Prediction and control method of metal streamlines in space envelope forming of thin-walled high-rib components

By designing convergent flash forgings and calculating the position of the splitting surface, the problem of metal streamline prediction and control in the spatial envelope forming of thin-walled and highly reinforced components is solved, achieving high-performance and efficient forming manufacturing and ensuring the mechanical properties of the components. and carrying capacity.

CN114239178BActive Publication Date: 2024-10-29WUHAN UNIV OF TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202111559419.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-20
Publication Date
2024-10-29
Estimated Expiration
2041-12-20

AI Technical Summary

Technical Problem

The existing technology cannot effectively predict and control the metal streamlines of thin-walled high-reinforced components during the spatial envelope forming process, causing the metal streamlines to penetrate the reinforcements, seriously weakening the mechanical properties and load-bearing capacity of the components, and unable to meet the needs of new large-capacity long-range voyages. Rigorous requirements for carrying equipment.

Method used

By designing forgings with convergent horizontal flash, the equilibrium differential equation, static equilibrium equation and yield equation are listed, the vertical stress distribution and the position of the splitting surface are calculated, and the inclination angle of the flash is controlled to ensure symmetry of the splitting surfaces on both sides of the high rib. Achieve accurate prediction and control of metal streamlines.

Benefits of technology

It achieves high-performance and efficient forming and manufacturing of thin-walled high-reinforced components, ensures continuous dense and symmetrical distribution of metal streamlines, improves the mechanical properties and load-bearing capacity of components, and reduces design costs and manufacturing difficulty.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114239178B_ABST
    Figure CN114239178B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for predicting and controlling metal streamlines in space envelope forming of thin-walled high-rib components, comprising the following steps: S1, forging design; S2, listing equilibrium differential equations; S3, listing static equilibrium equations; S4, listing geometric relationships of inclined flash edges; S5, listing yield equations of primitive bodies at the web; S6, calculating vertical stress distributions in different regions of the blank; S7, calculating the positions of the left and right side flow dividers of the high ribs; S8, calculating the instantaneous increment of the left flash length and the instantaneous increment of the right flash length; S9, calculating the updated instantaneous increment of the left flash length and the instantaneous increment of the right flash length; S10, calculating the difference between the distances of the left and right flow dividers and the high-rib symmetry line at any time. The present invention can realize accurate prediction and control of metal streamlines in space envelope forming of thin-walled high-rib components, obtain continuous, dense and symmetrically distributed metal streamlines, ensure the mechanical properties and bearing capacity of thin-walled high-rib components, and realize high-performance space envelope forming manufacturing of thin-walled high-rib components.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of space envelope forming, and more specifically to a method for predicting and controlling metal streamlines in space envelope forming of thin-walled high-rib components. Background Art

[0002] As transport equipment is developing towards large capacity and long range, it is urgent to use lightweight and high-load bearing components. Thin-walled high-rib components are light in weight and high in rigidity and strength. They are the main load-bearing components of transport equipment and are widely used to manufacture aircraft bulkheads and skins. At present, milling is mainly used to manufacture thin-walled high-rib components. This manufacturing method has large material waste, low efficiency, and poor performance, and cannot meet the stringent requirements of the service performance of new large-capacity and long-range transport equipment.

[0003] Space envelope forming is a new process based on the envelope motion relationship between the three-dimensional motion trajectory of the envelope die and the upper surface of the blank. The blank undergoes incremental deformation under the action of multiple enveloping rolling between the lower die and the envelope die until the thin-walled high-ribbed component is formed as a whole. It has significant advantages such as high forming accuracy, good forming performance, low forming force, and high forming efficiency. It has become the frontier development direction of high-performance and high-efficiency thin-walled high-ribbed component manufacturing technology for carrier equipment. However, the thin-walled high-ribbed component has a thin web, high and thin ribs, and an extreme geometric structure. The metal flow during its space envelope forming process is very complex. It is very easy for the web metal to flow from one side of the rib to the other side, and the metal streamlines to penetrate the ribs, which seriously weakens the mechanical properties and bearing capacity of the thin-walled high-ribbed component, thus causing the thin-walled high-ribbed component to be scrapped. Therefore, accurately predicting and controlling the metal streamlines and obtaining continuous, dense, and symmetrically distributed metal streamlines are the prerequisites for realizing space envelope forming of thin-walled high-ribbed components. At present, there is no report on the prediction and control method of metal streamlines in space envelope forming of thin-walled high-ribbed components. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a method for predicting and controlling metal streamlines in the spatial envelope forming of thin-walled high-rib components, which can achieve high-performance and high-efficiency forming and manufacturing of thin-walled high-rib components.

