Nickel cobalt hydroxide and preparation method, nickel cobalt oxide, lithium ion battery positive electrode material, positive electrode, battery and electrical equipment

By using the multi-layer structure of nickel-cobalt hydroxide material in lithium-ion batteries, the cycle performance and safety problems of high-nickel large-particle precursors are solved, the capacity and rate performance of the battery are improved, and more stable battery operation is achieved .

CN114261997BActive Publication Date: 2024-11-15GUANGXI CNGR NEW ENERGY SCI & TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111623523.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-28
Publication Date
2024-11-15
Estimated Expiration
2041-12-28

AI Technical Summary

Technical Problem

The existing 8-Series and 9-Series high-nickel large-particle ternary and binary precursors have insufficient cycling performance and safety in lithium-ion batteries, resulting in low battery capacity, poor rate performance and prone to safety accidents.

Method used

Nickel-cobalt hydroxide material is used, which consists of the inner core area, the intermediate area and the outer shell area. The porosity of the intermediate area is greater than that of the inner core area and the outer shell area. It is prepared through a specific precipitation reaction and firing process to form a multi-layer structure to improve the material. Stability and battery performance.

Benefits of technology

It improves the circulation performance, safety and capacity of lithium-ion batteries, reduces lithium diffusion resistance, enhances the structural strength of the battery, and extends the service life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114261997B_ABST
    Figure CN114261997B_ABST
Patent Text Reader

Abstract

The present application provides a nickel cobalt hydroxide and a preparation method, nickel cobalt oxide, a positive electrode material for lithium-ion batteries, a positive electrode, a battery and electrical equipment. Nickel cobalt hydroxide includes an inner core region, an intermediate region and an outer shell region, wherein the intermediate region covers the inner core region, and the outer shell region covers the intermediate region; the porosity of the intermediate region is greater than the porosity of the inner core region and the porosity of the outer shell region. The preparation method of nickel cobalt hydroxide: mixing raw materials including a nickel cobalt binary aqueous solution, a sodium hydroxide aqueous solution and ammonia water, and obtaining seed crystals through a first coprecipitation reaction; mixing raw materials including the seed crystals, a nickel cobalt binary aqueous solution, a sodium hydroxide aqueous solution and ammonia water, and obtaining the nickel cobalt hydroxide through a second coprecipitation reaction. The nickel cobalt hydroxide provided in the present application has a special pore distribution and a stable material structure, and can effectively improve battery capacity, cycle performance, safety, etc.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of lithium-ion batteries, and in particular to a nickel-cobalt hydroxide and a preparation method thereof, a nickel-cobalt oxide, a lithium-ion battery positive electrode material, a positive electrode, a battery and electrical equipment. Background Art

[0002] The global automotive industry is developing rapidly. As an emerging environmentally friendly power source, lithium batteries are increasingly used in the automotive industry. As the most important component of lithium batteries, cathode precursor materials have always been the core of the technology. Currently, the most common ternary precursors on the market are 5-series and 6-series, but their low capacity limits their application in new energy vehicles.

[0003] In order to compete for market resources, some precursor manufacturers have begun to develop 8 series and 9 series high-nickel large-particle ternary and binary precursors. However, the 8 series and 9 series high-nickel large-particle ternary and binary precursors have not been fully promoted due to problems such as poor cycle performance and poor safety.

[0004] High-nickel large-particle precursors are generally synthesized by intermittent method, with extremely narrow particle size distribution, which can also make the particle structure highly uniform. Batteries prepared by loose precursors have high capacity and good rate performance, but the particle strength itself is insufficient. During multiple charge and discharge processes, the particles are easily broken, affecting the capacity, poor cycle performance and prone to safety accidents. Batteries prepared by dense precursors have large lithium ion diffusion resistance and insufficient rate performance.

[0005] Therefore, how to improve the cycle performance and safety of 8 series and 9 series high-nickel large-particle ternary and binary precursors is the main difficulty currently faced. Summary of the invention

[0006] The purpose of this application is to provide a nickel cobalt hydroxide and a preparation method, a nickel cobalt oxide, a lithium ion battery positive electrode material, a positive electrode, a battery and electrical equipment to solve the above problems.

[0007] To achieve the above objectives, this application adopts the following technical solutions:

[0008] A nickel-cobalt hydroxide, comprising an inner core region, an intermediate region and an outer shell region, wherein the intermediate region covers the inner core region, and the outer shell region covers the intermediate region;

[0009] The porosity of the middle region is greater than the porosity of the inner core region and the porosity of the outer shell region.

[0010] Preferably, the nickel cobalt hydroxide satisfies at least one of the following conditions:

[0011] a. The porosity of the intermediate zone is 5%-10%, and the porosity of the inner core zone and the porosity of the outer shell zone are each independently 1%-5%;

[0012] b. The pores in the inner core area are distributed in a network shape, the pores in the middle area are radially divergent toward the outer shell area, and the pores in the outer shell area are distributed in a scattered point shape;

[0013] c. The diameter of the inner core region is 3 μm-6 μm;

[0014] d. The diameter of the intermediate zone is 5 μm-14 μm;

[0015] e. The diameter of the shell region is 10 μm-16 μm;

[0016] f. The peak intensity ratio (I101:I001) of the nickel cobalt hydroxide is not less than 1.1;

[0017] g. The peak intensity ratio (I101:I001) of the nickel cobalt hydroxide is 1.2-1.5;

[0018] h. The 001 half-peak width of the nickel cobalt hydroxide is 0.5-0.9, and the 101 half-peak width is 0.45-0.85;

[0019] i. The (D95-D5) / D50 of the nickel cobalt hydroxide is 0.35-0.5.

[0020] Preferably, the molecular formula of the nickel-cobalt hydroxide is Ni x Co (1-x) (OH)2, where 0.8≤x<1.0.

[0021] The present application also provides a method for preparing the nickel-cobalt hydroxide, comprising:

[0022] Mixing raw materials including a nickel-cobalt binary aqueous solution, a sodium hydroxide aqueous solution, and ammonia water, and obtaining seed crystals through a first coprecipitation reaction;

[0023] The raw materials including the seed crystal, the nickel-cobalt binary aqueous solution, the sodium hydroxide aqueous solution and the ammonia water are mixed, and the nickel-cobalt hydroxide is obtained through a second coprecipitation reaction.

[0024] Preferably, the preparation method satisfies at least one of the following conditions:

[0025] j. The concentration of the nickel-cobalt binary aqueous solution is 80g / L-120g / L;

[0026] k. During the first coprecipitation reaction and the second coprecipitation reaction, the flow rate of the nickel-cobalt binary aqueous solution is independently 300 L / h-600 L / h, the flow rate of the sodium hydroxide aqueous solution is independently 60 L / h-250 L / h, and the flow rate of the ammonia water is independently 10 L / h-50 L / h;

[0027] l. During the first coprecipitation reaction and the second coprecipitation reaction, the temperature is independently 40°C-60°C, and the stirring speed is independently 180r / min-220r / min;

[0028] m. During the first coprecipitation reaction, the pH was 10-13; during the second coprecipitation reaction, the pH control range of the system was: the pH within 2 days of the reaction was 10.3-10.8, and the pH from 3 days to the end of the reaction was 11.4-12;

[0029] n. The seed crystal particle size is 3μm-7μm;

[0030] o. After the first coprecipitation reaction is completed, the seed crystal having a water content of less than or equal to 25% is obtained by solid-liquid separation;

[0031] p. The particle size of the nickel-cobalt hydroxide is not less than 12 μm;

[0032] q. After the second coprecipitation reaction, the step further comprises: sequentially washing the reaction product with alkali, washing with water, solid-liquid separation and drying;

[0033] The concentration of the sodium hydroxide aqueous solution used in the alkali washing is 3wt%-10wt%; the drying temperature is 90°C-150°C.

