A high heat-resistant copolymer negative photoresist composition and preparation method thereof
The three-dimensional copolymer is formed by copolymerizing trifunctional silane monomers, which solves the problem of photoresist prone to yellowing and reduced light transmittance at high temperatures, achieves the improvement of high heat resistance and yellowing resistance, and extends the liquid crystal display panel service life.
Patent Information
- Application Number
- CN202111509236.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-10
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2041-12-10
AI Technical Summary
Existing photoresist tends to yellow and reduce light transmittance at high temperatures, which affects the life of the liquid crystal display panel. In addition, existing modified acrylic resins still have cracking and yellowing problems at long-term high temperatures, which is difficult to effectively solve.
The trifunctional silane monomer is used to form a three-dimensional copolymer. By copolymerizing cyclohexyltrimethoxysilane with a trifunctional silane monomer containing double bonds and carboxyl groups, the content of phenyl functional groups is reduced, and a high heat-resistant copolymerization negative property is formed. Photoresist composition.
It significantly improves the high temperature heat resistance and yellowing resistance of photoresist, extends the service life of the display panel, and reduces the cracking and yellowing speed of the resin.
Smart Images

Figure 773205DEST_PATH_IMAGE002
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of liquid crystal display, and in particular relates to a new photoresist material. Background Art
[0002] In a liquid crystal display panel, in order to maintain a certain unit spacing between two substrates, spacer particles such as glass beads with a fixed particle size are used. However, since these spacer particles are freely scattered on the glass substrate, if there are spacer particles in the image forming area, the spacer particles will be printed in, and the incident light will be scattered, which will reduce the contrast of the liquid crystal display panel. Therefore, in order to solve this problem, a method for forming spacers by photolithography is adopted. This method coats a photoresist composition on a substrate, develops through a prescribed mask and after ultraviolet exposure, and forms dot-shaped or stripe-shaped spacers. Since the spacers are formed only in a prescribed place outside the image forming area, the above-mentioned problem can be basically solved.
[0003] Generally speaking, the composition of this type of photoresist includes a photopolymerizable resin, a photopolymerizable monomer, a photoinitiator, a solvent and an auxiliary agent. The photocurable pattern is formed by cross-linking the monomer and the resin after exposure, and then through a development process. In order to improve the heat resistance of photoresist exposure in the prior art, the photopolymerizable resin in the photoresist often uses phenyl or diphenyl functional groups to improve its heat resistance, and the proportion of phenyl to other photoinitiated polymerization double bonds is usually 50~60%, or even more. However, the phenyl functional group is easily yellowed under high temperature, resulting in a decrease in light transmittance and affecting the life of the display panel. Therefore, most studies have adopted the method of reducing the use of phenyl functional groups or using other methods.
[0004] In addition, the curable photoresist used in the prior art usually contains acrylic resin that is prone to high temperature cracking and yellowing. As the device is used for a longer time, the light transmittance is easily reduced, affecting the service life of the display panel. The prior art discloses a silicone-modified acrylate photoresist (CN111413848A), the main film-forming resin of which is obtained by polymerizing acrylic acid derivative monomers and then modified by silicone. Its main structure is still acrylic polymer, and the main structure of its main acrylic resin cannot be changed. Its long-term high temperature cracking and yellowing problems are still obvious.
[0005] In order to solve the above problems, the industry has tried many methods, such as reducing the impurity content in acrylic resin, introducing high temperature resistant chemical components to modify acrylic resin, or adding a small amount of high temperature resistant additives, but none of them achieved the desired effect. Summary of the invention
[0006] Purpose of the invention: In view of the above-mentioned existing problems and shortcomings, the purpose of the present invention is to provide a high heat-resistant copolymer negative photoresist composition and a preparation method thereof, which adopts trifunctional silane monomer copolymerization, has excellent high-temperature heat resistance and anti-yellowing properties, and greatly improves the life of the display panel.