[0005] The technical solution adopted by the present invention to solve its technical problems is: construct a metal streamline prediction and control method for spatial envelope forming of thin-walled high-rib component, including the following steps: S1, forging design: set a convergent horizontal flash on the left web of the thin-walled high-rib component, set a horizontal flash on the right web of the thin-walled high-rib component, the flash thickness is equal to the web thickness of the thin-walled high-rib component, and the thin-walled high-rib component after adding the left and right flashes is a forging; S2, according to the force balance relationship of the primitive body in the horizontal direction at the web, list the equilibrium differential equation; S3, according to the static balance relationship of the primitive body at the web, list the static balance equation; S4, list the geometric relationship of the inclined flash; S5, list the yield equation of the primitive body at the web; S6, calculate the vertical stress distribution in different areas of the blank; S7, calculate the position of the left and right diversion surfaces of the high rib; S8, calculate the instantaneous increment L of the left flash length ti1 and the instantaneous increment of the right flash length L ti2 ; S9, calculate the updated left flash length instantaneous increment L ti1 and the instantaneous increment of the right flash length L ti2 ; S10, calculate the difference in distance between the left and right side diversion surfaces and the high-rib symmetry line at any time, and adjust the inclination angle of the convergent fin so that the difference is equal to 0.

[0006] According to the above scheme, in step S2, the equilibrium differential equation is as described in equation (1):

[0007] σ x h-(σ x +dσ x )(h+2tanαdx)-2τdx+2σ u tanαdx=0 (1)

[0008] where σ x is the horizontal stress, h is the height of the unit body, dx is the width of the unit body, α is the inclination angle of the convergent flash edge, τ is the shear stress, σ u is the stress in the inclined direction.

[0009] According to the above scheme, in step S3, the static equilibrium equation is as described in equation (2):

[0010] σ u =σ y -τtanα (2)

[0011] where σ y is the vertical stress.

[0012] According to the above scheme, in step S4, the geometric relationship of the inclined flash edge is as described in equation (3):

[0013] h=H-vt i +2xtanα (3)

[0014] Where H is the initial thickness of the blank, v is the die feed rate, and t i is the instantaneous forming time, i is the time variable, i = 0, 1, 2... n, and x is the horizontal distance between the elementary volume and the starting end of the inclined flash.

[0015] According to the above scheme, in the step S5, the yield equation is as described in Equation (4):

[0016] σ y -σ x = 2k (4)

[0017] Where k is the shear yield strength.

[0018] According to the above scheme, in the step S6, the above Equations (1), (2), (3), and (4) are联立, and the stress boundary conditions are substituted: when x = x e σ y = σ ye , and the vertical stress distribution in different regions of the blank is obtained by using the principal stress method, as described in Equation (5):

[0019]

[0020] Where m is the friction factor.

[0021] According to the above scheme, in the step S7, the real-time split surface position is determined according to the vertical stress distribution on both sides of the split surface being equal at the split surface. From Equation (5), it can be obtained that when the left split surface of the high rib satisfies x i1 < L0, the position x i1 of the left split surface of the high rib is as described in Equation (6):

[0022]

[0023] Where L0 is the initial distance between the high rib and the left end of the blank, and L Si1 is the instantaneous length of the left flash;

[0024] From Equation (5), it can be obtained that when the left split surface of the high rib satisfies x i1 > L0, the position x i1 of the left split surface of the high rib is as described in Equation (7):

[0025]

[0026] From Equation (5), it can be obtained that the position x i2 of the right split surface of the high rib is as described in Equation (8):

[0027]

[0028] Where b is the rib width, L is the initial width of the blank, and L Si2 is the instantaneous length of the right side flash;

