, the half mirror film for projected image display of the present invention and the half mirror film in the second embodiment of the laminated glass of the present invention are also collectively referred to as half mirror film.
[0324] The projection image display portion can be formed by arranging the half-mirror film on the outer surface of the glass plate of the windshield or between two glass plates in the windshield (laminated glass). When the half-mirror film is arranged on the outer surface of the glass plate of the windshield, the half-mirror film can be arranged on the visual recognition side when viewed from the glass plate, or on the opposite side, but is preferably arranged on the visual recognition side. The half-mirror film is more preferably arranged between the two glass plates. This is because the half-mirror film, which has lower scratch resistance than the glass plate, can be protected.
[0325] In this specification, the projection image display portion is a portion that can display a projection image by reflected light, and any portion can be used as long as the projection image projected from a projector or the like can be visibly displayed.
[0326] The projected image display part functions as a combiner of the head-up display system. In the head-up display system, the combiner refers to an optical component that can visually display the image projected from the projector, and when the combiner is viewed from the same side where the image is displayed, information or scenery on the opposite side can be simultaneously viewed. That is, the combiner has the function of being an optical path combiner that displays the external light and the image light in an overlapping manner.
[0327] The projection image display part (superimposed image mirror) may be present on the entire surface of the windshield, or may be present on a portion relative to the entire area of the windshield. When it is a portion, the projection image display part may be set at any position of the windshield, but when used as a head-up display system, it is preferably set to display a virtual image at a position that is easily recognizable by an observer (e.g., a driver). For example, the position of setting the projection image display part may be determined based on the relationship between the position of the driver's seat of the applicable vehicle and the position where the projector is set.
[0328] The projection image display portion may be a flat surface without a curved surface, but may also have a curved surface, or may have a concave or convex shape as a whole, so as to display the projection image in an enlarged or reduced manner.
[0329] [Glass sheets for laminated glass]
[0330] In this specification, in a windshield, a glass plate on the visual recognition side is referred to as a first glass plate, and a glass plate located far from the visual recognition side is referred to as a second glass plate.
[0331] As the glass plate, a glass plate commonly used for windshields can be used. For example, a glass plate having a visible light transmittance of 73%, 76%, or 80% or less, such as green glass with high heat insulation, can be used. Even when such a glass plate with low visible light transmittance is used, by using the half mirror for projected image display used in the present invention, a windshield having a visible light transmittance of 70% or more in the projected image display portion can be manufactured.
[0332] In the laminated glass of the present invention, it is preferred that the two glass plates have curved surfaces, and it is particularly preferred that the surface of the glass plate on the half-mirror film side is a concave curved surface, as in the second embodiment of the laminated glass of the present invention. Figure 3 As shown, it is preferred that a half mirror film is closely bonded to the curved surface via a heat seal layer.
[0333] The laminated glass of the present invention is preferably used as a windshield.
[0334] The thickness of the glass plate is not particularly limited, but may be about 0.5 to 5.0 mm, preferably 1.0 to 3.0 mm, and more preferably 2.0 to 2.3 mm.
[0335] The materials and thicknesses of the first glass plate and the second glass plate may be the same or different.
[0336] (Intermediate film)
[0337] The intermediate film may be any known intermediate film used in known laminated glass. For example, a resin film containing a resin selected from the group consisting of polyvinyl butyral (PVB), ethylene vinyl acetate copolymer, and chlorine-containing resin may be used. Preferably, the above resin is the main component of the intermediate film. In addition, the main component refers to a component that accounts for 50% by mass or more of the intermediate film.
[0338] Among the above resins, polyvinyl butyral or ethylene vinyl acetate copolymer is preferred, and polyvinyl butyral is more preferred. The resin is preferably a synthetic resin.
[0339] Polyvinyl butyral can be obtained by acetalizing polyvinyl alcohol with butyraldehyde. The preferred lower limit of the acetalization degree of polyvinyl butyral is 40%, the preferred upper limit is 85%, the more preferred lower limit is 60%, and the more preferred upper limit is 75%.
[0340] Polyvinyl alcohol is generally obtained by saponifying polyvinyl acetate, and polyvinyl alcohol having a saponification degree of 80 to 99.8 mol % is generally used.
[0341] Furthermore, the preferred lower limit of the degree of polymerization of the polyvinyl alcohol is 200, and the preferred upper limit is 3000. If the degree of polymerization of the polyvinyl alcohol is 200 or more, the penetration resistance of the obtained laminated glass is not easily reduced, and if it is 3000 or less, the formability of the resin film is good, and the rigidity of the resin film does not become too large, and the processability is good. A more preferred lower limit is 500, and a more preferred upper limit is 2000.
[0342] As a preferred embodiment of the present invention, the half mirror film and the intermediate film are arranged in such a manner that all ends of the transparent support and all ends of the selective reflection layer are 5 mm or more inwardly disposed relative to the ends of the intermediate film, and then, the two glass plates, the half mirror film and the intermediate film are sealed while the transparent support is heated. The ends are sealed relative to the ends of the intermediate film by the intermediate film, and air intrusion from the side is suppressed, so that wrinkles are not generated.
[0343] All the ends of the transparent support and all the ends of the selective reflection layer are preferably located at least 10 mm inward from the ends of the intermediate film, and particularly preferably at least 15 mm inward.
[0344] (Intermediate film including half mirror film)
[0345] The laminated interlayer film for laminated glass including the half mirror film can be formed by laminating the half mirror film to the surface of the interlayer film. Alternatively, the half mirror film can be sandwiched between two interlayer films. The two interlayer films can be the same or different, but are preferably the same.
[0346] The half mirror film and the intermediate film may be laminated by a known lamination method, but lamination is preferably performed. When lamination is performed so that the laminate and the intermediate film do not peel off after processing, it is preferably performed under a certain degree of heating and pressurization.
[0347] In order to perform stable lamination, the film surface temperature of the adhesive side of the intermediate film is preferably 50 to 130°C, more preferably 70 to 100°C.
[0348] During lamination, it is preferred to apply pressure. The pressure condition is preferably less than 2.0 kg / cm 2 (less than 196 kPa), more preferably 0.5 to 1.8 kg / cm 2 (49 to 176 kPa), more preferably 0.5 to 1.5 kg / cm 2 (49~147kPa) range.
[0349] [Layer located on the visual recognition side relative to the selective reflection layer]
[0350] Typically, in a projection image display component, a ghosting (or multiple image) problem occurs due to the overlap of an image based on reflected light from a layer that reflects the projection light and an image based on reflected light from a surface near the front or a back side when viewed from the light incident side of the projection image display component.
