KrF photoresist and preparation method thereof
Through the cross-linking of phenolic resin and poly-para-hydroxystyrene resin and the addition of high-boiling point polar solvents and organic alkaline compounds, the problem of KrF photoresist pattern collapse is solved, the photolithography accuracy and pattern quality are improved, and photolithography is realized. Stable bonding and efficient preparation of resist.
Patent Information
- Application Number
- CN202111650135.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-30
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2041-12-30
AI Technical Summary
When KrF photoresist is used to produce patterns with a large aspect ratio, the photolithography pattern is prone to collapse due to the surface tension of the developer, affecting the quality of the photolithography pattern.
Phenolic resin and polyparahydroxystyrene resin are used to cross-link each other, and the bonding strength between polyparahydroxystyrene resin and the substrate is improved through the bridging effect of phenolic resin, and high boiling point polar solvents and organic alkaline compounds are added. Optimize photoresist composition and preparation methods.
Significantly improves the stability and quality of lithography patterns, improves lithography accuracy and substrate adhesion, ensures that the lithography pattern does not collapse, and the minimum line width that can be separated is below 0.25μm, and the minimum line width that the pattern does not collapse Below 0.3μm.
Abstract
Description
Technical Field
[0001] The present application relates to the field of photoresists, and more specifically, to a KrF photoresist and a preparation method thereof. Background Art
[0002] Photoresist is a thin film material that is etched with corrosion resistance and whose solubility changes under the irradiation of ultraviolet light, electron beam, ion beam or X-ray. It is a key material in the photolithography process and is of great significance for the production of transistors and integrated circuits.
[0003] Photoresists can be divided into g-line photoresists, i-line photoresists, KrF photoresists, ArF photoresists and EUV photoresists according to the different photolithography precision and light source wavelength. Among them, the light source wavelength of g-line photoresists is 436nm, and the light source wavelength of i-line photoresists is 365nm, both of which are near-ultraviolet photoresists; the light source wavelength of KrF photoresists is 248nm, and the light source wavelength of ArF photoresists is 193nm, both of which are deep ultraviolet photoresists; EUV photoresists are called extreme ultraviolet photoresists, and their light source wavelength is 13.5nm. Among these photoresists, KrF photoresists are currently the most commonly used photoresists, mainly used for the production of 8-inch wafers; KrF photoresists not only have high photolithography precision, but also have a certain process tolerance.
[0004] However, the applicant has found through research that when KrF photoresist is used to produce patterns with a large aspect ratio, the photolithographic pattern is prone to collapse due to the surface tension of the developer, which seriously affects the quality of the photolithographic pattern. Summary of the invention
[0005] In order to reduce the problem of photolithography pattern collapse, the present application provides a KrF photoresist and a preparation method thereof.
[0006] In the first aspect, a KrF photoresist is provided, which adopts the following technical solution:
[0007] The KrF photoresist is prepared from the following raw materials in parts by weight: 100 parts of poly(p-hydroxystyrene) resin, 1-5 parts of photoacid generator, 2-20 parts of phenolic resin and 400-600 parts of solvent.
[0008] By adopting the above technical solution, the network-like molecular structure of the phenolic resin and the molecular chains of the poly(p-hydroxystyrene) resin are intertwined and cross-linked, and can be stably combined together; at the same time, the phenolic resin has good wettability to the photolithography substrate and can form a stable connection with the substrate. Through the bridge effect of the phenolic resin, the bonding firmness of the poly(p-hydroxystyrene) resin and the substrate is improved, thereby greatly improving the problem of photolithography pattern collapse and improving the quality of the photolithography pattern.
[0009] In a specific embodiment, the poly(p-hydroxystyrene) resin is a terpolymer of hydroxystyrene-styrene-tert-butyl acrylate.
[0010] By adopting the above technical scheme, hydroxystyrene and styrene can play a role in adjusting the solubility of the resin, while tert-butyl acrylate can be deprotected after exposure, so that the exposed photoresist resin can be dissolved in the developer; through the mutual polymerization and synergy of the three, the poly(p-hydroxystyrene) resin is endowed with good lithography performance.
