Antioxidant and preparation method thereof
By introducing polyether segments into hindered or semi-hindered phenols, the problem of easy migration of antioxidants in polyethers is solved, better antioxidant effects and efficient production are achieved, the reaction process is simplified and safety is improved.
Patent Information
- Application Number
- CN202011049671.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-09-29
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2040-09-29
AI Technical Summary
Existing hindered phenol antioxidants are prone to migration in polymers with high polarity such as polyethers, resulting in reduced antioxidant effects, and cumbersome synthesis process and poor economic benefits.
By introducing polyether segments in the para-position of hindered or semi-hindered phenols, reacting with a catalyst to increase the compatibility between antioxidants and polyethers, thereby improving the antioxidant effect, a simple one-step reaction method is adopted Synthesis of hindered phenol or semi-hindered phenol antioxidants suitable for polyethers.
It achieves better antioxidant effects in polyether, simplifies the reaction process, improves production efficiency, is safe and reliable, avoids separation steps, and is directly miscible in polyether.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to a hindered phenol or semi-hindered phenol antioxidant, which can be applied to polymers with relatively high polarity such as polyether, and belongs to the technical field of chemical production. Background Art
[0002] Hindered phenol antioxidants are a type of antioxidant that is currently widely used. They can be used alone or in combination with other types of antioxidants to achieve a synergistic antioxidant effect. They are a type of phenolic compound with a sterically hindered structure that can react with other free radicals to form a quinone resonance structure, stabilize the free radical system, and thus achieve an antioxidant effect. This type of antioxidant can also be used in combination with other types of antioxidants to achieve a synergistic antioxidant effect.
[0003] At present, hindered phenol antioxidants have been widely used in the application and processing of polymers. The more commonly used grades are 1010, 1076, 1330, etc. Their structures are shown below:
[0004]
[0005] However, the hindered phenol antioxidants currently used generally have low polarity and are prone to migration when used in polymers with high polarity (such as polyethers), thereby reducing the antioxidant effect.
[0006] In addition, the synthesis of modified hindered phenol antioxidants is relatively cumbersome, resulting in a decrease in economic benefits. Summary of the invention
[0007] In view of the advantages of hindered phenol or semi-hindered phenol antioxidants and the problems they currently face, one of the technical problems to be solved by the present invention is to provide a hindered phenol or semi-hindered phenol antioxidant that is more suitable for polyether.
[0008] The second technical problem to be solved by the present invention is to provide a method for synthesizing the above-mentioned hindered phenol or semi-hindered phenol antioxidant, so as to synthesize the hindered phenol or semi-hindered phenol antioxidant which is more suitable for polyether.
[0009] Under the action of a catalyst, by introducing a polyether segment at the para position of the hindered phenol or semi-hindered phenol, the compatibility between the antioxidant and the polyether can be increased, thereby achieving a good antioxidant effect.
[0010] One of ordinary skill in the art will understand "about" and will vary to some extent in the context in which the term is used. If the use of a term is unclear to one of ordinary skill in the art, given the context in which it is used, "about" will mean up to plus or minus 20% of the particular term.
[0011] The term "mainly consisting of..." as used herein refers to the main component constituting the mixture. If not otherwise specified, a main component is generally considered to be a component with a weight percentage of more than 50%. The main component may be a pure substance or a mixture of components with similar structures or chemical properties that can be classified into the same category as known to those skilled in the art.
[0012] Any temperature range, pH range, weight (mass) range, molecular weight range, percentage range, etc. herein, whether or not expressed using the term "range" or "various ranges", includes the specified endpoints and each point between the two endpoints.
[0013] In one aspect, the present invention relates to a hindered phenol or semi-hindered phenol antioxidant suitable for use in polyethers.
[0014] In one or more specific embodiments, the antioxidant suitable for polyether is a polymer of formula I.
[0015] In one or more specific embodiments, n is a positive integer.
[0016] In one or more specific embodiments, R0 is H or methyl or ethyl or isopropyl or tert-butyl.
[0017] In one or more specific embodiments, R1 is H or methyl.
[0018] In one or more specific embodiments, R2 is H or methyl.
[0019] In one or more specific embodiments, R3 is H or methyl.
[0020] In one or more specific embodiments, the molecular weight of the molecule of Formula I is preferably in the range of 300 to 10,000.
[0021] In one aspect, the present invention relates to an antioxidant suitable for use in polyethers consisting essentially of one or more of the polymers of formula I.