[0034] The present application also provides a nickel-cobalt oxide, the nickel-cobalt oxide comprising a first region, a second region and a third region, the second region covers the first region, and the third region covers the second region;

[0035] The porosity of the second region is greater than the porosity of the first region, and the porosity of the second region is greater than or equal to the porosity of the third region.

[0036] Preferably, the nickel-cobalt oxide satisfies at least one of the following conditions:

[0037] r. The porosity of the first region is 3%-10%, the porosity of the second region is 15%-25%, and the porosity of the third region is 5%-15%;

[0038] s. The diameter of the first region is 3 μm-6 μm, the diameter of the second region is 5 μm-14 μm, and the diameter of the third region is 10 μm-16 μm;

[0039] t. The (D95-D5) / D50 of the nickel cobalt oxide is 0.18-0.32;

[0040] u. The peak intensity ratio (I012:I101) of the nickel cobalt oxide is not less than 1.4, the half-peak width of 101 is 0.50-0.85, and the half-peak width of 012 is 0.60-0.95;

[0041] v. The molecular formula of the nickel-cobalt oxide is Ni y Co (1-y) O, where 0.8≤y<1.0.

[0042] Preferably, the nickel cobalt oxide is obtained by sintering nickel cobalt hydroxide, the nickel cobalt hydroxide comprises a core region, a middle region and a shell region, the middle region covers the core region, and the shell region covers the middle region; the porosity of the middle region is greater than the porosity of the core region and the porosity of the shell region;

[0043] Preferably, the firing satisfies at least one of the following conditions:

[0044] w. The firing temperature is 400 ℃ -600 ℃;

[0045] x. During the firing process, the feed rate of the kiln is 200kg / h-500kg / h, and the air volume of the kiln is 400m 3 / h-600m 3 / h, the kiln speed is 1r / min-6r / min.

[0046] The present application also provides a lithium-ion battery positive electrode material, the raw materials of which include the nickel cobalt hydroxide or the nickel cobalt oxide.

[0047] The present application also provides a lithium-ion battery positive electrode, the raw materials of which include the lithium-ion battery positive electrode material.

[0048] The present application also provides a lithium-ion battery, comprising the lithium-ion battery positive electrode.

[0049] The present application also provides an electrical device, comprising the lithium-ion battery or powered by the lithium-ion battery.

[0050] Compared with the prior art, the beneficial effects of this application include:

[0051] The nickel cobalt hydroxide provided in the present application has an inner core region, an intermediate region and an outer shell region, and the porosity of the intermediate region is greater than the porosity of the inner core region and the porosity of the outer shell region; the inner core region has a low porosity, which can stabilize the material structure and ensure the stability of the battery product; the middle region has a high porosity, which reduces lithium diffusion resistance, increases discharge capacity and improves charge and discharge efficiency; the outer shell region has a low porosity and high structural strength, which prevents the battery from breaking particles under continuous charge and discharge, thereby improving battery capacity, cycle performance, safety and other performance.

[0052] The method for preparing nickel cobalt hydroxide provided in the present application has a special pore distribution, which can effectively improve the stability of the material and the performance of the battery.

[0053] The nickel cobalt oxide provided in the present application is obtained by sintering the above-mentioned nickel cobalt hydroxide, and has a first region, a second region and a third region similar to the above-mentioned nickel cobalt hydroxide, and the porosity of the second region is greater than the porosity of the first region, and the porosity of the second region is greater than or equal to the porosity of the third region, and an effect similar to the above-mentioned nickel cobalt hydroxide can be obtained.

[0054] The lithium-ion battery positive electrode material, positive electrode, battery and electrical equipment provided in this application have good stability, high electrical performance and good safety. BRIEF DESCRIPTION OF THE DRAWINGS

[0055] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope of the present application.

[0056] Figure 1 A schematic diagram of the structure of nickel-cobalt hydroxide provided in this application;

[0057] Figure 2 This is a multiple narrow peak analysis particle size distribution diagram of the nickel cobalt hydroxide obtained in Example 1;

[0058] Figure 3 This is a particle size distribution diagram of the multiple narrow peak analysis of the nickel-cobalt oxide obtained in Example 1;

[0059] Figure 4 The XRD pattern of the nickel cobalt hydroxide obtained in Example 1;

[0060] Figure 5 The XRD pattern of the nickel-cobalt oxide obtained in Example 1;

[0061] Figure 6 This is a surface electron microscope photograph of the nickel-cobalt hydroxide obtained in Example 1;

[0062] Figure 7This is a cross-sectional electron microscope photograph of the nickel-cobalt hydroxide obtained in Example 1;

[0063] Figure 8 This is a surface electron microscope photograph of the nickel-cobalt oxide obtained in Example 1;

[0064] Fig. 9 This is a cross-sectional electron microscope photograph of the nickel-cobalt oxide obtained in Example 1;

[0065] Fig.10 This is a high-power cross-sectional electron microscope photograph of the nickel-cobalt oxide obtained in Example 1;

[0066] Fig.11 This is a cross-sectional electron microscope photograph of the nickel cobalt hydroxide obtained in Comparative Examples 1-4. DETAILED DESCRIPTION

[0067] As used herein:

[0068] "Prepared from" is synonymous with "comprising." As used herein, the terms "comprising," "including," "having," "containing," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that comprises the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.

[0069] The conjunction "consisting of excludes any unspecified element, step, or component. If used in a claim, this phrase renders the claim closed-ended so that it does not include materials other than those described, except for conventional impurities associated therewith. When the phrase "consisting of" appears in a clause of the body of a claim rather than immediately following the subject matter, it limits only the elements described in that clause; other elements are not excluded from the claim as a whole.

[0070] When an amount, concentration, or other value or parameter is expressed as a range, a preferred range, or a range defined by a series of upper preferred values ​​and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value with any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when a range of "1 to 5" is disclosed, the described range should be interpreted as including ranges "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5", etc. When a numerical range is described in this article, unless otherwise stated, the range is intended to include its end values ​​and all integers and fractions within the range.

[0071] In these examples, parts and percentages are by mass unless otherwise indicated.

[0072] "Parts by mass" refers to the basic unit of measurement for expressing the mass ratio of multiple components. 1 part can represent any unit mass, such as 1g or 2.689g. If we say that the mass of component A is a parts and the mass of component B is b parts, it means the ratio of the mass of component A to the mass of component B is a:b. Alternatively, it means that the mass of component A is aK and the mass of component B is bK (K is an arbitrary number, indicating a multiple factor). It should not be misunderstood that, unlike the mass parts, the sum of the mass of all components is not limited to 100 parts.

[0073] “And / or” is used to indicate that one or both of the stated situations may occur, for example, A and / or B includes (A and B) and (A or B).