[0029] According to the above scheme, in step S8, the real-time metal volume distribution is completed according to the real-time diversion surface position, and the left flash length instantaneous increment L ti1 and the instantaneous increment of the right flash length L ti2 As described in equation (9) and equation (10) respectively:

[0030] (L ti1 tanα+2L Si1 tanα+H-vt i )L ti1 =(L Si1 +L0-x i1 )vΔt (9)

[0031]

[0032] Where Δt is the instantaneous increment of forming time;

[0033] According to the above scheme, in step S9, according to the instantaneous increment L of the left and right flash edges, ti1 and L ti2 Update the deformed blank shape and the new left flash instantaneous length L Si1 and the new instantaneous length L of the right flash edge Si2 As described in equation (11):

[0034]

[0035] Repeat the above process from S1 to S10 until the spatial envelope is formed and multiple groups of x are obtained. i1 and x i2 The value of .

[0036] According to the above scheme, in step S10, a function is defined to represent the difference between the distances between the left and right side flow dividing surfaces and the high rib symmetry line at any time, as described in equation (12):

[0037] f(x)=x i2 -x i1 (12)

[0038] The α value is adjusted so that f(x) is equal to 0, that is, the volume of metal extruded into the high ribs on the left and right sides is equal, so as to obtain high-quality metal streamlines for spatial envelope forming of thin-walled high-rib components, thereby achieving precise control of metal streamlines for spatial envelope forming of thin-walled high-rib components.

[0039] The present invention determines the prediction and control principle of metal streamlines for space envelope forming of thin-walled high-rib components as follows:

[0040] In the spatial enveloping forming, the lower die and the blank are actively fed along the vertical axis to approach the enveloping die. The conical enveloping die actively swings around its cone apex and contacts the upper surface of the blank. The motion trajectory of the enveloping die forms an enveloping motion relationship with the upper surface of the blank. The blank undergoes incremental deformation under the multiple enveloping rolling action of the lower die and the enveloping die. The three-way flow of the slab metal realizes the thinning of the web and the thickening of the ribs until the thin-walled high-rib component is nearly net-formed as a whole. In the spatial enveloping forming of thin-walled high-rib components, if the position of the web diverter surface on both sides of the ribs is asymmetrical, the web metal flows from one side of the ribs to the other side, the metal streamlines penetrate the ribs, and the thin-walled high-rib components are scrapped. The position of the web diverter surface on both sides of the ribs can be calculated to predict the metal streamlines of the spatial enveloping forming of thin-walled high-rib components. The position of the web diverter surface on both sides of the ribs is optimized to ensure the symmetry of the web diverter surface on both sides of the ribs, thereby ensuring that the metal streamlines do not penetrate the ribs, and the metal streamlines of the spatial enveloping forming of thin-walled high-rib components can be effectively controlled.

[0041] The implementation of the metal streamline prediction and control method for space envelope forming of thin-walled high-rib component of the present invention has the following beneficial effects:

[0042] (1) The present invention can achieve accurate prediction and control of metal streamlines in the spatial envelope forming of thin-walled high-ribbed components, obtain continuous, dense and symmetrically distributed metal streamlines, and further ensure the mechanical properties and bearing capacity of thin-walled high-ribbed components, thereby realizing high-performance thin-walled high-ribbed components spatial envelope forming manufacturing.

[0043] (2) The present invention can quickly realize the accurate prediction and control of metal streamlines in the spatial envelope forming of thin-walled high-rib components, thereby improving the design efficiency of the spatial envelope forming process of thin-walled high-rib components and reducing the design cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] The present invention will be further described below with reference to the accompanying drawings and embodiments, in which:

[0045] Figure 1 It is a schematic diagram of the axial section of the thin-walled high-rib component to be formed;

[0046] Figure 2 is a schematic diagram of the blank;

[0047] Figure 3 It is a schematic diagram of the design of convergent fins on the left and open fins on the right;

[0048] Figure 4 It is a schematic diagram of mechanical analysis of inclined flash;

[0049] Figure 5 It is a polyline inclined flash edge generated by combining multiple obtained α values;

[0050] Figure 6 This is a partial enlarged view of the inclined flash edge of the polyline;

[0051] Figure 7 It is the simulation result of metal streamline without metal streamline control;

[0052] Figure 8 This is the metal streamline simulation result under metal streamline control. DETAILED DESCRIPTION

[0053] In order to have a clearer understanding of the technical features, purposes and effects of the present invention, specific embodiments of the present invention are now described in detail with reference to the accompanying drawings.