[0007] Technical solution: To achieve the above-mentioned invention object, the present invention adopts the following technical solution: a highly heat-resistant copolymer negative photoresist composition, comprising the following components in parts by weight:
[0008] 10~30 parts of alkali soluble light-curable silicone resin
[0009] 1.5~8 parts of alkali soluble acrylic monomer
[0010] Photoinitiator 0.5~2.5 parts
[0011] Surfactant 0.01~0.02 parts
[0012] and 12 to 60 parts of solvent;
[0013] The alkali-soluble light-curable silicone resin is a three-dimensional copolymer obtained by copolymerizing and cross-linking cyclohexyltrimethoxysilane, a trifunctional silane monomer containing a double bond and a trifunctional silane monomer containing a carboxyl group.
[0014] Among the photoresist components, photocurable silicone resins usually use siloxane silicone resins and acrylate resins as the main components of photoresists. In order to improve the thermal stability and high-temperature cracking problems of photoresists, the phenyl content on the siloxane monomer needs to be relatively high, usually exceeding 50%. However, if the phenyl content is too high, it is easy to cause yellowing of the photoresist and reduce the light transmittance of the photoresist. In this application, the cross-linked structure is formed by copolymerization of trifunctional siloxanes to improve its thermal stability, and at the same time, it is beneficial to reduce the content of components that are prone to yellowing and reduce the yellowing speed. In this application, phenyltrimethoxysilane can also be used as needed.
[0015] As a preferred embodiment, the trifunctional organosilane monomer containing a double bond is γ-methacryloxypropyltrimethoxysilane, acryloxypropyltrimethoxysilane or γ-methacryloxypropylmethyldimethoxysilane.
[0016] As a preferred embodiment, the carboxyl-containing trifunctional silane monomer is trimethoxysilyl propionic acid, triethoxysilyl propionic acid, trimethoxysilyl butyric acid or triethoxysilyl butyric acid.
[0017] As a preferred embodiment, the weight ratio of the cyclohexyltrimethoxysilane to the trifunctional silane monomer containing a double bond and the trifunctional silane monomer containing a carboxyl group is (30-40): (12-17): (12-17).
[0018] As a preferred embodiment, the alkali-soluble acrylic acid ester monomer is a combination of one or more of pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, and dipentaerythritol hexa(meth)acrylate modified by succinic anhydride. The present invention preferably uses pentaerythritol tri(meth)acrylate and pentaerythritol tetra(meth)acrylate modified by succinic anhydride, and other pentaerythritol acrylic acid ester monomer options have the same or similar functions and are also applicable.
[0019] As a preferred embodiment, the solvent is alcohol, ether, aromatic hydrocarbon, ketone, ester, preferably glycol ether, more preferably ethylene glycol alkyl ether acetate, diethylene glycol, propylene glycol monoalkyl ether, propylene glycol alkyl ether acetate, propylene glycol alkyl ether propionate.
[0020] As a preferred embodiment, the surfactant is a fluorine-based surfactant, a silicon-based surfactant or a nonionic surfactant.
[0021] The present invention also provides a method for preparing the above-mentioned high heat-resistant copolymer negative photoresist composition, comprising the following steps:
[0022] Step S1, preparation of alkali-soluble photocurable silicone resin: cyclohexyltrimethoxysilane, pure water and solvent are added to a reactor in proportion, and then an appropriate amount of phosphoric acid catalyst is added to perform a reflux stirring prepolymerization reaction for 2.5 to 6 hours;
[0023] Step S2, continue to add double bond-containing organic silane monomer and carboxyl-containing silane monomer, and add appropriate amount of pure water, and distill and stir to react at 75-85° C. for 2-4 hours;
[0024] Step S3, after cooling the obtained product, diluting it with a solvent to obtain an alkali-soluble light-curable silicone resin having a solid content of 20-50% and a weight average molecular weight of 5000-8000Da;
[0025] Step S4, uniformly mixing the alkali-soluble photocurable silicone resin, the alkali-soluble acrylate monomer, the photoinitiator and the surfactant, dissolving them in a solvent, and filtering to obtain a composition solution with a solid content of 16-25%.
[0026] Preferably, the organosilane monomer is cyclohexyltrimethoxysilane (monomer 1), the double bond-containing organosilane monomer is γ-methacryloxypropyltrimethoxysilane (monomer 2), the carboxyl-containing silane monomer is trimethoxysilylpropionic acid (monomer 3), and the solvent is propylene glycol monomethyl ether acetate (solvent).