[0351] In the laminated glass of the present invention, light passing through the selective reflection layer becomes circularly polarized light of a hand direction opposite to the circularly polarized light reflected by the selective reflection layer or becomes polarized light of a direction orthogonal to the linearly polarized light reflected by the selective reflection layer. When the layer located on the inner side of the selective reflection layer has low birefringence, most of the reflected light from the inner side usually becomes polarized light reflected by the selective reflection layer, so that it is difficult to generate a noticeable double image. In particular, by using polarized light as projection light, it is possible to configure that most of the projection light is reflected by the selective reflection layer.
[0352] On the other hand, the reflected light from the surface near the front side is likely to produce obvious double images. In particular, if the distance from the center of gravity of the selective reflection layer to the surface near the front side when observed from the light incident side of the laminated glass is a constant value or more, the double image is likely to become obvious. Specifically, in the structure of the laminated glass of the present invention, if the total thickness of the layer located closer to the first phase difference layer side than the selective reflection layer (excluding the thickness of the selective reflection layer), that is, the distance from the surface of the visual recognition side of the selective reflection layer to the surface of the visual recognition side of the laminated glass (windshield) becomes 0.5 mm or more, then the double image is likely to become obvious, if it is more than 1 mm, then it is likely to become more obvious, if it is more than 1.5 mm, then it is likely to become more obvious, if it is more than 2.0 mm, then it is likely to become particularly obvious. As a layer located closer to the visual recognition side than the selective reflection layer, in addition to the first phase difference layer, a support, an intermediate film, a second glass plate, etc. can also be cited.
[0353] However, in the laminated glass of the present invention, in projected image display using p-polarized light as described later, even when the total thickness of the layers located on the visual recognition side of the selective reflection layer is as described above, the projected image can be recognized without noticeable double images.
[0354] <Head-up display system (image display system)>
[0355] The laminated glass of the present invention can be used as a component of a head-up display system (image display system). As an example, the laminated glass of the present invention can be used as a windshield that constitutes a head-up display system in a vehicle, etc. The head-up display system preferably includes a projector.
[0356] Figure 7 2 , an example of a head-up display system using the laminated glass of the present invention as a windshield is conceptually shown. Figure 7 The example shown is Figure 2 The first embodiment of the laminated glass of the present invention shown is used as an example of laminated glass. The projector 100 projects an image from the first glass 6 side onto the windshield (laminated glass), and the user visually recognizes the image from the first glass 6 side.
[0357] in addition, Figure 7 In the example shown, Figure 2 The first embodiment of the laminated glass of the present invention shown in FIG. Figure 3 to Figure 6 When the second embodiment of the laminated glass of the present invention is used as laminated glass, a head-up display system can be similarly constituted. Figure 3 to Figure 6 In the case of the second embodiment of the laminated glass of the present invention shown above, as an example, an image is similarly projected from the first glass 6 side, and the image is visually recognized from the first glass 6 side.
[0358] [Projector]
[0359] In this specification, "projector" means "a device for projecting light or an image", including "a device for projecting a drawn image". In the head-up display system used in the present invention, the projector is configured to be able to project light incident on the windshield at the above-mentioned oblique incident angle using a half-reflecting mirror for displaying a projected image. In the head-up display system, the projector includes a drawing device, and preferably displays the image (real image) drawn on the small intermediate image screen as a virtual image through a combiner.
[0360] (Drawing equipment)
[0361] The drawing device may be a device that displays an image by itself, or may be a device that emits light that can draw an image. In the drawing device, the light from the light source may be adjusted by a drawing method such as a light modulator, a laser brightness modulation mechanism, or a light deflection mechanism for drawing. In this specification, the drawing device refers to a device that includes a light source and, depending on the drawing method, includes a light modulator, a laser brightness modulation mechanism, or a light deflection mechanism for drawing.
[0362] (light source)
[0363] The light source is not particularly limited, and can include LED (Light Emitting Diode), organic electroluminescent diode (OLED (Organic Light Emitting Diode)), discharge tube and laser light source. Among these, LED and discharge tube are preferred. This is because they are suitable for the light source of the drawing device that emits linear polarized light. Among these, LED is particularly preferred.
[0364] This is because the emission wavelength of the LED is not continuous in the visible light region and therefore is suitable for combination with a combiner using a cholesteric liquid crystal layer that shows selective reflection in a specific wavelength region as described later.
[0365] (Description method)
[0366] The drawing method can be selected according to the light source used, the application, etc., and is not particularly limited.
[0367] Examples of the drawing method include a fluorescent display tube, an LCD (Liquid Crystal Display) method using liquid crystal, an LCOS (Liquid Crystal on Silicon) method, a DLP (Digital Light Processing) method, and a scanning method using lasers. The drawing method may be a method using a fluorescent display tube integrated with a light source. As the drawing method, LCD is preferred.
[0368] In the LCD method and the LCOS method, light of each color is modulated and combined by a light modulator, and then emitted from a projection lens.
[0369] The DLP method uses a display system using a DMD (Digital Micromirror Device), which is equipped with micromirrors corresponding to several pixels for drawing and emits light from a projection lens.
[0370] The scanning method is a method of scanning a light beam on a screen and using the residual image of the eye to create an image. For example, the descriptions of Japanese Patent Application Laid-Open No. 7-270711 and Japanese Patent Application Laid-Open No. 2013-228674 can be referred to. In the scanning method using laser, laser beams of various colors (for example, red light, green light, and blue light) with modulated brightness are converged into one light beam through a multiplexing optical system or a focusing lens, and the light beam is scanned by a light deflection mechanism and drawn on an intermediate image screen described later.
[0371] In the scanning method, the brightness modulation of the laser beam of each color (for example, red light, green light, blue light) can be performed directly as a change in the intensity of the light source, or can be performed by an external modulator.
[0372] As the light deflection mechanism, a Galvano mirror, a combination of a Galvano mirror and a polygonal mirror, or MEMS (MicroElectro Mechanical Systems) can be cited, among which MEMS is preferred. As the scanning method, a random scanning method and a raster scanning method can be cited, and the raster scanning method is preferably used. In the raster scanning method, for example, the laser beam can be driven with a resonant frequency in the horizontal direction and with a sawtooth wave in the vertical direction. The scanning method does not require a projection lens, so the device can be easily miniaturized.
[0373] The light emitted from the drawing device may be linearly polarized light or natural light (non-polarized light).
[0374] The emitted light from the drawing device included in the head-up display system used in the present invention is preferably linearly polarized light. In the drawing device using LCD or LCOS as the drawing method and the drawing device using a laser light source, the emitted light is essentially linearly polarized light. When the drawing device is a device whose emitted light is linearly polarized light and the emitted light contains light of multiple wavelengths (colors), the polarization directions (transmission axis directions) of the polarized light of the multiple lights are preferably the same or orthogonal to each other. Regarding commercially available drawing devices, there are known drawing devices in which the polarization directions of the emitted light in the wavelength regions of red, green, and blue light are not uniform (refer to Japanese Patent Gazette No. 2000-221449). Specifically, there are known examples in which the polarization direction of green light is orthogonal to the polarization directions of red light and blue light.