[0011] In a specific embodiment, the hydroxystyrene-styrene-tert-butyl acrylate terpolymer is copolymerized by hydroxystyrene, styrene, and tert-butyl acrylate in a mass ratio of 10:(3-4):(3-4);
[0012] The average molecular weight of the hydroxystyrene-styrene-tert-butyl acrylate copolymer is 7000-15000, and the molecular weight distribution index is less than 2.
[0013] By adopting the above technical scheme, the ratio of hydroxystyrene, styrene and tert-butyl acrylate and the molecular weight of the terpolymer are optimized, thereby further improving the lithography performance of the hydroxystyrene-styrene-tert-butyl acrylate terpolymer.
[0014] In a specific embodiment, the phenolic resin has an average molecular weight of 4000-6000 and is copolymerized by p-cresol, m-cresol and formaldehyde.
[0015] By adopting the above technical solution, the phenolic resin is optimized, which is beneficial to further improve the bonding degree between the poly(p-hydroxystyrene) resin and the substrate.
[0016] In a specific embodiment, the photoacid generator is triphenylsulfonium salt.
[0017] In a specific embodiment, the solvent is a polar solvent having a boiling point higher than 100°C.
[0018] By adopting the above technical solution, the use of a high-boiling-point polar solvent can make the phenolic resin and the hydroxystyrene resin have better solubility, and the high-boiling-point solvent is more conducive to spin coating to form a flat and uniform photoresist film.
[0019] In a specific embodiment, the solvent is one of propylene glycol methyl ether acetate, propylene glycol methyl ether, dipropylene glycol methyl ether, and cyclohexanone.
[0020] In a specific embodiment, 3-8 parts by weight of an organic basic compound is further included.
[0021] By adopting the above technical solution, the addition of organic alkaline compounds can play a role in adjusting the photosensitivity of the photoresist system.
[0022] In a specific embodiment, the organic basic compound is an organic amine and a salt thereof.
[0023] In a second aspect, a method for preparing the above-mentioned KrF photoresist is provided, which adopts the following technical solution:
[0024] The preparation method of KrF photoresist comprises the following steps: taking various raw materials according to the formula, mixing them evenly, filtering and filling them.
[0025] By adopting the above technical solution, KrF photoresist is successfully prepared. The obtained KrF photoresist has good bonding with the substrate, so the pattern collapse problem obtained by photolithography is less.
[0026] In summary, the present application has at least one of the following beneficial technical effects:
[0027] 1. The minimum line width that can be separated by the photoresist obtained in this application is less than 0.25 μm, and the minimum line width corresponding to the non-collapse of the pattern is less than 0.3 μm, showing good photolithography accuracy and substrate adhesion.
[0028] 2. The present application uses the network-like molecular structure of the phenolic resin to cross-link the phenolic resin and the poly(p-hydroxystyrene) resin to form a stable whole; at the same time, the phenolic resin and the substrate form a stable connection through the good wettability between the phenolic resin and the substrate. The bridging effect of the phenolic resin can improve the bonding between the poly(p-hydroxystyrene) resin and the substrate, thereby greatly improving the problem of photolithographic pattern collapse and improving the quality of the photolithographic pattern.
[0029] 3. The present application improves the photosensitivity of the photoresist by adding an organic alkaline compound. DETAILED DESCRIPTION
[0030] The present application is further described in detail below with reference to the embodiments.
[0031] Example 1
[0032] This embodiment discloses a KrF photoresist, which includes the following raw materials: 100 kg of poly(p-hydroxystyrene) resin, 1 kg of photoacid generator, 2 kg of phenolic resin and 400 kg of solvent.
[0033] Among them: In this embodiment, the poly(p-hydroxystyrene) resin used as the main material of the photoresist is specifically a hydroxystyrene-styrene-tert-butyl acrylate terpolymer, which is copolymerized by hydroxystyrene, styrene and tert-butyl acrylate in a mass ratio of 100:30:30; the average molecular weight of the terpolymer is 15,000, and the molecular weight distribution index is 1.9. In the hydroxystyrene-styrene-tert-butyl acrylate terpolymer: hydroxystyrene and styrene are used to adjust the solubility of the resin, and tert-butyl acrylate is used for deprotection after exposure, so that the exposed photoresist resin is soluble in the developer.