[0074] A nickel-cobalt hydroxide, comprising an inner core region, an intermediate region and an outer shell region, wherein the intermediate region covers the inner core region, and the outer shell region covers the intermediate region;

[0075] The porosity of the middle region is greater than the porosity of the inner core region and the porosity of the outer shell region.

[0076] In an optional embodiment, the nickel cobalt hydroxide satisfies at least one of the following conditions:

[0077] a. The porosity of the intermediate zone is 5%-10%, and the porosity of the inner core zone and the porosity of the outer shell zone are each independently 1%-5%;

[0078] Optionally, the porosity of the middle zone may be 5%, 6%, 7%, 8%, 9%, 10% or any value between 5% and 10%, and the porosity of the inner core zone and the porosity of the outer shell zone may be 1%, 2%, 3%, 4%, 5% or any value between 1% and 5% independently;

[0079] b. The pores in the inner core area are distributed in a network shape, the pores in the middle area are radially divergent toward the outer shell area, and the pores in the outer shell area are distributed in a scattered point shape;

[0080] c. The diameter of the inner core region is 3 μm-6 μm;

[0081] d. The diameter of the intermediate zone is 5 μm-14 μm;

[0082] e. The diameter of the shell region is 10 μm-16 μm;

[0083] Figure 1 This is a schematic diagram of the structure of nickel cobalt hydroxide provided in this application. Figure 1 As shown, area A corresponds to the inner core area, area B corresponds to the middle area, and area C corresponds to the outer shell area.

[0084] It should be noted that the diameter referred to in this application refers to the distance from the edge of one side of the region through the center of the circle to the edge of the other side. For example, the diameter of the outer shell region refers to the diameter of the entire nickel cobalt hydroxide particle, not the thickness of the region.

[0085] Optionally, the diameter of the inner core region may be 3 μm, 4 μm, 5 μm, 6 μm or any value between 3 μm and 6 μm; the diameter of the middle region may be 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm or any value between 5 μm and 14 μm; the diameter of the outer shell region may be 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, 16 μm or any value between 10 μm and 16 μm;

[0086] f. The peak intensity ratio (I101:I001) of the nickel cobalt hydroxide is not less than 1.1;

[0087] g. The peak intensity ratio (I101:I001) of the nickel cobalt hydroxide is 1.2-1.5;

[0088] h. The 001 half-peak width of the nickel cobalt hydroxide is 0.5-0.9, and the 101 half-peak width is 0.45-0.85;

[0089] i. The (D95-D5) / D50 of the nickel cobalt hydroxide is 0.35-0.5.

[0090] The product has a high peak intensity ratio in the XRD spectrum. Under this peak intensity ratio and half-peak width, the particles in the product are arranged in an orderly manner, which can improve the battery cycle performance.

[0091] Optionally, the peak intensity ratio (I101:I001) of the nickel cobalt hydroxide can be 1.2, 1.3, 1.4, 1.5 or any value between 1.2-1.5; the 001 half-peak width of the nickel cobalt hydroxide can be 0.5, 0.6, 0.7, 0.8, 0.9 or any value between 0.5-0.9, and the 101 half-peak width can be 0.45, 0.50, 0.55, 0.60, 0.65, 0.70, 0.75, 0.80, 0.85 or any value between 0.45-0.85; the (D95-D5) / D50 of the nickel cobalt hydroxide can be 0.35, 0.40, 0.45, 0.5 or any value between 0.35-0.5.

[0092] In an optional embodiment, the molecular formula of the nickel cobalt hydroxide is Ni x Co (1-x) (OH)2, where 0.8≤x<1.0.

[0093] The present application also provides a method for preparing the nickel-cobalt hydroxide, comprising:

[0094] Mixing raw materials including a nickel-cobalt binary aqueous solution, a sodium hydroxide aqueous solution, and ammonia water, and obtaining seed crystals through a first coprecipitation reaction;

[0095] The raw materials including the seed crystal, the nickel-cobalt binary aqueous solution, the sodium hydroxide aqueous solution and the ammonia water are mixed, and the nickel-cobalt hydroxide is obtained through a second coprecipitation reaction.

[0096] In an optional embodiment, the preparation method satisfies at least one of the following conditions:

[0097] j. The concentration of the nickel-cobalt binary aqueous solution is 80g / L-120g / L;

[0098] Optionally, the concentration of the nickel-cobalt binary aqueous solution may be 80 g / L, 90 g / L, 100 g / L, 110 g / L, 120 g / L or any value between 80 g / L and 120 g / L;

[0099] k. During the first coprecipitation reaction and the second coprecipitation reaction, the flow rate of the nickel-cobalt binary aqueous solution is independently 300 L / h-600 L / h, the flow rate of the sodium hydroxide aqueous solution is independently 60 L / h-250 L / h, and the flow rate of the ammonia water is independently 10 L / h-50 L / h;

[0100] Optionally, during the first coprecipitation reaction and the second coprecipitation reaction, the flow rate of the nickel-cobalt binary aqueous solution can be independently 300 L / h, 400 L / h, 500 L / h, 600 L / h or any value between 300 L / h and 600 L / h, and the flow rate of the sodium hydroxide aqueous solution can be independently 60 L / h, 70 L / h, 80 L / h, 90 L / h, 100 L / h, 110 L / h, 120 L / h, 130 L / h. , 140L / h, 150L / h, 160L / h, 170L / h, 180L / h, 190L / h, 200L / h, 210L / h, 220L / h, 230L / h, 240L / h, 250L / h or any value between 60L / h-250L / h, the flow rate of the ammonia water can be independently 10L / h, 20L / h, 30L / h, 40L / h, 50L / h or any value between 10L / h-50L / h;

[0101] l. During the first coprecipitation reaction and the second coprecipitation reaction, the temperature is independently 40°C-60°C, and the stirring speed is independently 180r / min-220r / min;

[0102] Optionally, during the first coprecipitation reaction and the second coprecipitation reaction, the temperature can be 40°C, 50°C, 60°C or any value between 40°C and 60°C, and the stirring speed can be 180r / min, 190r / min, 200r / min, 210r / min, 220r / min or any value between 180r / min and 220r / min.

[0103] m. During the first coprecipitation reaction, the pH was 10-13; during the second coprecipitation reaction, the pH control range of the system was: the pH within 2 days of the reaction was 10.3-10.8, and the pH from 3 days to the end of the reaction was 11.4-12;

[0104] Optionally, during the first coprecipitation reaction, the pH may be 10, 10.1, 10.2, 10.3, 10.4, 10.5, 10.6, 10.7, 10.8, 10.9, 11, 11.1, 11.2, 11.3, 11.4, 11.5, 11.6, 11.7, 11.8, 11.9, 12, 12.1, 12.2, 12.3, 12.4, 12.5, 12.6, 12.7, 12.8, 12.9 , 13 or any value between 10-13; during the second coprecipitation reaction, the system pH control range is: the pH within 2 days of the reaction can be 10.3, 10.4, 10.5, 10.6, 10.7, 10.8 or any value between 10.3-10.8, and the pH from 3 days to the end of the reaction can be 11.4, 11.5, 11.6, 11.7, 11.8, 11.9, 12 or any value between 11.4-12;

[0105] n. The seed crystal particle size is 3μm-7μm;

[0106] Optionally, the particle size of the seed crystal may be 3 μm, 4 μm, 5 μm, 6 μm, 7 μm or any value between 3 μm and 7 μm;

[0107] o. After the first coprecipitation reaction is completed, the seed crystal having a water content of less than or equal to 25% is obtained by solid-liquid separation;

[0108] p. The particle size of the nickel-cobalt hydroxide is not less than 12 μm;

[0109] q. After the second coprecipitation reaction, the step further comprises: sequentially washing the reaction product with alkali, washing with water, solid-liquid separation and drying;

[0110] The concentration of the sodium hydroxide aqueous solution used in the alkali washing is 3wt%-10wt%; the drying temperature is 90°C-150°C.