[0375] (Intermediate Image Screen)
[0376] As described above, the drawing device may be a device using an intermediate image screen. In this specification, the "intermediate image screen" is a screen on which an image is drawn. That is, in a case where the light emitted from the drawing device is not yet recognizable as an image, the drawing device forms a recognizable image on the intermediate image screen using the light.
[0377] The image depicted on the intermediate image screen can be projected onto the combiner by light passing through the intermediate image screen, or can be projected onto the combiner by reflection from the intermediate image screen.
[0378] Examples of the intermediate image screen include a scattering film, a microlens array, and a screen for rear projection. When a plastic material is used as the intermediate image screen, if the intermediate image screen has birefringence, the polarization plane and light intensity of polarized light incident on the intermediate image screen are disturbed, and as a result, color unevenness is likely to occur in the combiner. However, the use of a phase difference layer having a predetermined phase difference can reduce the problem of color unevenness.
[0379] As the intermediate image screen, it is preferable to have a function of diffusing incident light to transmit it. This is because it can magnify and display the projected image. As such an intermediate image screen, for example, a screen composed of a microlens array can be cited. Regarding the microlens array used in the head-up display, for example, there are descriptions in Japanese Patent Publication No. 2012-226303, Japanese Patent Publication No. 2010-145745, and Japanese Patent Table No. 2007-523369.
[0380] The projector may include a reflecting mirror or the like for adjusting the optical path of the projection light formed by the drawing device.
[0381] For a head-up display system using a windshield as a member for projecting image display, reference can be made to Japanese Patent Application Laid-Open Nos. 2-141720, 10-096874, 2003-098470, U.S. Patent No. 5013134, and JP-A No. 2006-512622.
[0382] The laminated glass of the present invention is particularly useful in a windshield constituting a head-up display system, which is used in combination with a projector using a laser, LED, OLED, or the like whose emission wavelength is discontinuous in the visible light region as a light source. This is because the selective reflection center wavelength of the cholesteric liquid crystal layer can be adjusted in accordance with each emission wavelength. Furthermore, it can also be used for projection of a display such as an LCD (liquid crystal display) that displays polarized light.
[0383] [Projection light (incident light)]
[0384] By projecting an image from a p linearly polarized light source onto the laminated glass of the present invention, an image display system of the present invention can be obtained in which a viewer can visually recognize a reflected image. For example, when the laminated glass of the present invention is used for a windshield to constitute a head-up display system, by projecting an image from a p linearly polarized light source onto the windshield, an image display system of the present invention can be obtained in which a viewer can visually recognize a reflected image.
[0385] The direction in which p linear polarized light is incident is the direction in which the half mirror film built into the laminated glass functions as a reflective polarizer for linear polarized light. When the half mirror film has a selective reflection layer and a phase difference layer, the light source is configured so that p linear polarized light is incident from the phase difference layer side.
[0386] It is preferred that the incident light is incident at an oblique incident angle of 45° to 70° relative to the normal of the half-mirror for displaying the projected image. The Brewster angle of the interface between glass with a refractive index of about 1.51 and air with a refractive index of 1 is about 56°. By causing p-polarized light to be incident within the above-mentioned angle range, the following image display can be achieved, that is, the incident light for displaying the projected image has less reflected light from the windshield surface on the visual recognition side relative to the selective reflection layer, and the influence of ghosting is small. The above-mentioned angle is preferably 50° to 65°. At this time, any structure that can observe the projected image at an angle of 45° to 70°, preferably 50° to 65°, on the opposite side of the incident light relative to the normal of the selective reflection layer on the incident side of the projection light will suffice.
[0387] When the laminated glass of the present invention is used for a windshield, the incident light may enter the windshield from any direction such as up, down, left, or right, as long as it corresponds to the visual recognition direction. For example, it is preferably a structure in which the incident light enters from the bottom direction at the above-mentioned oblique incident angle when in use.
[0388] Furthermore, the slow axis of the retardation layer in the windshield is more preferably at an angle of 30° to 85° or 120° to 175° relative to the vibration direction of incident p-polarized light (incident plane of incident light), depending on the in-plane retardation of the retardation layer.
[0389] As described above, the projection light when displaying the projected image in the head-up display (the image display system of the present invention) is preferably p-polarized light vibrating in a direction parallel to the incident plane. When the emitted light of the projector is not linearly polarized light, it can be set to p-polarized light by configuring a linear polarizing film on the emitted light side of the projector, or it can be made into p-polarized light in the optical path from the projector to the windshield. As described above, for a projector whose emitted light has a non-uniform polarization direction in the wavelength region of red, green, and blue light, it is preferred to adjust the polarization direction in a wavelength-selective manner and make it incident as p-polarized light in the wavelength region of all colors.
[0390] The head-up display system may be a projection system in which the virtual image formation position is set to be variable. This projection system is described, for example, in Japanese Patent Publication No. 2009-150947. By setting the virtual image formation position to be variable, the driver can recognize the virtual image more comfortably and conveniently. The virtual image formation position is a position where the virtual image can be recognized from the driver of the vehicle, for example, a position more than 1000 mm away from the front of the windshield when usually viewed from the driver's side.
[0391] Among them, as described in the above-mentioned Japanese Patent Publication No. 2011-505330, if the glass is uneven (wedge-shaped) in the projection image display area, when changing the virtual image formation position, it is also necessary to change the angle of the wedge. Therefore, for example, as described in Japanese Patent Publication No. 2017-015902, it is necessary to change the projection position by partially changing the angle of the wedge, thereby simulating the change of the virtual image formation position.
[0392] In a head-up display system constructed using p-polarized light as described above and using the laminated glass of the present invention as a windshield, there is no need to use wedge-shaped glass, and the thickness of the glass can be made uniform in the projection image display area, so a projection system in which the above-mentioned virtual image formation position is set to be variable can be preferably used.
[0393] Example
[0394] Below, enumerate embodiment and reference example and the present invention is further specifically described.As long as do not depart from the purpose of the present invention, then the material, reagent, amount and ratio thereof, operation etc. shown in following embodiment, comparative example, preparation example can be appropriately changed.Therefore, the scope of the present invention is not limited to following embodiment and reference example.
[0395] <Preparation of coating solution>
[0396] (Coating liquid for forming cholesteric liquid crystal layer)
[0397] The following components were mixed to prepare coating solutions B, G, and R for forming a cholesteric liquid crystal layer having the following compositions.