[0034] The photoacid generator is a photosensitive compound, which plays an important role in making the photoresist dissolve in the developer. In this embodiment, the photoacid generator is triphenylsulfonium salt.
[0035] Phenolic resin and poly(p-hydroxystyrene) resin have similar structures and polarities, so they have good compatibility; when phenolic resin is introduced into the photoresist system, the network-like molecular structure of phenolic resin and the molecular chains of poly(p-hydroxystyrene) resin are intertwined and cross-linked, and are stably combined together; at the same time, phenolic resin has good wettability to the photolithographic substrate and can form a stable connection with the substrate. The bridging effect of phenolic resin improves the bonding firmness between poly(p-hydroxystyrene) resin and substrate. In the embodiment of the present application, the average molecular weight of phenolic resin is 4000, and it is copolymerized by p-cresol, m-cresol and formaldehyde, wherein the mass ratio of p-cresol to m-cresol is 2:3.
[0036] In this embodiment, the solvent is propylene glycol methyl ether acetate, which has a boiling point of 155° C. and is a high-boiling-point polar solvent. The use of a high-boiling-point polar solvent can make the phenolic resin and the hydroxystyrene resin more soluble, and the high-boiling-point solvent is more conducive to spin coating to form a flat and uniform photoresist film.
[0037] This embodiment also discloses a method for preparing the above-mentioned KrF photoresist, comprising the following steps:
[0038] S1. Accurately weigh 100 kg of poly(p-hydroxystyrene) resin, 1 kg of photoacid generator, 2 kg of phenolic resin and 400 kg of solvent.
[0039] S2. Place the solvent in a mixing container; at room temperature and pressure, add the poly(p-hydroxystyrene) resin, the photoacid generator and the phenolic resin into the solvent in batches, and mix the above raw materials evenly at a stirring speed of 80 rpm.
[0040] S3. The mixed raw material obtained in S2 is filtered three times through 0.45 μm, 0.20 μm and 0.10 μm filters in sequence and then bottled.
[0041] Embodiment 2-6
[0042] Embodiments 2-6 are basically the same as Embodiment 1, except that the amount of phenolic resin added in the raw material composition is different.
[0043] Specifically:
[0044] In Example 2, the raw material ratio of KrF photoresist is: 100 kg of poly(p-hydroxystyrene) resin, 1 kg of photoacid generator, 5 kg of phenolic resin and 400 kg of solvent.
[0045] In Example 3, the raw material ratio of KrF photoresist is: 100 kg of poly(p-hydroxystyrene) resin, 1 kg of photoacid generator, 8 kg of phenolic resin and 400 kg of solvent.
[0046] In Example 4, the raw material ratio of KrF photoresist is: 100 kg of poly(p-hydroxystyrene) resin, 1 kg of photoacid generator, 12 kg of phenolic resin and 400 kg of solvent.
[0047] In Example 5, the raw material ratio of KrF photoresist is: 100 kg of poly(p-hydroxystyrene) resin, 1 kg of photoacid generator, 16 kg of phenolic resin and 400 kg of solvent.
[0048] In Example 6, the raw material ratio of KrF photoresist is: 100 kg of poly(p-hydroxystyrene) resin, 1 kg of photoacid generator, 20 kg of phenolic resin and 400 kg of solvent.
[0049] Example 7
[0050] This embodiment discloses a KrF photoresist, which includes the following raw materials: 100 kg of poly(p-hydroxystyrene) resin, 2 kg of photoacid generator, 12 kg of phenolic resin and 450 kg of solvent.
[0051] Among them: In this embodiment, the poly(p-hydroxystyrene) resin is specifically a hydroxystyrene-styrene-tert-butyl acrylate terpolymer, which is copolymerized by hydroxystyrene, styrene and tert-butyl acrylate in a mass ratio of 100:30:40; its average molecular weight is 12,000 and its molecular weight distribution index is 1.6.