[0027] Beneficial effects: Compared with the prior art, the present invention obtains a three-dimensional copolymer by copolymerizing trifunctional siloxane units containing double bonds and carboxyl groups, and significantly improves the thermal stability of the photoresist by replacing phenyl silane with cyclohexyltrimethoxysilane, reduces the amount of phenyl used in the alkali-soluble photocurable silicone resin, and further reduces the resin cracking and yellowing, thereby greatly improving the life of the display panel. DETAILED DESCRIPTION
[0028] The present invention is further explained below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. After reading the present invention, various equivalent forms of modifications to the present invention by those skilled in the art all fall within the scope defined by the claims attached to this application.
[0029] The negative photoresist composition of the present invention comprises: an alkali-soluble photocurable silicone resin (A); an alkali-soluble acrylate monomer (B); a solvent (C) and a photoinitiator (D). If necessary, the negative photoresist composition may further comprise (E) a surfactant. The weight average molecular weight of each component as described below is measured by gel permeation chromatography (GPC, eluent: tetrahydrofuran) using polystyrene standards.
[0030] Alkali-soluble photocurable silicone resin (A): The monomer used for polymerization of the alkali-soluble photocurable silicone resin (A) of the present invention is cyclohexyltrimethoxysilane, and the following two silane monomers are copolymerized: the γ-methacryloxypropyltrimethoxysilane, acryloxypropyltrimethoxysilane, γ-methacryloxypropylmethyldimethoxysilane; trimethoxysilylpropionic acid, triethoxysilylpropionic acid, trimethoxysilylbutyric acid, triethoxysilylbutyric acid;
[0031] The type and amount of the solvent or acid or base catalyst used in the present invention can be selected arbitrarily without limitation. The hydrolysis polymerization reaction can be carried out at 20° C. or lower. However, the reaction can be accelerated by heating or refluxing. The required reaction time varies with the type and concentration of the silane monomer, the reaction temperature, etc. The reaction is carried out until the molecular weight of the condensate obtained thereby becomes about 500 to 50,000 Da, usually requiring 30 minutes to 3 days. However, the reaction time is not limited to this range.
[0032] Acrylic acid ester monomer (B): The type and amount of the alkali-soluble acrylic acid ester monomer (B) of the present invention are not particularly limited. For example, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate and combinations thereof modified with succinic anhydride may be used.
[0033] Solvent (C): The solvent of the present invention is not particularly limited as long as it can dissolve the above components and is chemically stable. For example, the solvent can be alcohol, ether, glycol ether, ethylene glycol alkyl ether acetate, diethylene glycol, propylene glycol monoalkyl ether, propylene glycol alkyl ether acetate, propylene glycol alkyl ether propionate, aromatic hydrocarbons, ketones, esters, and the like. Further embodiments include methanol, ethanol, tetrahydrofuran, dioxane, methyl cellosolve acetate, ethyl cellosolve acetate, ethyl acetoacetate, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, propylene glycol dimethyl ether, propylene glycol diethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol dimethyl ether, diethylene glycol ethyl methyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, dipropylene glycol dimethyl ether, dipropylene glycol diethyl ether, propylene glycol Methyl ether acetate, propylene glycol ethyl ether acetate, propylene glycol propyl ether acetate, dipropylene glycol methyl ether acetate, propylene glycol butyl ether acetate, toluene, xylene, methyl ethyl ketone, 4-hydroxy-4-methyl-2-pentanone, cyclopentanone, cyclohexanone, 2-heptanone, γ-butyrolactone, ethyl 2-hydroxypropionate, ethyl 2-hydroxy-2-methylpropionate, ethyl acetate, butyl acetate, ethyl lactate, butyl lactate, N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, etc.
[0034] The most preferred solvents of the present invention are ethylene glycol alkyl ether acetate, diethylene glycol, propylene glycol monoalkyl ether, propylene glycol alkyl ether acetate, ketones, etc. Specifically, preferred are diethylene glycol dimethyl ether, diethylene glycol ethyl methyl ether, dipropylene glycol dimethyl ether, dipropylene glycol diethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol methyl ether acetate, 2-methoxypropionic acid methyl ester, etc. The preferred solvents described above can be used alone or in combination of two or more thereof.