[0054] The thin-walled high-rib component of the present invention is composed of a web and high ribs. Figure 1 The schematic diagram of the axial section of the thin-walled high-rib component to be formed is shown in Figure 1. Its width is 48 mm, the web thickness is 4 mm, the rib height is 10 mm, the rib thickness is 6 mm, and the initial distance between the high rib and the left end of the blank is 16 mm. Figure 1 shown.

[0055] S1. Determine the prediction and control principle of metal streamlines in spatial envelope forming of thin-walled high-rib components: In spatial envelope forming, the lower die and the blank are actively fed along the vertical axis to approach the envelope die, the conical envelope die actively swings around its cone apex and contacts the upper surface of the blank, the motion trajectory of the envelope die and the upper surface of the blank form an envelope motion relationship, the blank undergoes incremental deformation under the multiple-pass enveloping rolling action of the lower die and the envelope die, the three-way flow of the slab metal realizes web thinning and rib thickening, until the thin-walled high-rib component is nearly net-formed as a whole. In the spatial envelope forming of thin-walled high-rib components, if the position of the web diverter surfaces on both sides of the ribs is asymmetrical, the web metal flows from one side of the ribs to the other, the metal streamlines penetrate the ribs, and the thin-walled high-rib components are scrapped. Calculating the position of the web diverter surfaces on both sides of the ribs can realize the prediction of metal streamlines in spatial envelope forming of thin-walled high-rib components. The positions of the web diverter surfaces on both sides of the high ribs are optimized to ensure symmetry of the web diverter surfaces on both sides of the high ribs, thereby ensuring that the metal streamlines do not penetrate the ribs, and effectively controlling the metal streamlines of the spatial envelope forming of thin-walled high-rib components.

[0056] S2. Forging design: a convergent horizontal burr is set on the left web of the thin-walled high-ribbed component, and a horizontal burr is set on the right web of the thin-walled high-ribbed component. The burr thickness is equal to the web thickness of the thin-walled high-ribbed component. The thin-walled high-ribbed component with the left and right burrs added is a forging.

[0057] S3. According to the force balance relationship of the element body in the horizontal direction at the web, the equilibrium differential equation is listed, as described in equation (1):

[0058] σ x h-(σ x +dσ x )(h+2tanαdx)-2τdx+2σ u tanαdx=0 (1)

[0059] where σ x is the horizontal stress, h is the height of the unit body, dx is the width of the unit body, α is the inclination angle of the convergent flash edge, τ is the shear stress, σ u is the stress in the tilt direction;

[0060] S4. According to the static equilibrium relationship of the basic body at the web, the static equilibrium equation is listed, as described in equation (2):

[0061] σ u =σ y -τtanα (2)

[0062] where σ y is the vertical stress;

[0063] S5. According to the geometric relationship of the inclined flash edge, as described in equation (3):

[0064] h=H-vt i +2xtanα (3)

[0065] Where H is the initial thickness of the blank, which is 6 mm in this embodiment, v is the die feed speed, which is 2 mm / s in this embodiment, and t i is the instantaneous forming moment, i is the time variable, i=0,1,2……n, x is the horizontal distance between the primitive body and the starting end of the inclined flash edge;

[0066] S6. Since the web element is subjected to vertical compression and horizontal tension, its yield equation is listed as described in equation (4):

[0067] σ y -σ x =2k (4)

[0068] Where k is the shear yield strength;

[0069] S7. Combine the above equations (1), (2), (3) and (4) and substitute the stress boundary conditions: when x = x e When y =σ ye , the principal stress method is used to obtain the vertical stress distribution in different regions of the blank, as described in equation (5):

[0070]

[0071] Where m is the friction factor, which is 0.3 in this embodiment;