[0398] ----------------------------------
[0399] Composition of coating liquid B
[0400] ----------------------------------
[0401] ·180 parts by mass of compound
[0402] ·Compound 220 parts by mass
[0403] · Fluorine compounds 10.02 parts by mass
[0404] ·30.01 parts by mass of fluorine compound
[0405] · Right-handed chiral reagent LC756 (manufactured by BASF)
[0406] Adjust according to the target reflection wavelength
[0407] ·Polymerization initiator IRGACURE OXE01 (manufactured by BASF) 0.75 parts by mass
[0408] Amount to make the concentration of the solvent (methyl acetate) dissolved matter 20% by mass
[0409] ----------------------------------
[0410] ----------------------------------
[0411] Composition of coating liquid G and R
[0412] ----------------------------------
[0413] ·Mixture 1100 parts by mass
[0414] · Fluorine compounds 10.05 parts by mass
[0415] · Fluorine compounds 20.04 parts by mass
[0416] · Right-handed chiral reagent LC756 (manufactured by BASF)
[0417] Adjust according to the target reflection wavelength
[0418] Polymerization initiator IRGACURE OXE01 (manufactured by BASF)
[0419] 1.0 parts by mass
[0420] Amount to make the concentration of the solvent (methyl ethyl ketone) 25% by mass
[0421] ----------------------------------
[0422] Mixture 1
[0423] [Chemical formula 6]
[0424]
[0425] Compound 1
[0426] [Chemical formula 7]
[0427]
[0428] Compound 2
[0429] [Chemical formula 8]
[0430]
[0431] Fluorine compounds 1
[0432] [Chemical formula 9]
[0433]
[0434] Fluorine compounds 2
[0435] [Chemical formula 10]
[0436]
[0437] ·Fluorine compounds 3
[0438] [Chemical formula 11]
[0439]
[0440] Coating solutions B, G and R were prepared by adjusting the formula amount of the chiral agent LC-756 in the above coating solution composition. Using each coating solution, a single-layer cholesteric liquid crystal layer was prepared on a peelable support in the same manner as when the following functional layer was prepared, and the reflection characteristics were confirmed. As a result, the prepared cholesteric liquid crystal layers were all right-handed circularly polarized light reflection layers, and the central reflection wavelength was as shown in Table 1 below.
[0441] [Table 1]
[0442] Coating liquid Central reflection wavelength Coating liquid B 515nm Coating liquid G 685nm Coating liquid R 775nm
[0443] (Coating liquid for forming phase difference layer)
[0444] The following components were mixed to prepare a coating liquid for forming a phase difference layer having the following composition.
[0445] ----------------------------------
[0446] Composition of coating liquid for forming phase difference layer
[0447] ----------------------------------
[0448] ·Mixture 1100 parts by mass
[0449] · Fluorine compounds 10.05 parts by mass
[0450] · Fluorine compound 20.01 parts by mass
[0451] Polymerization initiator IRGACURE OXE01 (manufactured by BASF)
[0452] 0.75 parts by mass
[0453] Amount to make the concentration of the solvent (methyl ethyl ketone) 25% by mass
[0454] ----------------------------------
[0455] <Saponification of Cellulose Acylate Film>
[0456] A 40 μm cellulose acylate film obtained by the same production method as Example 20 of International Publication No. 2014 / 112575 was passed through a dielectric heating roller at a temperature of 60° C., and the film surface temperature was raised to 40° C., and then coated with a bar coater at a coating amount of 14 mL / m 2 An alkaline solution having the composition shown below was applied to one side of the film, and the film was allowed to remain under a steam-type far-infrared heater (manufactured by Noritake Company, Limited) heated to 110° C. for 10 seconds.
[0457] Next, 3 mL / m 2 of pure water.
[0458] Next, after water washing with a jet coater and dehydration with an air knife were repeated three times, the film was allowed to stand in a drying zone at 70° C. for 5 seconds for drying, thereby producing a saponified cellulose acylate film 1 .
[0459] The in-plane phase difference of the cellulose acylate film 1 was measured by AxoScan and found to be 1 nm.
[0460] ----------------------------------
[0461] Composition of alkaline solution
[0462] ----------------------------------
[0463] Potassium hydroxide 4.7 parts by mass
[0464] · Water 15.7 parts by mass
[0465] · Isopropyl alcohol 64.8 parts by mass
[0466] Surfactant (C 16 H 33 O(CH2CH2O)10H) 1.0 parts by mass
[0467] Propylene glycol 14.9 parts by mass
[0468] ----------------------------------
[0469] <Formation of Orientation Film>
[0470] Use wire rod coater at 24mL / m 2 The saponified surface of the saponified cellulose acylate film 1 (transparent support) obtained above was coated with a coating liquid for forming an alignment film having the composition shown below, and dried with warm air at 100° C. for 120 seconds.
[0471] ----------------------------------
[0472] Composition of coating liquid for forming alignment film
[0473] ----------------------------------
[0474] · 28 parts by mass of the modified polyvinyl alcohol shown below
[0475] · Citrate ester (AS3, manufactured by Sankyo Kagaku Yakuhin Co., Ltd.) 1.2 parts by mass
[0476] Photopolymerization initiator (Irgacure 2959, manufactured by BASF) 0.84 parts by mass
[0477] Glutaraldehyde 2.8 parts by mass
[0478] · Water 699 parts by mass
[0479] Methanol 226 parts by mass
[0480] ----------------------------------
[0481] (Modified polyvinyl alcohol)
[0482] [Chemical formula 12]
[0483]
[0484] <Production of Cholesteric Liquid Crystal Layer Laminate>
[0485] The oriented film prepared above was subjected to a rubbing treatment (rayon cloth, pressure: 0.1 kgf (0.98 N), rotation speed: 1000 rpm, conveying speed: 10 m / min, number of times: 1 round trip) in a direction rotated 31.5° counterclockwise with respect to the short side direction.
[0486] After applying the coating liquid for forming a phase difference layer on the rubbed surface of the cellulose acylate film 1 by a wire bar, it was dried and heated at 55°C for 1 minute, placed on a hot plate at 50°C, and irradiated with ultraviolet rays for 6 seconds by an electrodeless lamp "D bulb" (60mW / cm) manufactured by Fusion UVSystems Ltd. to fix the liquid crystal phase and obtain a phase difference layer with a thickness of 1.9μm. At this time, the retardation and slow axis angle of the phase difference layer were measured by AxoScan, and the result was that the retardation was 349nm, and the slow axis angle was +58.5° relative to the vertical direction (short side direction) of the completed laminated glass.
[0487] After coating liquid B on the surface of the obtained phase difference layer using a wire rod, it was dried and heated at 85°C for 1 minute, placed on a hot plate at 80°C, and irradiated with ultraviolet rays for 6 seconds using an electrodeless lamp "D bulb" (60 mW / cm2) manufactured by Heraeus to fix the cholesteric liquid crystal phase and obtain a cholesteric liquid crystal layer with a thickness of 2.3 μm.
[0488] After further coating the coating liquid G on the surface of the obtained cholesteric liquid crystal layer using a wire rod, it was dried and heated at 70°C for 1 minute, placed on a hot plate at 75°C, and irradiated with ultraviolet rays for 6 seconds using an electrodeless lamp "D bulb" (60 mW / cm2) manufactured by Heraeus to fix the cholesteric liquid crystal phase and obtain a cholesteric liquid crystal layer with a thickness of 0.7 μm.