[0035] Photoinitiator (D): refers to a component that generates active seeds that can initiate polymerization of (A) alkali-soluble photocurable silicone resin; (B) alkali-soluble acrylate monomers through exposure to visible light, ultraviolet light, electron beam, etc. The present invention is selected from IRGACURE907, IRGACURE369, etc. commercially available from BASF.
[0036] Surfactant (E): The negative photoresist of the present invention can improve the coating property of the photoresist by adding a surfactant, improve the properties of the photoresist on the silicon-based surface, and facilitate the subsequent removal of the photoresist. Fluorine-based surfactants, silicon-based surfactants, non-ionic surfactants, etc. can be selected. Specifically, S-112 of Asahi Glass Co., Ltd. can be selected.
[0037] Hereinafter, the present invention will be described in more detail with reference to the following examples. However, these examples are provided only to illustrate the specific technical content of the present invention, and the protection scope of the present invention is not limited thereto. In the following synthetic examples, the weight average molecular weight of the present invention is determined by gel permeation chromatography (GPC) using polystyrene standard deviation.
[0038] 1. Synthesis and preparation of alkali-soluble light-curable silicone resin (A):
[0039] Synthesis Example 1:
[0040] 35 wt % of cyclohexyl trimethoxy silane and 10 wt % of pure water were loaded into a reactor equipped with a reflux condenser. 20 wt % of propylene glycol monomethyl ether acetate was added thereto, followed by 0.1 wt % of phosphoric acid catalyst in the presence of the total weight of the mixture, the mixture was refluxed and stirred for 3.5 hours, then 15 wt % of γ-methacryloxypropyl trimethoxy silane, 10 wt % of trimethoxysilyl propionic acid and 10 wt % of pure water were added and stirred at 80 degrees for 3 hours, and then cooled. Thereafter, the product was diluted with propylene glycol monomethyl ether acetate so that the solid content was 40 wt %. Therefore, an alkali-soluble photocurable silicone resin (A1) having a weight average molecular weight of about 6250 Da was synthesized.
[0041] Synthesis Example 2:
[0042] 30 wt % of cyclohexyl trimethoxy silane and 10 wt % of pure water were loaded into a reactor equipped with a reflux condenser. 20 wt % of propylene glycol monomethyl ether acetate was added thereto, followed by 0.1 wt % of phosphoric acid catalyst in the presence of the total weight of the mixture, the mixture was refluxed and stirred for 4 hours, then 15 wt % of γ-methacryloxypropyl trimethoxy silane, 15 wt % of trimethoxysilyl propionic acid and 10 wt % of pure water were added and stirred at 80 degrees for 3.5 hours, and then cooled. Thereafter, the product was diluted with propylene glycol monomethyl ether acetate so that the solid content was 40 wt %. Therefore, an alkali-soluble photocurable silicone resin (A2) having a weight average molecular weight of about 6860 Da was synthesized.
[0043] Synthesis Example 3:
[0044] 30 wt % of cyclohexyl trimethoxy silane and 10 wt % of pure water were loaded into a reactor equipped with a reflux condenser. 20 wt % of propylene glycol monomethyl ether acetate was added thereto, followed by 0.1 wt % of phosphoric acid catalyst in the presence of the total weight of the mixture, the mixture was refluxed and stirred for 2 hours, then 15 wt % of γ-methacryloxypropyl trimethoxy silane, 15 wt % of trimethoxysilyl propionic acid and 10 wt % of pure water mixture were added and stirred at 80 degrees for 2.5 hours, and then cooled. Thereafter, the product was diluted with propylene glycol monomethyl ether acetate so that the solid content was 40 wt %. Therefore, an alkali-soluble light-curable silicone resin (A3) having a weight average molecular weight of about 4600 Da was synthesized.
[0045] In the preparation process of the alkali-soluble photocurable silicone resin of the present invention, γ-methacryloxypropyltrimethoxysilane and trimethoxysilyl propionic acid are added later, which can effectively make the carboxyl group and the acrylate double bond as much as possible on the surface of the bulk resin, thereby improving the reactivity of the double bond and the alkaline water solubility of the carboxyl group. When the weight average molecular weight of the obtained silicone resin under the above reaction temperature and time conditions is controlled in the range of 5000~8000Da, the strength and heat resistance of the resin photocured film have relatively excellent performance in this range.