[0111] Optionally, the concentration of the sodium hydroxide aqueous solution used for the alkali washing can be 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt% or any value between 3wt% and 10wt%; the drying temperature can be 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C or any value between 90°C and 150°C.

[0112] The present application also provides a nickel-cobalt oxide, the nickel-cobalt oxide comprising a first region, a second region and a third region, the second region covers the first region, and the third region covers the second region;

[0113] The porosity of the second region is greater than the porosity of the first region, and the porosity of the second region is greater than or equal to the porosity of the third region.

[0114] In an optional embodiment, the nickel cobalt oxide satisfies at least one of the following conditions:

[0115] r. The porosity of the first region is 3%-10%, the porosity of the second region is 15%-25%, and the porosity of the third region is 5%-15%;

[0116] Optionally, the porosity of the first region may be 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10% or any value between 3% and 10%, the porosity of the second region may be 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25% or any value between 15% and 25%, and the porosity of the third region may be 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15% or any value between 5% and 15%;

[0117] s. The diameter of the first region is 3 μm-6 μm, the diameter of the second region is 5 μm-14 μm, and the diameter of the third region is 10 μm-16 μm;

[0118] Optionally, the diameter of the first region may be 3 μm, 4 μm, 5 μm, 6 μm or any value between 3 μm and 6 μm, the diameter of the second region may be 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm or any value between 5 μm and 14 μm, and the diameter of the third region may be 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, 16 μm or any value between 10 μm and 16 μm;

[0119] t. The (D95-D5) / D50 of the nickel cobalt oxide is 0.18-0.32;

[0120] u. The peak intensity ratio (I012:I101) of the nickel cobalt oxide is not less than 1.4, the half-peak width of 101 is 0.50-0.85, and the half-peak width of 012 is 0.60-0.95;

[0121] Optionally, the (D95-D5) / D50 of the nickel cobalt oxide may be 0.18, 0.19, 0.20, 0.21, 0.22, 0.23, 0.24, 0.25, 0.26, 0.27, 0.28, 0.29, 0.30, 0.31, 0.32 or any value between 0.18 and 0.32; the 101 half-peak width may be 0.50, 0.55, 0.60, 0.65, 0.70, 0.75, 0.80, 0.85 or any value between 0.50 and 0.85, and the 012 half-peak width may be 0.60, 0.65, 0.70, 0.75, 0.80, 0.85, 0.90, 0.95 or any value between 0.60 and 0.95;

[0122] v. The molecular formula of the nickel cobalt oxide is Ni y Co (1-y) O, where 0.8≤y<1.0.

[0123] In an optional embodiment, the nickel cobalt oxide is obtained by sintering nickel cobalt hydroxide, and the nickel cobalt hydroxide includes a core region, a middle region and a shell region, the middle region covers the core region, and the shell region covers the middle region; the porosity of the middle region is greater than the porosity of the core region and the porosity of the shell region;

[0124] In an optional embodiment, the firing satisfies at least one of the following conditions:

[0125] w. The firing temperature is 400 ℃ -600 ℃;

[0126] x. During the firing process, the feed rate of the kiln is 200kg / h-500kg / h, and the air volume of the kiln is 400m 3 / h-600m 3 / h, the kiln speed is 1r / min-6r / min.

[0127] Firing is the process of sintering and oxidizing hydroxide into oxide under a certain gas atmosphere by adjusting the appropriate temperature and time, and giving it a specific structure. The gas atmosphere is controlled by the air volume in and out of the kiln. The temperature and time during the sintering process will affect the sintering effect. If the temperature is too low and the time is too short, the material will not be oxidized enough. If the temperature is too high and the time is too long, the material will be over-oxidized and its structure will be destroyed. The sintering time in the kiln is controlled by the kiln speed.

[0128] Optionally, the firing temperature may be 400°C, 500°C, 600°C or any value between 400°C and 600°C; during the firing process, the feed rate of the kiln may be 200kg / h, 250kg / h, 300kg / h, 350kg / h, 400kg / h, 450kg / h, 500kg / h or any value between 200kg / h and 500kg / h, and the air volume of the kiln may be 400m 3 / h、500m 3 / h、600m 3 / h or 400m 3 / h-600m 3 / h, the kiln speed can be any value between 1r / min, 1.5r / min, 2r / min, 2.5r / min, 3r / min, 3.5r / min, 4r / min, 4.5r / min, 5r / min, 5.5r / min, 6r / min or any value between 1r / min-6r / min.

[0129] The present application also provides a lithium-ion battery positive electrode material, the raw materials of which include the nickel cobalt hydroxide or the nickel cobalt oxide.

[0130] The present application also provides a lithium-ion battery positive electrode, the raw materials of which include the lithium-ion battery positive electrode material.

[0131] The present application also provides a lithium-ion battery, comprising the lithium-ion battery positive electrode.

[0132] The present application also provides an electrical device, comprising the lithium-ion battery or powered by the lithium-ion battery.

[0133] The embodiments of the present application will be described in detail below in conjunction with specific examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If specific conditions are not specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0134] Example 1

[0135] (1) A certain amount of nickel sulfate crystals and cobalt sulfate crystals are dissolved in water and mixed to prepare a mixed metal salt solution with a nickel-cobalt ratio of 92:8 and a metal concentration of 110 g / L.

[0136] (2) Add 8m 3 Water and appropriate amount of liquid alkali and ammonia water are added to adjust the pH to 12.0, and then the reaction is started at a speed of 200r / min. During the reaction, the flow rate of binary solution is 400L / h, the flow rate of liquid alkali is 200L / h, and the flow rate of ammonia water is 30L / h. Under the condition of maintaining the reaction temperature at 60°C, a co-precipitation reaction is carried out to obtain seed crystals with a particle size of 5.0μm.

[0137] (3) Dehydrate the seed crystals using a centrifuge to obtain a wet seed crystal material having a moisture content of about 20%.

[0138] (4) An intermittent reaction was performed, and 150 kg of seed crystals were placed in a reactor to which liquid alkali and ammonia water had been added. The reaction was started at a speed of 200 r / min. During the reaction, the flow rate of the binary solution was 500 L / h, the flow rate of the liquid alkali was 200 L / h, and the flow rate of the ammonia water was 30 L / h. The reaction temperature was maintained at 50°C and the pH was 10.5. A coprecipitation reaction was performed to allow the seed crystals to grow slowly. The pH was adjusted to 11.4 in the later stage (3d-5d) to prepare nickel cobalt hydroxide with a particle size of 16 μm.