[0489] After further coating the coating liquid R on the surface of the obtained cholesteric liquid crystal layer using a wire rod, it was dried and heated at 70°C for 1 minute, placed on a hot plate at 75°C, and irradiated with ultraviolet rays for 6 seconds using an electrodeless lamp "D bulb" (60 mW / cm2) manufactured by Heraeus to fix the cholesteric liquid crystal phase and obtain a cholesteric liquid crystal layer with a thickness of 2.8 μm.
[0490] Thus, a cholesteric liquid crystal layer stack A (half-mirror film) having a functional layer consisting of a phase difference layer and three cholesteric liquid crystal layers was obtained. The transmission spectrum of the stack A was measured using a spectrophotometer (manufactured by JASCO Corporation, V-670), and as a result, a transmission spectrum having selective reflection center wavelengths at 515 nm, 685 nm, and 775 nm was obtained.
[0491] A cholesteric liquid crystal layer laminate B was prepared by the same procedure except that a PET film (Cosmo Shine A4100, thickness: 100 μm) manufactured by Toyobo Co., Ltd. was used as a transparent support. The PET film used as a transparent support has a primer layer on one side and a rubbing surface without a primer layer on the other side. A phase difference layer and a cholesteric liquid crystal layer were stacked on the rubbing surface of the PET film to obtain a cholesteric liquid crystal layer laminate B.
[0492] The in-plane retardation of the PET film at 550 nm was measured by AxoScan and found to be over 1000 nm.
[0493] <Production of heat seal layer 1>
[0494] (Coating liquid 1 for forming heat seal layer)
[0495] The following components were mixed to prepare heat seal layer-forming coating solutions 1 to 18 having the compositions shown in Table 2 below.
[0496]
[0497] <Preparation of Silica Particle Dispersion>
[0498] As inorganic fine particles preferably used as a heat seal layer in the present invention, AEROSIL RX300 (manufactured by NIPPON AEROSIL CO., LTD.) was added to MiBK (methyl isobutyl ketone) in a manner such that the solid content concentration was 5% by mass, and stirred for 30 minutes using a magnetic stirrer. Thereafter, ultrasonic dispersion was performed for 10 minutes using an ultrasonic disperser (manufactured by SMT Corporation, Ultrasonic Homogenizer UH-600S), thereby preparing a silica particle dispersion.
[0499] A portion of the obtained dispersion was collected for measurement of the average secondary particle size, and the average secondary particle size of the silica particles in the dispersion was measured using Microtrac MT3000 (manufactured by Microtrac BEL Corp.). As a result, the average secondary particle size was 190 nm.
[0500] As MEK-ST L (manufactured by NISSAN CHEMICAL INDUSTRIES. LTD.), a commercially available MEK dispersion (solid content concentration: 30% by mass) was used.
[0501] In the table, the amount of inorganic fine particles added is the amount of the dispersion added.
[0502] <Preparation of Heat-Sealable Laminate 1>
[0503] The coating liquids 1 to 18 for forming a heat seal layer were applied to the back side (the side not coated with cholesteric liquid crystal) of the cholesteric liquid crystal layer stack A using a wire bar, and then dried and heated at 50° C. for 1 minute to obtain heat seal layers 1 to 18 having a thickness of 0.5 μm. In this way, heat seal stacks Ah1 to 18 having a phase difference layer and three cholesteric liquid crystal layers (selective reflection layers) on one side of a transparent support and heat seal layers 1 to 18 on the other side of a transparent support were obtained.
[0504] The coating liquid 4 for forming a heat seal layer was applied to the back side of the cholesteric liquid crystal layer stack B (the side not coated with cholesteric liquid crystal and having the primer layer of the PET film) by using a wire bar, and then dried and heated at 50° C. for 1 minute to obtain a heat seal layer 18 having a thickness of 0.5 μm. In this way, a heat seal stack Ah19 having a functional layer composed of a phase difference layer and three cholesteric liquid crystal layers on the surface and a heat seal layer 18 on the back side was obtained.
[0505] <Production of laminated glass>
[0506] On a curved glass plate convex upwardly convexly 260 mm in length by 330 mm in width and 2 mm in thickness, heat-seal laminates Ah1 to 19 convexly 220 mm in length by 290 mm in width were arranged at the center of the glass plate with the heat-seal layer side facing downward. Thus, a laminate having the first glass plate, the heat-seal layer, the transparent support, the phase difference layer, and the selective reflection layer (cholesteric liquid crystal layer) in this order was formed.
[0507] A PVB film (intermediate film) manufactured by SEKISUI CHEMICAL CO., LTD., measuring 260 mm in length, 330 mm in width, and 0.38 mm in thickness, was placed on the laminate, and a curved glass plate (second glass plate) measuring 260 mm in length, 330 mm in width, and 2 mm in thickness, which was convex upward, was further placed on the laminate. After being kept at 90°C and 10 kPa (0.1 atmospheric pressure) for 1 hour, it was heated at 140°C and 1.3 MPa (13 atmospheric pressure) for 20 minutes in an autoclave (manufactured by KURIHARA company) to remove bubbles, thereby obtaining laminated glasses A to S. The laminated glasses A to S have the same Figure 2 Same layer structure of the laminated glass shown.
[0508] (Determination of storage modulus)
[0509] After conditioning the cellulose acylate film 1 used as a transparent support and a PET film (Cosmo Shine A4100, thickness: 100 μm) manufactured by Toyobo Co., Ltd. used as a transparent support at 25°C and a relative humidity of 60% for more than 2 hours, the storage modulus was measured using a dynamic viscoelasticity measuring apparatus (manufactured by IT Keisoku Seigyo Co., Ltd., Vibron: DVA-225) at a clamp distance of 20 mm, a heating rate of 2°C / min, a measuring temperature range of 30°C to 220°C, and a frequency of 1 Hz, and the storage modulus value at the set temperature of each autoclave was read.
[0510] (Evaluation of the presence or absence of a mixed layer between the heat seal layer and the transparent support)
[0511] The presence or absence of a mixed layer between the heat seal layer and the transparent support of the heat seal laminate was evaluated by observing the cross section of the heat seal laminate using SEM, and the presence or absence of the mixed layer was indicated in the table.
[0512] (Evaluation of Adhesion Between Heat Seal Layer and Transparent Support)
[0513] The adhesion between the heat seal layer of the heat seal laminate and the transparent support was tested by a cross-hatch method specified in JIS K5600-5-6, and the peelability from the transparent support was evaluated according to the following criteria.
[0514] The smaller the area of heat seal layer peeling, the less likely it is that the heat seal layer will peel off during the laminated glass manufacturing process, and the generation of micro wrinkles can be suppressed. In addition, the smaller the area of heat seal layer peeling, the stronger the laminated glass is, and it can withstand impact tests.