[0046] 2. Preparation of the negative photoresist composition of the present invention
[0047] The alkali-soluble photocurable organic silicone resin prepared in the above synthesis example was used to prepare a photoresist composition, and compared with the comparative example. The following is the content of each component of the photoresist composition of the present invention.
[0048] Table 1: Types and solid contents of various components in the embodiments of the present invention
[0049]
[0050] Embodiment 1:
[0051] 15 g of the alkali-soluble photocurable silicone resin (A1) of Synthesis Example 1, 3 g of pentaerythritol triacrylate modified by succinic anhydride (B), 1 g of IRGACURE369 (D) and 0.02 g of surfactant (E) were uniformly mixed. In this case, the corresponding contents are those calculated based on the solid content excluding the solvent. The mixture was dissolved in propylene glycol methyl ether acetate so that the solid content of the mixture was 20% by weight. The solution was stirred for 2 hours and filtered through a membrane filter with a pore size of 0.2 μm to obtain a composition solution having a solid content of 20% by weight.
[0052] Compared with the synthetic preparation method of Example 1, Examples 2 and 3 are different in the types and / or contents of the response components, as shown in Table 2 below.
[0053] Table 2: Content of each component in each embodiment and comparative example
[0054] Recipe No. Alkali soluble resin type code Alkali soluble resin (A), g Alkali soluble acrylic monomer (B), g Photoinitiator (D), g Surfactant (E), g Example 1 A1 15 3 1 0.02 Example 2 A2 15 3 1 0.02 Example 3 A3 15 3 1 0.02 Comparative Example A4 15 3 1 0.02
[0055] 3. Result Testing and Evaluation
[0056] (1) Negative photoresist test environment of each embodiment: The copolymer compositions prepared in the examples and comparative examples were each applied to a glass substrate by spin coating. The coated substrate was then pre-baked on a hot plate maintained at 110° C. for 90 seconds to form a dried film. The dried film was developed for 60 seconds at 23° C. with a developer (which was a 0.05 wt % aqueous solution of potassium hydroxide). Then, using an aligner (model name: MA6) that emits light with a wavelength of 200 nm to 450 nm, it was exposed to light at an exposure rate of 200 mJ / cm2 for a certain period of time, based on a wavelength of 365 nm. Thereafter, the exposed film thus obtained was heated in a convection oven at 230° C. for 30 minutes to prepare a cured film with a thickness of 2 μm.
[0057] (2) Heat resistance weight loss rate %
[0058] The above process was performed without using a mask to form a cured film on a glass substrate. The thickness H1 of the obtained cured film was measured. The cured film was then additionally baked in an oven at 250°C for 3 hours. The thickness H2 of the cured film was then measured. The thickness change rate (%) was calculated as the heat resistance weight loss rate (%) using the following calculation.
[0059] Heat resistance weight loss rate % = (H1-H2) / H1*100% When this value is 3% or less, it is judged that the heat resistance is excellent.
[0060] (3) Heat resistance and light transmittance%
[0061] The above process was used to form a cured film on a glass substrate without using a mask. The transmittance T1 of the obtained cured film was measured using a spectrophotometer at a wavelength in the range of 400-800nm. The cured film was then baked in an oven at 250°C for 3 hours, and the transmittance T2 of the cured film was measured. The transmittance change rate (%) was calculated as the heat-resistant transmittance (%) using the following calculation.
[0062] Heat-resistant light transmittance % = (T1-T2) / T1*100% When this value is 5% or less, it is judged to be excellent in heat resistance.
[0063] Table 3: Comparison of the resistance performance of each embodiment and the comparative example
[0064] Recipe No. Heat resistance weight loss rate% Heat resistance and light transmittance% Heat resistance (grade determination) Example 1 0.97 4.26 Excellent Example 2 1.52 3.64 Excellent Example 3 3.93 5.35 generally Comparative Example 5.68 7.98 generally
[0065] As shown in Table 3 above, the compositions of the examples within the scope of the present invention are generally excellent in heat resistance. In contrast, the compositions of the comparative examples not within the scope of the present invention show that at least one of these properties is unfavorable.