[0052] The photoacid generator is triphenylsulfonium salt. The average molecular weight of the phenolic resin is 5000, and it is copolymerized by p-cresol, m-cresol and formaldehyde, wherein the mass ratio of p-cresol to m-cresol is 2:3. The solvent is propylene glycol methyl ether; the boiling point of the solvent is 119°C, which is a high boiling point polar solvent.
[0053] This embodiment also discloses a method for preparing the above-mentioned KrF photoresist, comprising the following steps:
[0054] S1. Accurately weigh 100 kg of poly(p-hydroxystyrene) resin, 2 kg of photoacid generator, 12 kg of phenolic resin and 450 kg of solvent.
[0055] S2. Place the solvent in a mixing container; at room temperature and pressure, add the poly(p-hydroxystyrene) resin, the photoacid generator and the phenolic resin into the solvent in batches, and mix the above raw materials evenly at a stirring speed of 100 rpm.
[0056] S3. The mixed raw material obtained in S2 is filtered three times through 0.45 μm, 0.20 μm and 0.10 μm filters in sequence and then bottled.
[0057] Example 8
[0058] This embodiment discloses a KrF photoresist, which includes the following raw materials: 100 kg of poly(p-hydroxystyrene) resin, 3 kg of photoacid generator, 12 kg of phenolic resin and 500 kg of solvent.
[0059] Among them: In this embodiment, the poly(p-hydroxystyrene) resin is specifically a hydroxystyrene-styrene-tert-butyl acrylate terpolymer, which is copolymerized by hydroxystyrene, styrene and tert-butyl acrylate in a mass ratio of 60:20:20; its average molecular weight is 10,000 and its molecular weight distribution index is 1.5.
[0060] The photoacid generator is triphenylsulfonium salt. The average molecular weight of the phenolic resin is 5000, and it is copolymerized by p-cresol, m-cresol and formaldehyde, wherein the mass ratio of p-cresol to m-cresol is 1:1. The solvent is cyclohexanone; the boiling point of the solvent is 156°C, which is a high boiling point polar solvent.
[0061] This embodiment also discloses a method for preparing the above-mentioned KrF photoresist, comprising the following steps:
[0062] S1. Accurately weigh 100 kg of poly(p-hydroxystyrene) resin, 3 kg of photoacid generator, 12 kg of phenolic resin and 500 kg of solvent.
[0063] S2. Place the solvent in a mixing container; at room temperature and pressure, add the poly(p-hydroxystyrene) resin, the photoacid generator and the phenolic resin into the solvent in batches, and mix the raw materials evenly at a stirring speed of 120 rpm.
[0064] S3. The mixed raw material obtained in S2 is filtered three times through 0.45 μm, 0.20 μm and 0.10 μm filters in sequence and then bottled.
[0065] Example 9
[0066] This embodiment discloses a KrF photoresist, which includes the following raw materials: 100 kg of poly(p-hydroxystyrene) resin, 4 kg of photoacid generator, 12 kg of phenolic resin and 550 kg of solvent.
[0067] Among them: In this embodiment, the poly(p-hydroxystyrene) resin is specifically a hydroxystyrene-styrene-tert-butyl acrylate terpolymer, which is copolymerized by hydroxystyrene, styrene and tert-butyl acrylate in a mass ratio of 100:40:30; its average molecular weight is 9000 and its molecular weight distribution index is 1.2.
[0068] The photoacid generator is triphenylsulfonium salt. The average molecular weight of the phenolic resin is 5000, and it is copolymerized by p-cresol, m-cresol and formaldehyde, wherein the mass ratio of p-cresol to m-cresol is 3:2. The solvent is dipropylene glycol methyl ether; the boiling point of the solvent is 190°C, which is a high boiling point polar solvent.
[0069] This embodiment also discloses a method for preparing the above-mentioned KrF photoresist, comprising the following steps:
[0070] S1. Accurately weigh 100 kg of poly(p-hydroxystyrene) resin, 4 kg of photoacid generator, 12 kg of phenolic resin and 550 kg of solvent.
[0071] S2. Place the solvent in a mixing container; at room temperature and pressure, add the poly(p-hydroxystyrene) resin, the photoacid generator and the phenolic resin into the solvent in batches, and mix the raw materials evenly at a stirring speed of 120 rpm.