[0072] S8. According to the vertical stress distribution on both sides of the diverter surface, the vertical stress is equal at the diverter surface to determine the real-time diverter surface position. From equation (5), it can be obtained that when the diverter surface on the left side of the high rib meets x i1When L0, the position x of the left shunting surface of the high rib i1 As described in Equation (6):

[0073]

[0074] where L0 is the initial distance between the high rib and the left end of the blank, taken as 16 mm in this embodiment, and L Si1 is the instantaneous length of the left flash;

[0075] It can be obtained from Equation (5) that when the left shunting surface of the high rib satisfies x i1 > L0, the position x of the left shunting surface of the high rib i1 As described in Equation (7):

[0076]

[0077] It can be obtained from Equation (5) that the position x of the right shunting surface of the high rib i2 As described in Equation (8):

[0078]

[0079] where b is the rib width, taken as 6 mm in this embodiment, L is the initial width of the blank, taken as 45 mm in this embodiment, and L Si2 is the instantaneous length of the right flash;

[0080] S9. Complete the real-time metal volume distribution according to the real-time shunting surface position. The instantaneous increment L ti1 of the left flash length and the instantaneous increment L ti2 of the right flash length are respectively as described in Equation (9) and Equation (10):

[0081] (L ti1 tanα + 2L Si1 tanα + H - vt i )L ti1 = (L Si1 + L0 - x i1 )vΔt (9)

[0082]

[0083] where Δt is the instantaneous increment of the forming time, taken as 0.01 s in this embodiment;

[0084] S10. Update the shape of the deformed blank according to the instantaneous increments L ti1 and L ti2 of the left and right flashes. The new instantaneous length L Si1 of the left flash and the new instantaneous length L Si2 of the right flash are as described in Equation (11):

[0085]

[0086] Repeat the above process from S1 to S10 until the spatial envelope is formed and multiple groups of x are obtained. i1 and x i2 The value of

[0087] S11. Define a function to represent the difference in distance between the left and right side flow dividers and the high rib symmetry line at any time, as described in equation (12):

[0088] f(x)=x i2 -x i1 (12)

[0089] The α value is adjusted so that f(x) is equal to 0, that is, the volume of metal extruded into the high ribs on the left and right sides is equal, so as to obtain high-quality metal streamlines for spatial envelope forming of thin-walled high-rib components, thereby achieving precise control of metal streamlines for spatial envelope forming of thin-walled high-rib components. Figure 7 is the metal streamline simulation result without metal streamline control. Figure 7 It can be seen that the web metal flows from the right side of the rib to the left side, and the metal streamline ( Figure 7 The black line in the figure is to the left (the red line is the high-rib symmetry line. If the black line coincides with or is close to the red line, it indicates that the metal streamline is intact, otherwise the metal streamline is unreasonable), and reinforcement penetration occurs, resulting in the scrapping of the thin-walled high-rib component. Figure 8 This is the metal streamline simulation result under metal streamline control. Figure 8 It can be seen that the metal flow line ( Figure 8 The black line in the figure is almost coincident with the red line, indicating that the metal streamline is intact, thus proving that the metal streamline prediction and control method for space envelope forming of thin-walled high-rib component proposed in the present invention is effective.

[0090] The embodiments of the present invention are described above in conjunction with the accompanying drawings, but the present invention is not limited to the above-mentioned specific implementation methods. The above-mentioned specific implementation methods are merely illustrative and not restrictive. Under the enlightenment of the present invention, ordinary technicians in this field can also make many forms without departing from the scope of protection of the purpose of the present invention and the claims, which all fall within the protection of the present invention.