[0066] It can be seen from the above embodiments and test results that, relative to the prior art, the negative photoresist composition provided by the present invention has significant improvements in heat resistance and resistance to poor light transmittance caused by high temperature yellowing. The present invention adopts cyclohexyltrimethoxysilane, and forms a three-dimensional copolymer structure through copolymerization and cross-linking with a trifunctional silane monomer containing a double bond and a trifunctional silane monomer containing a carboxyl group. Compared with the linear silane copolymer, it has higher thermal stability while reducing the content of phenyl and cyclic groups, which can effectively improve the anti-yellowing performance of the photoresist. At the same time, the present invention can greatly improve its heat resistance by replacing conventional phenylsilane monomers with cyclohexyltrimethoxysilane.
Claims
1. A highly heat-resistant copolymer negative photoresist composition, characterized in that The composition includes the following components in parts by weight: 10~30 parts of alkali soluble light curing silicone resin 1.5~8 parts of alkali soluble acrylic monomer Photoinitiator 0.5~2.5 parts Surfactant 0.01~0.02 parts and 12 to 60 parts of solvent; The alkali-soluble photocurable silicone resin is a three-dimensional copolymer obtained by copolymerizing and crosslinking cyclohexyltrimethoxysilane, a trifunctional silane monomer containing a double bond and a trifunctional silane monomer containing a carboxyl group, and the weight average molecular weight of the alkali-soluble photocurable silicone resin is 5000-8000Da.
2. The high heat-resistant copolymer negative photoresist composition according to claim 1, characterized in that: The trifunctional silane monomer containing a double bond is γ-methacryloxypropyltrimethoxysilane, acryloxypropyltrimethoxysilane or γ-methacryloxypropylmethyldimethoxysilane.
3. The high heat-resistant copolymer negative photoresist composition according to claim 1, characterized in that: The carboxyl-containing trifunctional silane monomer is trimethoxysilyl propionic acid, triethoxysilyl propionic acid, trimethoxysilyl butyric acid or triethoxysilyl butyric acid.
4. The high heat-resistant copolymer negative photoresist composition according to claim 1, characterized in that: The weight ratio of the cyclohexyltrimethoxysilane to the trifunctional silane monomer containing a double bond and the trifunctional silane monomer containing a carboxyl group is (30-40): (12-17): (12-17).
5. The high heat-resistant copolymer negative photoresist composition according to claim 1, characterized in that: The alkali-soluble acrylic ester monomer is pentaerythritol tri(meth)acrylate modified by succinic anhydride.
6. The high heat-resistant copolymer negative photoresist composition according to claim 1, characterized in that: The solvent is diethylene glycol dimethyl ether, diethylene glycol ethyl methyl ether, dipropylene glycol dimethyl ether, dipropylene glycol diethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol methyl ether acetate, and 2-methoxypropionic acid methyl ester.
7. The high heat-resistant copolymer negative photoresist composition according to claim 1, characterized in that: The surfactant is a fluorine-based surfactant, a silicon-based surfactant or a nonionic surfactant.
8. A method for preparing the highly heat-resistant copolymer negative photoresist composition according to any one of claims 1 to 7, characterized in that The following steps are involved: Step S1, preparation of alkali-soluble photocurable silicone resin: cyclohexyltrimethoxysilane, pure water and solvent are added to a reactor in proportion, and then an appropriate amount of phosphoric acid catalyst is added to perform a reflux stirring prepolymerization reaction for 2.5 to 6 hours; Step S2, continue to add the trifunctional silane monomer containing a double bond and the trifunctional silane monomer containing a carboxyl group, and add an appropriate amount of pure water, and distill and stir to react at 75-85° C. for 2-4 hours; Step S3, after cooling the obtained product, diluting it with a solvent to obtain an alkali-soluble light-curable silicone resin having a solid content of 20-50% and a weight average molecular weight of 5000-8000Da; Step S4, uniformly mixing the alkali-soluble photocurable silicone resin, the alkali-soluble acrylate monomer, the photoinitiator and the surfactant, dissolving them in a solvent, and filtering to obtain a composition solution with a solid content of 16-25%.