[0022] In one or more specific embodiments, the antioxidant suitable for polyether is mainly composed of one or more of the polymers of formula I, wherein n is a positive integer; R0 is H or methyl or ethyl or isopropyl or tert-butyl; R1 is H or methyl; R2 is H or methyl; R3 is H or methyl; the molecular weight range of the molecule of formula I is preferably 300 to 10,000.
[0023] In one aspect, the present invention relates to an antioxidant suitable for use in polyethers comprising one or more of the polymers of formula I.
[0024] In one or more specific embodiments, the antioxidant suitable for polyether comprises one or more of the polymers of formula I, wherein n is a positive integer; R0 is H or methyl or ethyl or isopropyl or tert-butyl; R1 is H or methyl; R2 is H or methyl; R3 is H or methyl; the molecular weight range of the molecule of formula I is preferably 300 to 10,000.
[0025] In another aspect, the present invention relates to a method for synthesizing the antioxidant of formula I.
[0026] In one or more specific embodiments, n is a positive integer; R0 is H or methyl or ethyl or isopropyl or tert-butyl; R1 is H or methyl; R2 is H or methyl; R3 is H or methyl.
[0027] In one or more specific embodiments, hindered phenol and / or semi-hindered phenol is mixed with polyether, base and catalyst and heated to react under inert atmosphere.
[0028] In one or more specific embodiments, the hindered phenol is at least one of the phenol derivatives having a steric hindering group on each side of the ortho position of the phenolic hydroxyl group. Specifically, the steric hindering group is a tert-butyl group; the hindered phenol can be specifically 2,6-di-tert-butylphenol.
[0029] In one or more specific embodiments, the semi-hindered phenol is at least one of the phenol derivatives having a sterically hindered group at the ortho position of the phenolic hydroxyl group. Specifically, the sterically hindered group is a tert-butyl group; the semi-hindered phenol can be selected from at least one of 2-tert-butylphenol, 2-methyl-6-tert-butylphenol, 2-ethyl-6-tert-butylphenol and 2-isopropyl-6-tert-butylphenol.
[0030] In one or more specific embodiments, the catalyst can be selected from (1,5-cyclooctadiene)iridium (I) chloride dimer, dichloro (pentamethylcyclopentadienyl)iridium (III) dimer, AgNO3, AgBr, triphenylphosphine, etc., or a mixture thereof.
[0031] In one or more specific embodiments, the base can be selected from one of inorganic or organic alkaline substances such as NaOH, Na2CO3, KOH, K2CO3, CH3OK, or a mixture thereof.
[0032] In one or more specific embodiments, the polyether is selected from polyethylene glycol, polypropylene glycol, polyethylene glycol monomethyl ether, polypropylene glycol monomethyl ether, ethylene glycol propylene glycol copolymer, etc., with a molecular weight ranging from 200 to 10,000, or a mixture thereof.
[0033] In one or more specific embodiments, the inert atmosphere can be nitrogen, a rare gas (such as argon, neon) or other gases that do not participate in the reaction, or a mixture thereof.
[0034] In one or more specific embodiments, the reaction temperature is 50-150° C. and the pressure is normal pressure.
[0035] In one or more specific embodiments, if the sum of the molar equivalents of hindered phenol and semi-hindered phenol is 1, preferably: the molar equivalent of the catalyst is 0.05-10%, the molar equivalent of the base is 0.5-10, and the molar equivalent of the polyether is 5 or more.
[0036] Preferably, if the molar equivalent of 2,6-di-tert-butylphenol is 1, the molar equivalent of the catalyst is 0.05-10%, the molar equivalent of the base is 0.5-10, and the molar equivalent of the polyether is 5 or more.
[0037] In one or more specific embodiments, the reaction time is 4-72 hours.
[0038] In one or more specific embodiments, if the sum of the molar equivalents of hindered phenol and semi-hindered phenol is 1, more preferably: the molar equivalent of the catalyst is 0.5-5%, the molar equivalent of the base is 1-5, and the molar equivalent of the polyether is 50 or more.
[0039] More preferably, if the molar equivalent of 2,6-di-tert-butylphenol is 1, the molar equivalent of the catalyst is 0.5-5%, the molar equivalent of the base is 1-5, and the molar equivalent of the polyether is 50 or more.
[0040] In one or more specific embodiments, the more preferred reaction temperature is 70-120° C.; the more preferred reaction time is 8-36 hours.