[0139] (5) The nickel-cobalt hydroxide slurry is alkali-washed and water-washed with 10% dilute alkali and pure water respectively, and finally dehydrated to obtain a wet material with a moisture content of about 10%.

[0140] (6) Drying the nickel cobalt hydroxide wet material in an oven at 120° C. to finally obtain a nickel cobalt hydroxide product.

[0141] (7) The nickel-cobalt hydroxide is heated in a kiln at 600°C with a feed rate of 300 kg / h and an air volume of 600 m / s. 3 / h, and the kiln speed was 2r / min, a nickel-cobalt oxide with special pores was prepared.

[0142] Figure 2 This is a multiple narrow peak analysis particle size distribution diagram of the nickel cobalt hydroxide obtained in Example 1; Figure 3 This is a particle size distribution diagram of the nickel-cobalt oxide obtained in Example 1 through multiple narrow peak analysis; Figure 4 The XRD pattern of the nickel cobalt hydroxide obtained in Example 1; Figure 5 This is the XRD spectrum of the nickel-cobalt oxide obtained in Example 1.

[0143] Figure 6 This is a surface electron microscope photograph of the nickel-cobalt hydroxide obtained in Example 1. Figure 7 This is a cross-sectional electron microscope photograph of the nickel-cobalt hydroxide obtained in Example 1. Figure 6 and Figure 7 It can be seen that the nickel cobalt hydroxide product obtained in Example 1 has a smooth and dense surface morphology, and the primary particles grow from the inside to the outside; the interior of the product is a three-layer structure, which is the inner core area, the middle area and the outer shell area from the inside to the outside.

[0144] Figure 8 This is a surface electron microscope photograph of the nickel-cobalt oxide obtained in Example 1. Fig. 9 This is a cross-sectional electron microscope photograph of the nickel-cobalt oxide obtained in Example 1. Fig.10 This is a high-power cross-sectional electron microscope photograph of the nickel-cobalt oxide obtained in Example 1. Figures 8 to 10 It can be seen that the surface morphology of the nickel-cobalt oxide obtained in Example 1 is smooth and dense, the primary particles are crisscrossed and have microcracks; from the inside to the outside, they are the first region, the second region and the third region.

[0145] Example 2

[0146] (1) A certain amount of nickel sulfate crystals and cobalt sulfate crystals are dissolved in water and mixed to prepare a mixed metal salt solution with a nickel-cobalt ratio of 93:7 and a metal concentration of 110 g / L.

[0147] (2) Add 8m 3 Water and appropriate amount of liquid alkali and ammonia water are added to adjust the pH to 12.0, and then the reaction is started at a speed of 200r / min. During the reaction, the flow rate of binary solution is 400L / h, the flow rate of liquid alkali is 200L / h, and the flow rate of ammonia water is 30L / h. Under the condition of maintaining the reaction temperature at 60°C, a co-precipitation reaction is carried out to obtain seed crystals with a particle size of 5.0μm.

[0148] (3) Dehydrate the seed crystals using a centrifuge to obtain a wet seed crystal material having a moisture content of about 20%.

[0149] (4) An intermittent reaction was performed, and 150 kg of seed crystals were placed in a reactor to which liquid alkali and ammonia water had been added. The reaction was started at a speed of 200 r / min. During the reaction, the flow rate of the binary solution was 500 L / h, the flow rate of the liquid alkali was 200 L / h, and the flow rate of the ammonia water was 30 L / h. The reaction temperature was maintained at 50°C and the pH was 10.5. A coprecipitation reaction was performed to allow the seed crystals to grow slowly. The pH was adjusted to 11.4 in the later stage (3d-5d) to prepare nickel cobalt hydroxide with a particle size of 16 μm.

[0150] (5) The nickel-cobalt hydroxide slurry is alkali-washed and water-washed with 10% dilute alkali and pure water respectively, and finally dehydrated to obtain a wet material with a moisture content of about 10%.

[0151] (6) Drying the nickel cobalt hydroxide wet material in an oven at 120° C. to finally obtain a nickel cobalt hydroxide product.

[0152] (7) The nickel-cobalt hydroxide is heated in a kiln at 600°C with a feed rate of 300 kg / h and an air volume of 600 m / s. 3 / h, and the kiln speed was 2r / min, a nickel-cobalt oxide with special pores was prepared.

[0153] Example 3

[0154] (1) A certain amount of nickel sulfate crystals and cobalt sulfate crystals are dissolved in water and mixed to prepare a mixed metal salt solution with a nickel-cobalt ratio of 92:8 and a metal concentration of 110 g / L.

[0155] (2) Add 8m 3 Water and appropriate amount of liquid alkali and ammonia water are added to adjust the pH to 12.0, and then the reaction is started at a speed of 200r / min. During the reaction, the flow rate of binary solution is 400L / h, the flow rate of liquid alkali is 200L / h, and the flow rate of ammonia water is 30L / h. Under the condition of maintaining the reaction temperature at 60°C, a co-precipitation reaction is carried out to obtain seed crystals with a particle size of 5.0μm.

[0156] (3) Dehydrate the seed crystals using a centrifuge to obtain a wet seed crystal material having a moisture content of about 20%.

[0157] (4) An intermittent reaction was performed, and 150 kg of seed crystals were put into a reactor to which liquid alkali and ammonia water had been added. The reaction was started at a speed of 200 r / min. During the reaction, the flow rate of the binary solution was 300 L / h, the flow rate of the liquid alkali was 150 L / h, and the flow rate of the ammonia water was 25 L / h. The reaction temperature was maintained at 50°C and the pH was 10.5. A coprecipitation reaction was performed to allow the seed crystals to grow slowly. The pH was adjusted to 11.4 in the later stage (3d-5d) to prepare nickel cobalt hydroxide with a particle size of 16 μm.

[0158] (5) The nickel-cobalt hydroxide slurry is alkali-washed and water-washed with 10% dilute alkali and pure water respectively, and finally dehydrated to obtain a wet material with a moisture content of about 10%.

[0159] (6) Drying the nickel cobalt hydroxide wet material in an oven at 120° C. to finally obtain a nickel cobalt hydroxide product.

[0160] (7) The nickel-cobalt hydroxide is heated in a kiln at 600°C with a feed rate of 300 kg / h and an air volume of 600 m / s. 3 / h, and the kiln speed was 2r / min, a nickel-cobalt oxide with special pores was prepared.

[0161] Example 4

[0162] (1) A certain amount of nickel sulfate crystals and cobalt sulfate crystals are dissolved in water and mixed to prepare a mixed metal salt solution with a nickel-cobalt ratio of 92:8 and a metal concentration of 110 g / L.

[0163] (2) Add 8m 3 Water and appropriate amount of liquid alkali and ammonia water are added to adjust the pH to 12.0, and then the reaction is started at a speed of 200r / min. During the reaction, the flow rate of binary solution is 400L / h, the flow rate of liquid alkali is 200L / h, and the flow rate of ammonia water is 30L / h. Under the condition of maintaining the reaction temperature at 60°C, a co-precipitation reaction is carried out to obtain seed crystals with a particle size of 5.0μm.

[0164] (3) Dehydrate the seed crystals using a centrifuge to obtain a wet seed crystal material having a moisture content of about 20%.