[0072] S3. The mixed raw material obtained in S2 is filtered three times through 0.45 μm, 0.20 μm and 0.10 μm filters in sequence and then bottled.
[0073] Example 10
[0074] This embodiment discloses a KrF photoresist, which includes the following raw materials: 100 kg of poly(p-hydroxystyrene) resin, 5 kg of photoacid generator, 12 kg of phenolic resin and 600 kg of solvent.
[0075] Among them: In this embodiment, the poly(p-hydroxystyrene) resin is specifically a hydroxystyrene-styrene-tert-butyl acrylate terpolymer, which is copolymerized by hydroxystyrene, styrene and tert-butyl acrylate in a mass ratio of 100:40:40; its average molecular weight is 7000 and its molecular weight distribution index is 1.2.
[0076] The photoacid generator is triphenylsulfonium salt. The average molecular weight of the phenolic resin is 6000, and it is copolymerized by p-cresol, m-cresol and formaldehyde, wherein the mass ratio of p-cresol to m-cresol is 3:2. The solvent is cyclohexanone.
[0077] This embodiment also discloses a method for preparing the above-mentioned KrF photoresist, comprising the following steps:
[0078] S1. Accurately weigh 100 kg of poly(p-hydroxystyrene) resin, 5 kg of photoacid generator, 12 kg of phenolic resin and 600 kg of solvent.
[0079] S2. Place the solvent in a mixing container; at room temperature and pressure, add the poly(p-hydroxystyrene) resin, the photoacid generator and the phenolic resin into the solvent in batches, and mix the raw materials evenly at a stirring speed of 150 rpm.
[0080] S3. The mixed raw material obtained in S2 is filtered three times through 0.45 μm, 0.20 μm and 0.10 μm filters in sequence and then bottled.
[0081] Embodiment 11
[0082] This embodiment is basically the same as the embodiment 8, except that the raw materials of the KrF photoresist further include an organic alkaline compound. The addition of the organic alkaline compound can adjust the photosensitivity of the photoresist system.
[0083] The specific composition ratio of the raw materials is: 100 kg of polyparahydroxystyrene resin, 3 kg of photoacid generator, 12 kg of phenolic resin, 3 kg of organic alkaline compound and 500 kg of solvent.
[0084] The preparation method of KrF photoresist comprises the following steps:
[0085] S1. Accurately weigh 100 kg of poly(p-hydroxystyrene) resin, 3 kg of photoacid generator, 12 kg of phenolic resin, 3 kg of organic alkaline compound and 500 kg of solvent.
[0086] S2. Place the solvent in a mixing container; at room temperature and pressure, add the poly(p-hydroxystyrene) resin, the photoacid generator, the organic alkaline compound and the phenolic resin to the solvent in batches, and mix the above raw materials evenly at a stirring speed of 120 rpm.
[0087] S3. The mixed raw material obtained in S2 is filtered three times through 0.45 μm, 0.20 μm and 0.10 μm filters in sequence and then bottled.
[0088] In this embodiment, the organic alkaline compound is tripentylamine; in other embodiments, the organic alkaline compound can also be other conventional organic amines and their salts; such as acrylamide, p-phenylenediamine, 1-naphthylamine, dimethylamine hydrochloride, diethylamine hydrochloride, m-phenylenediamine sulfate, etc.
[0089] Examples 12-13
[0090] Examples 12-13 are basically the same as Example 11, except that the amount of organic alkaline compound added in the raw material composition is different.
[0091] Specifically:
[0092] In Example 12, the raw material ratio of KrF photoresist is: 100 kg of poly(p-hydroxystyrene) resin, 3 kg of photoacid generator, 12 kg of phenolic resin, 6 kg of organic alkaline compound and 500 kg of solvent.
[0093] In Example 13, the raw material ratio of KrF photoresist is: 100 kg of poly(p-hydroxystyrene) resin, 3 kg of photoacid generator, 12 kg of phenolic resin, 8 kg of organic alkaline compound and 500 kg of solvent.