[0515] A: The area of the heat seal layer peeling off is 20% or less.
[0516] B: The area of the heat seal layer peeling off is more than 20 and less than 60%.
[0517] C: The area where the heat seal layer peeled off exceeded 60%.
[0518] (Evaluation of Adhesion of Heat Seal Layer to Glass (Adhesion))
[0519] For each laminate, the adhesion when laminating the surface opposite to the liquid crystal layer coating surface and glass was evaluated according to the following criteria: The less sticky feeling, the better the slipperiness, the better the handleability of the laminate during laminated glass processing, and the less likely wrinkles to form.
[0520] A: There is no stickiness at all.
[0521] B: Almost no stickiness.
[0522] C: Strong sense of adhesion.
[0523] (Evaluation of wrinkles)
[0524] Whether or not fine wrinkle-like unevenness was generated in the laminated body after the laminated glass was processed was evaluated by visual observation according to the following criteria.
[0525] A: There are no fine wrinkles at all.
[0526] B: There are no fine wrinkles but slight irregularities are visible.
[0527] C: Fine wrinkles were generated.
[0528] (Evaluation of image visibility)
[0529] Regarding image visibility, Figure 4 As shown, p-polarized light was irradiated onto the concave surface of the laminated glass to project an image, and the presence or absence of distortion and color unevenness of the generated virtual image was evaluated as image visibility based on the following criteria.
[0530] A: No distortion or uneven color.
[0531] C: Distortion and uneven color.
[0532] (Evaluation of haze of laminated glass)
[0533] The haze of each laminated glass was measured using a haze meter (Nippon Denshoku Industries Co., Ltd., haze meter NDH2000). The evaluation results were based on the following criteria.
[0534] A: 0.5 or less
[0535] B: 0.5 or more and 1.0 or less
[0536] C: 1.0 or above
[0537]
[0538] In the table, Re [nm] is the in-plane phase difference of the cellulose acylate film and the PET film as the transparent support.
[0539] Laminated glasses C to E, G to I, K to M, O to Q can be processed without producing fine wrinkle-like unevenness in the laminated body, and have good external light reflection and image visibility. In particular, laminated glasses H, I, L, M, P, and Q have good adhesion of the heat seal layer to the glass, so the workability during laminated glass processing is improved, and wrinkles are further improved.
[0540] In laminated glasses A and B, the adhesion between the heat seal layer and the cellulose acylate film was poor, resulting in fine wrinkle-like unevenness. In laminated glass S, the PET film (manufactured by Toyobo Co., Ltd., Cosmo Shine A4100, thickness: 100 μm) used as a transparent support had a large retardation, so rainbow-like color change patterns appeared in the external light reflection, which became a problem. In addition, the p-polarized light of the projected image was disturbed, and the light could not be efficiently reflected in the cholesteric liquid crystal layer, so the color tone of the visually recognized virtual image changed, and the brightness of the image decreased.
[0541] In addition, laminated glass S (reference example 19) does not have a mixed layer, but uses a PET film having a primer layer as a transparent support, and a heat-sealing layer is formed on the surface having the primer layer. Therefore, even if there is no mixed layer, high adhesion is obtained between the primer layer and the heat-sealing layer.
[0542] <Production of Cholesteric Liquid Crystal Layer Laminate 2>
[0543] The oriented film formed on the cellulose acylate film 1 was subjected to a rubbing treatment (rayon cloth, pressure: 0.1 kgf (0.98 N), rotation speed: 1000 rpm, conveying speed: 10 m / min, number of times: 1 round trip) in a direction rotated 31.5° counterclockwise with respect to the short side direction.
[0544] After applying the coating liquid for forming the phase difference layer on the rubbed surface with a wire rod, it was dried and heated at 55°C for 1 minute, placed on a hot plate at 50°C, and irradiated with ultraviolet light for 6 seconds by an electrodeless lamp "D bulb" (60mW / cm) manufactured by Fusion UV Systems Ltd. to fix the liquid crystal phase to obtain a phase difference layer with a thickness of 1.9μm. At this time, the delay and slow axis angle of the phase difference layer were measured using AxoScan (manufactured by Axometrics Inc.), and the result was that the delay was 349nm, and the slow axis angle was +58.5° relative to the vertical direction (short side direction) of the completed laminated glass.
[0545] After coating liquid B on the surface of the obtained phase difference layer using a wire rod, it was dried and heated at 85°C for 1 minute, placed on a hot plate at 80°C, and irradiated with ultraviolet rays for 6 seconds using an electrodeless lamp "D bulb" (60 mW / cm2) manufactured by Heraeus to fix the cholesteric liquid crystal phase and obtain a cholesteric liquid crystal layer with a thickness of 2.3 μm.
[0546] After further coating the coating liquid G on the surface of the obtained cholesteric liquid crystal layer using a wire rod, it was dried and heated at 70°C for 1 minute, placed on a hot plate at 75°C, and irradiated with ultraviolet rays for 6 seconds using an electrodeless lamp "D bulb" (60 mW / cm2) manufactured by Heraeus to fix the cholesteric liquid crystal phase and obtain a cholesteric liquid crystal layer with a thickness of 0.7 μm.
[0547] After further coating the coating liquid R on the surface of the obtained cholesteric liquid crystal layer using a wire rod, it was dried and heated at 70°C for 1 minute, placed on a hot plate at 75°C, and irradiated with ultraviolet rays for 1 second using an electrodeless lamp "D bulb" (60 mW / cm2) manufactured by Heraeus to fix the cholesteric liquid crystal phase and obtain a cholesteric liquid crystal layer with a thickness of 2.8 μm.
[0548] In this manner, a cholesteric liquid crystal layer stack C (half mirror film) having a phase difference layer and three cholesteric liquid crystal layers (selective reflection layers) was obtained.
[0549] The transmission spectrum of the laminate C was measured using a spectrophotometer (V-670 manufactured by JASCO Corporation). As a result, transmission spectra having selective reflection center wavelengths at 515 nm, 685 nm, and 775 nm were obtained.
[0550] <Production of heat seal layer 1>
[0551] (Coating liquid 1 for forming heat seal layer)
[0552] The following components were mixed to prepare heat seal layer-forming coating solutions 19 and 20 having the compositions shown in Table 4 below.
[0553] [Table 4]
[0554]
[0555] <Production of Heat-Sealable Laminate 2>
[0556] After applying the coating liquid 8 and 19 for forming a heat seal layer to the surface of the cholesteric liquid crystal layer stack A where the cholesteric liquid crystal layer is not formed using a wire bar, it was dried and heated at 120° C. for 5 minutes to obtain a heat seal layer with a thickness of 0.5 μm. In this way, heat seal stacks Bh1 and 2 having a phase difference layer and three cholesteric liquid crystal layers (selective reflection layers) on one surface of a transparent support and a heat seal layer on the other surface of the transparent support were obtained.