[0165] (4) An intermittent reaction was performed, and 150 kg of seed crystals were put into a reactor to which liquid alkali and ammonia water had been added. The reaction was started at a speed of 200 r / min. During the reaction, the flow rate of the binary solution was 500 L / h, the flow rate of the liquid alkali was 200 L / h, and the flow rate of the ammonia water was 30 L / h. The reaction temperature was maintained at 50°C and the pH was 10.7. A coprecipitation reaction was performed to allow the seed crystals to grow slowly. The pH was adjusted to 11.8 in the later stage (3d-5d) to prepare nickel cobalt hydroxide with a particle size of 16 μm.

[0166] (5) The nickel-cobalt hydroxide slurry is alkali-washed and water-washed with 10% dilute alkali and pure water respectively, and finally dehydrated to obtain a wet material with a moisture content of about 10%.

[0167] (6) Drying the nickel cobalt hydroxide wet material in an oven at 120° C. to finally obtain a nickel cobalt hydroxide product.

[0168] (7) The nickel-cobalt hydroxide is heated in a kiln at 600°C with a feed rate of 300 kg / h and an air volume of 600 m / s.3 / h, and the kiln speed was 2r / min, a nickel-cobalt oxide with special pores was prepared.

[0169] Example 5

[0170] (1) A certain amount of nickel sulfate crystals and cobalt sulfate crystals are dissolved in water and mixed to prepare a mixed metal salt solution with a nickel-cobalt ratio of 92:8 and a metal concentration of 110 g / L.

[0171] (2) Add 8m 3 Water and appropriate amount of liquid alkali and ammonia water are added to adjust the pH to 12.0, and then the reaction is started at a speed of 200r / min. During the reaction, the flow rate of binary solution is 400L / h, the flow rate of liquid alkali is 200L / h, and the flow rate of ammonia water is 30L / h. Under the condition of maintaining the reaction temperature at 60°C, a co-precipitation reaction is carried out to obtain seed crystals with a particle size of 5.0μm.

[0172] (3) Dehydrate the seed crystals using a centrifuge to obtain a wet seed crystal material having a moisture content of about 20%.

[0173] (4) An intermittent reaction was performed, and 150 kg of seed crystals were put into a reactor to which liquid alkali and ammonia water had been added. The reaction was started at a speed of 180 r / min. During the reaction, the flow rate of the binary solution was 500 L / h, the flow rate of the liquid alkali was 200 L / h, and the flow rate of the ammonia water was 30 L / h. The reaction temperature was maintained at 50°C and the pH was 10.5. A coprecipitation reaction was performed to allow the seed crystals to grow slowly. The pH was adjusted to 11.4 in the later stage (3d-5d) to prepare nickel cobalt hydroxide with a particle size of 16 μm.

[0174] (5) The nickel-cobalt hydroxide slurry is alkali-washed and water-washed with 10% dilute alkali and pure water respectively, and finally dehydrated to obtain a wet material with a moisture content of about 10%.

[0175] (6) Drying the nickel cobalt hydroxide wet material in an oven at 120° C. to finally obtain a nickel cobalt hydroxide product.

[0176] (7) The nickel-cobalt hydroxide is heated in a kiln at 600°C with a feed rate of 300 kg / h and an air volume of 600 m / s. 3 / h, and the kiln speed was 2r / min, a nickel-cobalt oxide with special pores was prepared.

[0177] Comparative Example 1

[0178] (1) A certain amount of nickel sulfate crystals and cobalt sulfate crystals are dissolved in water and mixed to prepare a mixed metal salt solution with a nickel-cobalt ratio of 92:8 and a metal concentration of 110 g / L.

[0179] (2) Add 8m3 Water and appropriate amount of liquid alkali and ammonia water are added to adjust the pH to 12.0, and then the reaction is started at a speed of 200r / min. During the reaction, the flow rate of binary solution is 400L / h, the flow rate of liquid alkali is 200L / h, and the flow rate of ammonia water is 30L / h. Under the condition of maintaining the reaction temperature at 60°C, a co-precipitation reaction is carried out to obtain seed crystals with a particle size of 5.0μm.

[0180] (3) Dehydrate the seed crystals using a centrifuge to obtain a wet seed crystal material having a moisture content of about 20%.

[0181] (4) A batch reaction was performed, 150 kg of seed crystals were put into a reactor to which liquid alkali and ammonia water had been added, and the reaction was started at a speed of 200 r / min. During the reaction, the flow rate of the binary solution was 500 L / h, the flow rate of the liquid alkali was 200 L / h, and the flow rate of the ammonia water was 30 L / h. The reaction temperature was maintained at 50° C. and the pH was 10.5 (throughout the process), and a coprecipitation reaction was performed to allow the seed crystals to grow slowly, thereby preparing nickel cobalt hydroxide with a particle size of 16 μm.

[0182] (5) The nickel-cobalt hydroxide slurry is alkali-washed and water-washed with 10% dilute alkali and pure water respectively, and finally dehydrated to obtain a wet material with a moisture content of about 10%.

[0183] (6) Drying the nickel cobalt hydroxide wet material in an oven at 120° C. to finally obtain a nickel cobalt hydroxide product.

[0184] (7) The nickel-cobalt hydroxide is heated in a kiln at 600°C with a feed rate of 300 kg / h and an air volume of 600 m / s. 3 / h, and the kiln speed was 2r / min, a nickel-cobalt oxide with special pores was prepared.

[0185] Comparative Example 2

[0186] (1) A certain amount of nickel sulfate crystals and cobalt sulfate crystals are dissolved in water and mixed to prepare a mixed metal salt solution with a nickel-cobalt ratio of 92:8 and a metal concentration of 110 g / L.

[0187] (2) Add 8m 3 Water and appropriate amount of liquid alkali and ammonia water are added to adjust the pH to 12.0, and then the reaction is started at a speed of 200r / min. During the reaction, the flow rate of binary solution is 400L / h, the flow rate of liquid alkali is 200L / h, and the flow rate of ammonia water is 30L / h. Under the condition of maintaining the reaction temperature at 60°C, a co-precipitation reaction is carried out to obtain seed crystals with a particle size of 5.0μm.

[0188] (3) Dehydrate the seed crystals using a centrifuge to obtain a wet seed crystal material having a moisture content of about 20%.

[0189] (4) A batch reaction was performed, 150 kg of seed crystals were put into a reactor to which liquid alkali and ammonia water had been added, and the reaction was started at a speed of 200 r / min. During the reaction, the flow rate of the binary solution was 500 L / h, the flow rate of the liquid alkali was 200 L / h, and the flow rate of the ammonia water was 30 L / h. The reaction temperature was maintained at 50° C. and the pH was 11.4 (throughout the process), and a coprecipitation reaction was performed to allow the seed crystals to grow slowly, thereby preparing nickel cobalt hydroxide with a particle size of 16 μm.

[0190] (5) The nickel-cobalt hydroxide slurry is alkali-washed and water-washed with 10% dilute alkali and pure water respectively, and finally dehydrated to obtain a wet material with a moisture content of about 10%.

[0191] (6) Drying the nickel cobalt hydroxide wet material in an oven at 120° C. to finally obtain a nickel cobalt hydroxide product.

[0192] (7) The nickel-cobalt hydroxide is heated in a kiln at 600°C with a feed rate of 300 kg / h and an air volume of 600 m / s. 3 / h, and the kiln speed was 2r / min, a nickel-cobalt oxide with special pores was prepared.