[0094] Comparative Example 1
[0095] This comparative example discloses a KrF photoresist, which is mainly different from Example 1 in that the raw materials of the KrF photoresist do not contain phenolic resin.
[0096] Specifically, the raw materials of KrF photoresist include: 100 kg of polyparahydroxystyrene resin, 1 kg of photoacid generator and 400 kg of solvent.
[0097] Comparative Example 2
[0098] This comparative example discloses a KrF photoresist, which is mainly different from Example 1 in that the raw material of the KrF photoresist contains excessive phenolic resin.
[0099] Specifically, the raw materials of KrF photoresist include: 100 kg of polyparahydroxystyrene resin, 1 kg of photoacid generator, 25 kg of phenolic resin and 400 kg of solvent.
[0100] Performance Testing
[0101] 1. The KrF photoresists obtained in Examples 1-13 and Comparative Examples 1-2 were subjected to image collapse test and photolithography accuracy test.
[0102] 1. Image collapse test: It is characterized by the line width corresponding to the photolithography pattern without collapse. Specifically, the glue is applied on the polished silicon wafer by spin coating, and the solvent is dried on a hot plate to obtain a glue film, and the thickness of the glue film is controlled to be 0.5μm; then, the polished silicon wafers coated with the glue film are exposed using a Nikon-s204 KrF exposure machine, and the exposure amount is 35mj / cm 2After exposure, the film is baked for deprotection reaction; then it is placed in tetramethylammonium hydroxide developer (concentration of 2.38%) to develop and obtain the preset pattern; then it is observed and measured with Hitachi 9220 critical dimension measurement-scanning electron microscope (CDSEM) to obtain the minimum line width corresponding to the photolithography pattern not collapsing. The smaller the line width, the less likely the photolithography pattern is to collapse, and the better the quality of the photolithography pattern.
[0103] 2. Photolithography accuracy test: characterized by the minimum line width that can be separated by the photolithography pattern. Specifically, the glue is applied on the polished silicon wafer by spin coating, and the solvent is dried on a hot plate to obtain a glue film, and the thickness of the glue film is controlled to be 0.5μm; then, the polished silicon wafers coated with the glue film are exposed using a Nikon-s204 KrF exposure machine, and the exposure amount is 35mj / cm 2 After exposure, the film is baked for deprotection reaction; then it is placed in tetramethylammonium hydroxide exposure solution (concentration is 2.38%) for development to obtain the preset pattern; then it is observed and measured with Hitachi 9220 critical dimension measurement-scanning electron microscope (CDSEM) to obtain the minimum line width that can be separated by the photolithography pattern. The smaller the line width, the higher the photolithography accuracy.
[0104] It should be noted that the minimum line width obtained by the image collapse test will not be less than the minimum line width of the lithography accuracy.
[0105] The specific test results are shown in Table 1.
[0106] Table 1 Adhesion and photolithography accuracy of the photoresists obtained in Examples 1-13 and Comparative Examples 1-2
[0107] project Minimum line width without collapse / μm Minimum line width that can be separated / μm Example 1 0.3 0.2 Example 2 0.25 0.2 Example 3 0.25 0.2 Example 4 0.2 0.2 Example 5 0.25 0.25 Example 6 0.25 0.25 Example 7 0.25 0.2 Example 8 0.2 0.18 Example 9 0.2 0.18 Example 10 0.2 0.18 Embodiment 11 0.2 0.18 Example 12 0.2 0.2 Example 13 0.2 0.2 Comparative Example 1 0.4 0.2 Comparative Example 2 0.3 0.3
[0108] Referring to Table 1, analyzing the test results of Examples 1-13, it can be found that the minimum line width that can be separated by the photoresist obtained in each embodiment of the present application is less than 0.25 μm, and the minimum line width corresponding to the non-collapse of the pattern is less than 0.3 μm. This shows that the photoresist obtained in each embodiment of the present application has good photolithography accuracy and substrate bonding.