[0557] After the coating liquid 19 for forming a heat seal layer was applied to the cholesteric liquid crystal layer of the cholesteric liquid crystal layer stack C by a wire bar, it was dried and heated at 120° C. for 5 minutes to obtain a heat seal layer with a thickness of 0.5 μm. In this way, a heat seal stack Bh3 having a phase difference layer and three cholesteric liquid crystal layers (selective reflection layers) and a heat seal layer on the surface of a transparent support was obtained.
[0558] After applying the coating liquid 20 for forming a heat seal layer to the cholesteric liquid crystal layer of the cholesteric liquid crystal layer stack C using a wire rod, it was dried and subjected to a heat treatment at 120° C. for 5 minutes, and then placed on a hot plate at 75° C. and irradiated with ultraviolet light for 6 seconds using an electrodeless lamp "D bulb" (60 mW / cm) manufactured by Heraeus, thereby obtaining a heat seal layer with a thickness of 0.5 μm. In this way, a heat seal stack Bh4 having a phase difference layer and three cholesteric liquid crystal layers (selective reflection layers) and a heat seal layer on the surface of a transparent support was obtained.
[0559] <Production of laminated glass>
[0560] Laminated glass was produced using a 260mm long x 330mm wide, 2mm thick upwardly convex curved glass plate, a 260mm long x 330mm wide, 0.38mm thick PVB film (intermediate film) manufactured by SEKISUI CHEMICAL CO., LTD., and a 220mm long x 290mm wide heat-seal laminate Bh1 to 4.
[0561] First, laminated glasses 2A and 2B were produced.
[0562] Heat seal laminate Bh1, 2 is placed in the center of the curved glass plate (first glass plate) with the heat seal layer side facing downward, and an interlayer is placed thereon. A convex curved glass plate (second glass plate) with a length of 260 mm, a width of 330 mm, and a thickness of 2 mm is placed on this laminate.
[0563] After maintaining it at 90° C. and 10 kPa (0.1 atmosphere) for 1 hour, it was heated at 140° C. and 1.3 MPa (13 atmosphere) for 20 minutes in an autoclave (manufactured by KURIHARA company) to remove bubbles, thereby obtaining laminated glasses 2A and 2B.
[0564] They are all laminated glasses formed by sequentially layering a first glass plate, a heat sealing layer, a transparent support, a phase difference layer, a selective reflection layer (cholesteric liquid crystal layer), an intermediate film and a second glass plate. Figure 2 However, in the laminated glass 2B (heat-sealed laminate Bh2), no mixed layer is formed.
[0565] Next, laminated glasses 2C and 2D were produced.
[0566] An interlayer was placed in the center of the curved glass plate (first glass plate), and heat seal laminates Bh3 and 4 were placed thereon with the heat seal layer facing upward. Then, a second glass plate was bonded in the same manner as in the case of the laminated glass 2A, thereby obtaining laminated glasses 2C and 2D.
[0567] They are all laminated glasses formed by laminating a first glass plate, an intermediate film, a transparent support, a phase difference layer, a selective reflection layer (cholesteric liquid crystal layer), a heat sealing layer and a second glass plate in this order. Figure 3 Same layer structure of the laminated glass shown.
[0568] The produced heat-sealable laminate and laminated glass were evaluated in the same manner as above.
[0569] In addition, when evaluating the tightness of the heat-sealed laminate, for Examples B1 and B2 (laminated glass 2A and 2B), the tightness of the heat-sealed layer of the heat-sealed laminate and the transparent support was evaluated, and for Examples B3 and B4 (laminated glass 2C and 2D), the tightness of the heat-sealed layer of the heat-sealed laminate and the selective reflection layer (cholesteric liquid crystal layer) was evaluated.
[0570]
[0571] Laminated glasses 2A to 2D can be processed without producing fine wrinkle-like unevenness in the laminate, and have good external light reflection and image visibility. In particular, laminated glasses 2C and 2D have good adhesion to the glass due to the heat seal layer, so the operability during laminated glass processing is improved, and wrinkles are further improved.
[0572] In addition, the laminated glass 2D achieves good adhesion results due to the effect of the adhesion enhancer.
[0573] <Production of heat seal layer 2>
[0574] (Coating liquid 2 for forming heat seal layer)
[0575] The following components were mixed to prepare heat seal layer-forming coating solutions 21 to 25 having the compositions shown in Table 6 below.
[0576]
[0577] Adhesion enhancer 1 (compound having a polymerizable group and a boronic acid group)
[0578] [Chemical formula 13]
[0579]
[0580] Adhesion enhancer 2 (manufactured by TOSOH CORPORATION, CORONATE L: a compound having three isocyanate groups in one molecule)
[0581] Adhesion enhancer 3 (manufactured by Nippon Kayaku Co., Ltd., PET-30: a compound having 3 to 4 polymerizable groups in one molecule)
[0582] <Production of Heat-sealed Laminate 3>
[0583] After coating the heat seal layer-forming coating liquids 21 to 25 on the back side (the side not coated with cholesteric liquid crystal) of the cholesteric liquid crystal layer stack A with a wire bar, the coating liquids were dried and heated at 50° C. for 1 minute to obtain heat seal layers with thicknesses of 0.5 μm and 1.5 μm, respectively. In this way, heat seal stacks Ch1 to 10 having a phase difference layer and three cholesteric liquid crystal layers (selective reflection layers) on one side of a transparent support and a heat seal layer on the other side of a transparent support were obtained.
[0584] The evaluation of the adhesion between the heat seal layer and the transparent support of the heat seal laminates Ch1 to 10 was A in all cases.
[0585] <Production of laminated glass>
[0586] On a curved glass plate convex upward with a length of 260 mm × a width of 330 mm and a thickness of 2 mm, a heat-seal laminate Ch1 to 10 with a length of 220 mm × a width of 290 mm was arranged at the center of the glass plate with the heat-seal layer side facing downward. Next, a PVB film (intermediate film) manufactured by SEKISUI CHEMICAL CO., LTD with a length of 260 mm × a width of 330 mm and a thickness of 0.38 mm was arranged on the selective reflection layer of the heat-seal laminate. Thus, a laminate having the first glass plate, the heat-seal layer, the transparent support, the phase difference layer, the selective reflection layer (cholesteric liquid crystal layer) and the intermediate film in this order was formed.
[0587] A convex curved glass plate (second glass plate) with a length of 260 mm × a width of 330 mm and a thickness of 2 mm was further arranged on the laminate. After being kept at 90° C. and 10 kPa (0.1 atmospheric pressure) for 1 hour, it was heated at 140° C. and 1.3 MPa (13 atmospheric pressure) for 20 minutes in an autoclave (manufactured by KURIHARA company) to remove bubbles, thereby obtaining laminated glasses 3A to 3J.