[0193] Comparative Example 3

[0194] (1) A certain amount of nickel sulfate crystals and cobalt sulfate crystals are dissolved in water and mixed to prepare a mixed metal salt solution with a nickel-cobalt ratio of 92:8 and a metal concentration of 110 g / L.

[0195] (2) Add 8m 3 Water and appropriate amount of liquid alkali and ammonia water are added to adjust the pH to 12.0, and then the reaction is started at a speed of 200r / min. During the reaction, the flow rate of binary solution is 400L / h, the flow rate of liquid alkali is 200L / h, and the flow rate of ammonia water is 30L / h. Under the condition of maintaining the reaction temperature at 60°C, a co-precipitation reaction is carried out to obtain seed crystals with a particle size of 5.0μm.

[0196] (3) Dehydrate the seed crystals using a centrifuge to obtain a wet seed crystal material having a moisture content of about 20%.

[0197] (4) An intermittent reaction was performed, and 150 kg of seed crystals were put into a reactor to which liquid alkali and ammonia water had been added. The reaction was started at a speed of 200 r / min. During the reaction, the flow rate of the binary solution was 500 L / h, the flow rate of the liquid alkali was 200 L / h, and the flow rate of the ammonia water was 30 L / h. The reaction temperature was maintained at 50°C and the pH was 11.4. A coprecipitation reaction was performed to allow the seed crystals to grow slowly. The pH was adjusted to 10.5 in the later stage (3d-5d) to prepare nickel cobalt hydroxide with a particle size of 16 μm.

[0198] (5) The nickel-cobalt hydroxide slurry is alkali-washed and water-washed with 10% dilute alkali and pure water respectively, and finally dehydrated to obtain a wet material with a moisture content of about 10%.

[0199] (6) Drying the nickel cobalt hydroxide wet material in an oven at 120° C. to finally obtain a nickel cobalt hydroxide product.

[0200] (7) The nickel-cobalt hydroxide is heated in a kiln at 600°C with a feed rate of 300 kg / h and an air volume of 600 m / s. 3 / h, and the kiln speed was 2r / min, a nickel-cobalt oxide with special pores was prepared.

[0201] Comparative Example 4

[0202] (1) A certain amount of nickel sulfate crystals and cobalt sulfate crystals are dissolved in water and mixed to prepare a mixed metal salt solution with a nickel-cobalt ratio of 92:8 and a metal concentration of 110 g / L.

[0203] (2) Add 8m 3 Water and appropriate amount of liquid alkali and ammonia water are added to adjust the pH to 12.0, and then the reaction is started at a speed of 200r / min. During the reaction, the flow rate of binary solution is 400L / h, the flow rate of liquid alkali is 200L / h, and the flow rate of ammonia water is 30L / h. Under the condition of maintaining the reaction temperature at 60°C, a co-precipitation reaction is carried out to obtain seed crystals with a particle size of 5.0μm.

[0204] (3) Dehydrate the seed crystals using a centrifuge to obtain a wet seed crystal material having a moisture content of about 20%.

[0205] (4) An intermittent reaction was performed, and 150 kg of seed crystals were placed in a reactor to which liquid alkali and ammonia water had been added. The reaction was started at a speed of 200 r / min. During the reaction, the flow rate of the binary solution was 500 L / h, the flow rate of the liquid alkali was 200 L / h, and the flow rate of the ammonia water was 30 L / h. The reaction temperature was maintained at 50° C. and the pH was 10.5. A coprecipitation reaction was performed to allow the seed crystals to grow slowly. The pH was adjusted to 11.4 in the later stage (4d-5d) to prepare nickel cobalt hydroxide with a particle size of 16 μm.

[0206] (5) The nickel-cobalt hydroxide slurry is alkali-washed and water-washed with 10% dilute alkali and pure water respectively, and finally dehydrated to obtain a wet material with a moisture content of about 10%.

[0207] (6) Drying the nickel cobalt hydroxide wet material in an oven at 120° C. to finally obtain a nickel cobalt hydroxide product.

[0208] (7) The nickel-cobalt hydroxide is heated in a kiln at 600°C with a feed rate of 300 kg / h and an air volume of 600 m / s.3 / h, and the kiln speed was 2r / min, a nickel-cobalt oxide with special pores was prepared.

[0209] Fig.11 The cross-sectional electron microscope photos of the nickel-cobalt hydroxide obtained in Comparative Examples 1 to 4 are shown in FIG. 1 , the upper left corresponds to Comparative Example 1, the upper right corresponds to Comparative Example 2, the lower left corresponds to Comparative Example 3, and the lower right corresponds to Comparative Example 4.

[0210] The hydroxide materials obtained in Examples 1-5 and Comparative Examples 1-4 were prepared into half-cells for testing. The results are shown in Table 1, Table 2, and Table 3 below:

[0211] Table 1 Material test results

[0212]

[0213]

[0214] Table 2 Material test results

[0215]

[0216]

[0217] After many tests, the (D95-D5) / D50 of the nickel cobalt hydroxide obtained by the preparation method provided in the present application is 0.35-0.5, and the (D95-D5) / D50 of the nickel cobalt oxide is 0.18-0.32; the peak intensity ratio (I101:I001) of the nickel cobalt hydroxide is above 1.1, preferably 1.2-1.5, the 001 half-peak width is 0.5-0.9, and the 101 half-peak width is 0.45-0.85; the peak intensity ratio (I012:I101) of the nickel cobalt oxide is not less than 1.4, the 101 half-peak width is 0.50-0.85, and the 012 half-peak width is 0.60-0.95.

[0218] After multiple measurements of nickel cobalt hydroxide, the average data was obtained. The diameter of the inner core zone is 3-6μm, with a porous structure, no stripes or cracks, and a porosity of 1%-5%; the diameter of the middle zone is 5-14μm, with a porous structure, radial stripes, and a porosity of 5%-10%; the diameter of the outer shell zone is 10-16μm, with a porous structure, no stripes or cracks, and a porosity of 1%-5%.

[0219] After multiple measurements of the nickel cobalt oxide obtained in this application, the average data was obtained. The diameter of the first area is 3-6μm, which is a porous structure with a small amount of stripes and cracks, and the porosity is 3%-10%; the stripe width is 0-0.05μm; the diameter of the second area is 5-14μm, which is a porous structure with special radial stripes, the porosity is 15%-25%, and the stripe width is 0-0.25μm; the diameter of the third area is 10-16μm, which is a porous structure with a small amount of stripes and cracks, the porosity is 5%-15%, and the stripe width is 0-0.05μm.

[0220] It should be noted that in order to evaluate the characteristics of porosity, this application uses image analysis software (ImageJ) to directly calculate the pore area and cross-sectional area of ​​each region. The porosity of different regions is calculated by porosity = pore area of ​​each region / cross-sectional area of ​​each region × 100%. The porosity referred to in this application is characterized by this method.