Claims

1. A method for predicting and controlling metal streamlines in space envelope forming of thin-walled high-rib components, characterized in that: The following steps are involved: S1. Forging design: set a convergent horizontal burr on the left web of the thin-walled high-ribbed component, and set a horizontal burr on the right web of the thin-walled high-ribbed component. The burr thickness is equal to the web thickness of the thin-walled high-ribbed component. The thin-walled high-ribbed component with the left and right burrs added is a forging; S2. List the equilibrium differential equation based on the force balance relationship of the primitive body in the horizontal direction at the web; S3. List the static equilibrium equation based on the static equilibrium relationship of the primitive body at the web; S4. List the geometric relationship of the inclined burr; S5. List the yield equation of the primitive body at the web; S6. Calculate the vertical stress distribution in different areas of the billet; S7. Calculate the position of the diversion surface on the left and right sides of the high rib; S8. Calculate the instantaneous increment of the left burr length L ti1 and the instantaneous increment of the right flash length L ti2 ; S9, calculate the updated instantaneous increment of the left flash length L ti1 and the instantaneous increment of the right flash length L ti2 ; S10, calculate the difference between the distances between the left and right side diversion surfaces and the high rib symmetry line at any time, and adjust the inclination angle of the convergent fin so that the difference is equal to 0; In step S2, the balanced differential equation is as described in equation (1): (1) in σ x is the horizontal stress, h is the height of the primitive, dx is the primitive width, α is the inclination angle of the convergent fin, τ is the shear stress, σ u is the stress in the tilt direction; In step S3, the static equilibrium equation is as described in equation (2): (2) in σ y is the vertical stress; In step S4, the geometric relationship of the inclined flash edge is as described in equation (3): (3) in H is the initial thickness of the blank, v is the die feed speed, t i is the instant forming moment, i is the time variable, i =0,1,2…… n , x is the horizontal distance between the primitive body and the starting end of the inclined flash edge; In step S5, the yield equation is as described in equation (4): (4) in k is the shear yield strength; In step S6, the above equations (1), (2), (3) and (4) are combined and the stress boundary conditions are substituted: x = x e hour, σ y = σ ye , the principal stress method is used to obtain the vertical stress distribution in different regions of the blank, as described in equation (5): (5) in m is the friction factor.

2. The method for predicting and controlling metal streamlines of space envelope forming of thin-walled high-rib components according to claim 1 is characterized in that: In step S7, the real-time position of the diverter surface is determined according to the vertical stress distribution on both sides of the diverter surface. According to equation (5), when the diverter surface on the left side of the high rib satisfies When x i1 As described in equation (6): (6) in L 0 is the initial distance between the rib and the left end of the blank. L Si1 is the instantaneous length of the left flying edge; From equation (5), it can be obtained that when the left side flow distribution surface of the high rib satisfies When x i1 As described in equation (7): (7) From equation (5), we can get that the position of the diversion surface on the right side of the high rib is x i2 As described in equation (8): (8) in b It is the width of the tendon. L is the initial width of the blank, L Si2 is the instantaneous length of the right flash edge.

3. The method for predicting and controlling metal streamlines of space envelope forming of thin-walled high-rib components according to claim 2 is characterized in that: In step S8, the real-time metal volume distribution is completed according to the real-time diversion surface position, and the left flash length is instantaneously increased. L ti1 and the instantaneous increment of the right flash length L ti2 As described in equation (9) and equation (10) respectively: (9) (10) in Δt is the instantaneous increment of forming time.

4. The method for predicting and controlling metal streamlines of space envelope forming of thin-walled high-rib components according to claim 3 is characterized in that: In step S9, according to the instantaneous increment of the left and right flash edges L ti1 and L ti2 Update the deformed blank shape and the new left flash instantaneous length L Si1 and the new instantaneous length of the right fin L Si2 As described in equation (11): (11) Repeat the above process from S1 to S10 until the spatial envelope is formed and multiple groups of x i1 and x i2 The value of .

5. The method for predicting and controlling metal streamlines of space envelope forming of thin-walled high-rib components according to claim 4 is characterized in that: In the step S10, a function is defined to represent the difference in distance between the left and right side flow dividing surfaces and the high rib symmetry line at any time, as described in equation (12): (12) Adjust the α value so that f ( x ) is equal to 0, that is, the volume of metal extruded into the high ribs on the left and right sides is equal, so as to obtain high-quality metal streamlines for spatial envelope forming of thin-walled high-rib components, thereby realizing precise control of metal streamlines for spatial envelope forming of thin-walled high-rib components.

Citation Information

Patent Citations

  • Space enveloping forming method for thin-wall multi-ring high-rib component

    CN110918844A

  • Method for improving high reinforcement forming limit of spatial envelope forming of thin-walled high reinforcement component

    CN110918849A