[0588] The produced laminated glass was evaluated in the same manner as before.
[0589] In addition, the laminated glasses 3A to 3J basically have the same Figure 2 Same layer structure of the laminated glass shown.
[0590]
[0591] The laminated glasses 3A to 3J can be processed into laminated glasses without causing fine wrinkle-like unevenness in the laminated body, and have good external light reflection and image visibility.
[0592] <Production of heat seal layer 3>
[0593] (Preparation of coating solution for forming heat seal layer)
[0594] The following components were mixed to prepare heat seal layer-forming coating solutions 26 to 29 having the compositions shown in Table 8 below.
[0595] In addition, when preparing the coating liquid for forming a heat seal layer, the following materials were used.
[0596] ESREC KS-5 (manufactured by SEKISUI CHEMICAL CO., LTD.)
[0597] [Chemical formula 14]
[0598]
[0599] Here, 1 is 74±3, m is 3 or less, n is about 25, and the calculated molecular weight is about 130,000.
[0600] ESREC KS-10 (manufactured by SEKISUI CHEMICAL CO., LTD.)
[0601] [Chemical formula 15]
[0602]
[0603] Here, 1 is 74±3, m is 3 or less, n is about 25, and the calculated molecular weight is about 17,000.
[0604] As a cross-linking agent (epoxy-based additive) for the resin of the heat seal layer, Denacol EX832 (manufactured by Nagase ChemteX Corporation) was used.
[0605] [Chemical formula 16]
[0606]
[0607] Cationic polymerization initiator 1
[0608] [Chemical formula 17]
[0609]
[0610]
[0611] <Preparation of Heat-Sealable Laminates Dh1 to 4>
[0612] The heat seal layer forming coating liquids 26 to 29 were applied to the back side (the side not coated with cholesteric liquid crystal) of the cholesteric liquid crystal layer stack A using a wire bar, dried, and heated at 50°C for 1 minute to obtain heat seal layers 26 to 29 with a thickness of 0.5 μm.
[0613] Furthermore, the heat seal layer 29 was irradiated with ultraviolet rays for 33 seconds at room temperature in a nitrogen atmosphere using an electrodeless lamp "D bulb" (60 mW / cm) manufactured by Heraeus.
[0614] Thus, heat-seal laminated bodies Dh1 to Dh4 were obtained, each having a retardation layer and three cholesteric liquid crystal layers (selective reflection layers) on one surface of a transparent support and heat-seal layers 26 to 29 on the other surface of the transparent support.
[0615] <Production of laminated glass>
[0616] On a 260 mm long x 330 mm wide curved glass plate with a thickness of 2 mm and convex upward, heat-seal laminates Dh1 to 4 with a length of 220 mm x a width of 290 mm were arranged in the center of the glass plate with the heat-seal layer side facing downward. Thus, a laminate having the first glass plate, the heat-seal layer, the transparent support, the phase difference layer and the selective reflection layer (cholesteric liquid crystal layer) in this order was formed.
[0617] A 0.38 mm thick PVB film (intermediate film) manufactured by SEKISUI CHEMICAL CO., LTD. with a length of 260 mm and a width of 330 mm was placed on the selective reflection layer, and a 2 mm thick curved glass plate (second glass plate) with a length of 260 mm and a width of 330 mm was further placed thereon. After being kept at 90° C. and 10 kPa (0.1 atmosphere) for 1 hour, it was heated at 140° C. and 1.3 MPa (13 atmosphere) for 20 minutes in an autoclave (manufactured by KURIHARA company) to remove bubbles, thereby obtaining laminated glasses 4A to 4D.
[0618] In addition, the laminated glasses 4A to 4D have Figure 2 Same layer structure of the laminated glass shown.
[0619] The heat-sealed laminate and laminated glass thus prepared were evaluated in the same manner as above. As shown in Table 9 below, good results were obtained.
[0620]
[0621] Explanation of symbols
[0622] 1-transparent support, 2-phase difference layer, 3-selective reflection layer, 4-heat sealing layer, 5-intermediate film, 6-first glass plate, 7-second glass plate, 10-half mirror film, 100-projector (p-polarized light image).
Claims
1. A laminated glass for projected image display, wherein: The half mirror film and the intermediate film are sandwiched between a glass plate on the half mirror film side and a glass plate on the intermediate film side. A heat seal layer containing a thermoplastic resin and having a thickness of 0.1 μm to 10 μm is provided between the half mirror film and the glass plate on the half mirror side. The half mirror film has a selective reflection layer and a phase difference layer that show selective reflection in a part of the visible light wavelength region. The heat seal layer contains inorganic fine particles formed into secondary particles, wherein the secondary particles are formed by agglomeration of primary particles having an average primary particle diameter of 5 to 50 nm. The inorganic fine particles include at least one selected from the group consisting of silicon dioxide, aluminum oxide, titanium dioxide, zirconium oxide, calcium carbonate, talc, clay, calcined kaolin, calcined calcium silicate, hydrated calcium silicate, aluminum silicate, magnesium silicate and calcium phosphate.
2. The laminated glass for projected image display according to claim 1, wherein: The heat sealing layer is adjacent to the selective reflection layer or the phase difference layer.
3. The laminated glass for projected image display according to claim 2, wherein: The heat seal layer is adjacent to the selective reflection layer.
4. The laminated glass for projected image display according to any one of claims 1 to 3, wherein: The central wavelength of selective reflection of the selective reflection layer having a central wavelength of selective reflection at the shortest wavelength is 650 to 780 nm.
5. The laminated glass for projected image display according to any one of claims 1 to 3, wherein: The in-plane phase difference of the phase difference layer at a wavelength of 550 nm is 50 to 180 nm.
6. The laminated glass for projected image display according to any one of claims 1 to 3, wherein: The amount of the inorganic fine particles in the coating composition of the heat seal layer is 1 to 40% by mass based on the total solid content of the heat seal layer.
7. The laminated glass for projected image display according to any one of claims 1 to 3, wherein: It also has a transparent support body adjacent to the heat-sealing layer, The coating composition for forming the heat seal layer contains 30 to 70% by mass of at least one solvent having permeability to the transparent support, based on the total amount of the solvent.
8. The laminated glass for projected image display according to claim 7, wherein: The absolute value of the in-plane phase difference of the transparent support at a wavelength of 550 nm is 10 nm or less.
9. The laminated glass for projected image display according to any one of claims 1 to 3, wherein: The intermediate film is a resin film containing a resin selected from the group consisting of polyvinyl butyral (PVB), ethylene vinyl acetate copolymer, and chlorine-containing resin.
10. The laminated glass for projected image display according to any one of claims 1 to 3, wherein: The thickness of the heat-sealing layer is 0.1-5.0 μm.
11. An image display system, wherein: An image is projected from a p-linearly polarized light source onto the laminated glass for projection image display according to any one of claims 1 to 10.