[0221] Table 3 Battery performance test results

[0222]

[0223] As can be seen from Tables 1, 2 and 3 above, the half-cell prepared from the materials obtained in the embodiment has an average 0.1C first charge capacity of about 245 mAh / g, which is about 20 mAh / g higher than the comparative example. The average 0.1C first discharge capacity is about 214 mAh / g, which is about 15 mAh / g higher than the comparative example. The average capacity retention rate after 50 cycles at 1C is about 97%, which is about 8% higher than the comparative example. The average rate performance (1C / 0.1C) is about 93%, which is about 6% higher than the comparative example.

[0224] At the same time, by comparing Example 1 with Comparative Example 1, Comparative Example 2, Comparative Example 3 and Comparative Example 4, it can be shown that in the process of preparing nickel cobalt hydroxide by the intermittent method in step 4, the control of pH in the early stage (0-2d) and the later stage (3d-5d) has a greater impact on the product structure.

[0225] This proves that the hydroxide material with a special pore structure provided in the present application can significantly improve the battery capacity, cycle performance, and rate performance compared to hydroxide materials with a general structure.

[0226] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.

[0227] In addition, those skilled in the art will appreciate that, although some embodiments herein include certain features included in other embodiments but not other features, the combination of features of different embodiments is meant to be within the scope of the present application and form different embodiments. For example, in the above claims, any one of the claimed embodiments may be used in any combination. The information disclosed in this background technology section is intended only to deepen the understanding of the overall background technology of the present application and should not be regarded as an admission or in any form of implication that the information constitutes prior art known to those skilled in the art.

Claims

1. A nickel-cobalt hydroxide, It is characterized in that It comprises an inner core region, a middle region and an outer shell region, wherein the middle region covers the inner core region, and the outer shell region covers the middle region; The porosity of the middle region is greater than the porosity of the inner core region and the porosity of the outer shell region; The porosity of the middle zone is 5%-10%, and the porosity of the inner core zone and the porosity of the outer shell zone are each independently 1%-5%; The peak intensity ratio (I101:I001) of the nickel cobalt hydroxide is not less than 1.

1.

2. The nickel cobalt hydroxide according to claim 1, It is characterized in that The nickel cobalt hydroxide satisfies at least one of the following conditions: b. The pores in the inner core area are distributed in a network shape, the pores in the middle area are radially divergent toward the outer shell area, and the pores in the outer shell area are distributed in a scattered point shape; c. The diameter of the inner core region is 3μm -6μm; d. The diameter of the intermediate region is 5 μm -14 μm; e. The diameter of the shell region is 10μm -16μm; g. The peak intensity ratio (I101:I001) of the nickel cobalt hydroxide is 1.2-1.5; h. The 001 half-peak width of the nickel cobalt hydroxide is 0.5-0.9, and the 101 half-peak width is 0.45-0.85; i. The (D95-D5) / D50 of the nickel cobalt hydroxide is 0.35-0.

5.

3. The nickel-cobalt hydroxide according to claim 1 or 2, It is characterized in that Its molecular formula is Ni x Co (1-x) (OH) 2 , where 0.8≤x<1.

0.

4. A method for preparing the nickel-cobalt hydroxide according to any one of claims 1 to 3, It is characterized in that include: Mixing raw materials including a nickel-cobalt binary aqueous solution, a sodium hydroxide aqueous solution, and ammonia water, and obtaining seed crystals through a first coprecipitation reaction; Mixing raw materials including the seed crystal, a nickel-cobalt binary aqueous solution, a sodium hydroxide aqueous solution and ammonia water, and obtaining the nickel-cobalt hydroxide through a second coprecipitation reaction; The flow rate of the sodium hydroxide aqueous solution is independently 60 L / h-250 L / h, and the flow rate of the ammonia water is independently 10 L / h-50 L / h; During the first coprecipitation reaction, the pH was 10-13; during the second coprecipitation reaction, the system pH control range was: the pH within 2 days of the reaction was 10.3-10.8, and the pH from 3 days to the end of the reaction was 11.4-12.

5. The preparation method according to claim 4, It is characterized in that The preparation method satisfies at least one of the following conditions: j. The concentration of the nickel-cobalt binary aqueous solution is 80g / L-120g / L; k. During the first coprecipitation reaction and the second coprecipitation reaction, the flow rate of the nickel-cobalt binary aqueous solution is independently 300L / h-600L / h; l. During the first coprecipitation reaction and the second coprecipitation reaction, the temperature is independently 40°C-60°C, and the stirring speed is independently 180r / min-220r / min; n. The seed crystal particle size is 3μm-7μm; o. After the first coprecipitation reaction is completed, the seed crystal having a water content of less than or equal to 25% is obtained by solid-liquid separation; p. The particle size of the nickel-cobalt hydroxide is not less than 12 μm; q. After the second coprecipitation reaction, the step further comprises: sequentially washing the reaction product with alkali, washing with water, solid-liquid separation and drying; The concentration of the sodium hydroxide aqueous solution used in the alkali washing is 3wt%-10wt%; the drying temperature is 90°C-150°C.

6. A nickel-cobalt oxide, It is characterized in that The nickel-cobalt oxide includes a first region, a second region and a third region, the second region covers the first region, and the third region covers the second region; The porosity of the second region is greater than that of the first region, and the porosity of the second region is greater than or equal to that of the third region; the porosity of the first region is 3%-10%, the porosity of the second region is 15%-25%, and the porosity of the third region is 5%-15%; The peak intensity ratio (I012:I101) of the nickel-cobalt oxide is not less than 1.

4.

7. The nickel-cobalt oxide according to claim 6, It is characterized in that The nickel-cobalt oxide satisfies at least one of the following conditions: s. The diameter of the first region is 3 μm-6 μm, the diameter of the second region is 5 μm-14 μm, and the diameter of the third region is 10 μm-16 μm; t. The (D95-D5) / D50 of the nickel-cobalt oxide is 0.18-0.32; u. The 101 half-peak width of the nickel cobalt oxide is 0.50-0.85, and the 012 half-peak width is 0.60-0.95; v. The molecular formula of the nickel-cobalt oxide is Ni y Co (1-y) O, where 0.8≤y<1.

0.

8. The nickel-cobalt oxide according to claim 6 or 7, It is characterized in that The nickel cobalt oxide is obtained by sintering nickel cobalt hydroxide, and the nickel cobalt hydroxide includes an inner core region, an intermediate region and an outer shell region, wherein the intermediate region covers the inner core region, and the outer shell region covers the intermediate region; and the porosity of the intermediate region is greater than the porosity of the inner core region and the porosity of the outer shell region.

9. The nickel-cobalt oxide according to claim 8, Features The firing satisfies at least one of the following conditions: w. The firing temperature is 400 ℃ -600 ℃; x. During the firing process, the feed rate of the kiln is 200kg / h-500kg / h, and the air volume of the kiln is 400m 3 / h-600m 3 / h, the kiln speed is 1r / min-6r / min.

10. A positive electrode material for a lithium-ion battery, It is characterized in that The raw material comprises the nickel-cobalt hydroxide described in any one of claims 1 to 3, or the nickel-cobalt oxide described in any one of claims 6 to 9.

11. A lithium ion battery positive electrode, It is characterized in that The raw materials include the lithium ion battery positive electrode material according to claim 10.

12. A lithium ion battery, It is characterized in that The lithium-ion battery positive electrode comprises the positive electrode of claim 11.

13. An electrical device, It is characterized in that Comprising the lithium ion battery of claim 12 or powered by the lithium ion battery of claim 12.