[0109] Comparing the test results of Examples 1-6 and Comparative Examples 1-2, it can be found that when no phenolic resin is added, the minimum line width corresponding to the non-collapse of the obtained photoresist pattern is relatively wide; with the continuous addition of phenolic resin, the minimum line width corresponding to the non-collapse of the obtained photoresist after exposure and development is relatively wide and gradually decreases, and the quality of the pattern is getting better and better. This is because with the addition of phenolic resin, on the one hand, the network-like molecular structure of phenolic resin is entangled and cross-linked with more molecular chains of poly(p-hydroxystyrene) resin, so that the binding of phenolic resin and poly(p-hydroxystyrene) resin is better; on the other hand, the connectivity of phenolic resin to the substrate is more firm; thus, with the continuous increase in the amount of phenolic resin added, the binding firmness of poly(p-hydroxystyrene) resin and substrate is getting better and better, and then the obtained photolithographic pattern is less and less likely to collapse, and the quality of the obtained photolithographic pattern is getting better and better. However, as the proportion of phenolic resin increases, it will have a certain impact on the photolithographic accuracy of the photoresist.
[0110] 2. Take the KrF photoresist obtained in Examples 8, 11-13 and conduct photosensitivity test.
[0111] Photosensitivity test: Characterized by the minimum exposure required to separate the same line width. Specifically: Spin coating is used on the polished silicon wafer, and the solvent is dried on a hot plate to obtain a film, and the thickness of the film is controlled to be 0.5μm; then the polished silicon wafers coated with the film are exposed using a Nikon-s204 KrF exposure machine; after exposure, the film is baked for deprotection reaction; then it is placed in a tetramethylammonium hydroxide exposure solution (concentration of 2.38%) for development to obtain a preset pattern; then a Hitachi 9220 critical dimension measurement-scanning electron microscope (CDSEM) is used for observation and measurement to detect whether the line width that can be separated by the photolithography pattern reaches the preset value (set to 0.2μm in this application); if it does not reach it, the exposure is increased and tested again, and repeated several times to obtain the minimum exposure that can separate the preset line width. The smaller the minimum exposure, the better the photosensitivity of the surface photoresist.
[0112] The specific test results are shown in Table 2.
[0113] Table 2 Photosensitivity of the photoresists obtained in Examples 8, 11-13
[0114] project <![CDATA[Minimum exposure / mj·cm -2 > Example 8 36 Embodiment 11 32 Example 12 30 Example 13 29
[0115] Referring to Table 2, it can be seen from the test results of Examples 8, 11-13 that the addition of organic alkaline compounds is beneficial to improving the photosensitivity of the photoresist.
[0116] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A KrF photoresist, characterized in that: The invention is prepared from the following raw materials in parts by weight: 100 parts of poly(p-hydroxystyrene) resin, 1-5 parts of photoacid generator, 2-20 parts of phenolic resin and 400-600 parts of solvent; The poly(p-hydroxystyrene) resin is a terpolymer of hydroxystyrene-styrene-tert-butyl acrylate; The hydroxystyrene-styrene-tert-butyl acrylate terpolymer is copolymerized by hydroxystyrene, styrene and tert-butyl acrylate in a mass ratio of 10:(3-4):(3-4); The average molecular weight of the hydroxystyrene-styrene-tert-butyl acrylate copolymer is 7000-15000, and the molecular weight distribution index is less than 2; The phenolic resin has an average molecular weight of 4000-6000 and is copolymerized by p-cresol, m-cresol and formaldehyde.
2. The KrF photoresist according to claim 1, characterized in that: The photoacid generator is triphenylsulfonium salt.
3. The KrF photoresist according to claim 1, characterized in that: The solvent is a polar organic solvent with a boiling point higher than 100°C.
4. The KrF photoresist according to claim 3, characterized in that: The solvent is one of propylene glycol methyl ether acetate, propylene glycol methyl ether, dipropylene glycol methyl ether and cyclohexanone.
5. The KrF photoresist according to any one of claims 1 to 4, characterized in that: It also includes 3-8 parts by weight of an organic basic compound.
6. The KrF photoresist according to claim 5, characterized in that: The organic basic compound is an organic amine and a salt thereof.
7. The method for preparing the KrF photoresist according to any one of claims 1 to 6, characterized in that: The following steps are involved: Take the raw materials according to the recipe, mix them evenly, filter and fill them.