[0041] Specifically, under nitrogen protection, 2,6-di-tert-butylphenol is mixed with a catalyst, a base and a polyether are added, the temperature is raised to react, and the product is obtained by filtering after cooling, that is, a hindered phenol structure modified with a polyether at the para position.
[0042] In this reaction, the catalyst can be selected from one or more of [Ir(cod)Cl]2 (chemical name: (1,5-cyclooctadiene) iridium (I) chloride dimer), [CP*IrCl2]2 (chemical name: dichloro(pentamethylcyclopentadienyl) iridium (III) dimer), AgNO3, AgBr, PPh3 (chemical name: triphenylphosphine), the base can be selected from one or more of NaOH, Na2CO3, KOH, K2CO3, CH3OK, and the polyether can be selected from polyethylene glycol, polypropylene glycol, polyethylene glycol monomethyl ether, polypropylene glycol monomethyl ether, ethylene glycol propylene glycol copolymer, etc., with a molecular weight of 200 to 10,000. If the ratio of the reactants is 1 molar equivalent of 2,6-di-tert-butylphenol, the catalyst is 0.05-10 (%) equivalents, preferably 0.5-5 (%) equivalents, the ratio of the base is 0.5-10 equivalents, preferably 1-5 equivalents, and the polyether is 5 times or more equivalents, preferably 50 times or more equivalents; the reaction temperature is generally 50-150°C, preferably 70-120°C, and the reaction time is generally 4-72h, preferably 8-36h.
[0043] The general structure of the obtained product is shown in Formula I:
[0044]
[0045]
[0046] Depending on the added reactants, the hindered phenol antioxidant of formula I can be specifically represented by molecules of structures of formula I-1, formula I-2, formula I-3 and formula I-4, etc. If the added reactants are a mixture of polyethers, the obtained product is also a corresponding mixture.
[0047] Compared with the prior art, the present invention has the following beneficial effects:
[0048] 1. The hindered phenol antioxidant of formula I has better antioxidant effect when used in polyether.
[0049] 2. The reaction process is simple. Compared with the traditional method of synthesizing hindered phenol antioxidants, this method can directly react with polyether for grafting, and the reaction can be completed in only one step.
[0050] 3. High production efficiency. The antioxidant after reaction is directly mixed and dissolved in the polyether. It does not need to be separated and then added. It can be used directly, which improves the production efficiency.
[0051] 4. The safety factor is high. The raw materials of the entire reaction are simple and easy to obtain, without volatile and toxic components, and the safety of the production process can be guaranteed. DETAILED DESCRIPTION
[0052] The present invention is further described below in conjunction with specific embodiments and drawings.
[0053] Embodiment 1:
[0054] At room temperature, 1.24 g of 2,6-di-tert-butylphenol, 0.24 g of [CP*IrCl2]2, and 1.3 g of potassium hydroxide were added to a 50 ml three-necked flask, and then 25 g of polyethylene glycol (molecular weight 400) was added. After purging with nitrogen for 3 times, nitrogen protection was used, and the temperature was gradually increased to 105°C and maintained for 24 hours. After the reaction was completed, the temperature was lowered to room temperature, and the product was separated after filtration to obtain 2,6-di-tert-butyl-4-polyethylene glycol phenol with a yield of 86%.
[0055] Embodiment 2:
[0056] Dissolve 0.12g of [CP*IrCl2]2 in 25g of polyethylene glycol (molecular weight 400), take 1g of the solution and add it together with 24g of polyethylene glycol into a 50ml flask, then add 1.24g of 2,6-di-tert-butylphenol and 1.3g of potassium hydroxide into the flask, purge it with nitrogen three times and then use nitrogen protection, keep the temperature at 85℃ and react for 72h. After the reaction is completed, lower the temperature to room temperature, and separate 2,6-di-tert-butyl-4-polyethylene glycol phenol, with a yield of 21%.
[0057] Embodiment 3:
[0058] At room temperature, add 1.24g of 2,6-di-tert-butylphenol, 0.48g of [CP*IrCl2]2, and 1.6g of potassium methoxide into a 50ml flask, then add 25g of polyethylene glycol (molecular weight 2000), purge with nitrogen for 3 times, and then use nitrogen protection, gradually increase the temperature to 95°C to melt the polyethylene glycol, and continue to maintain the temperature at 115°C for 24h. After the reaction is completed, cool to room temperature, and separate to obtain 2,6-di-tert-butyl-4-polyethylene glycol phenol, with a yield of 88%.
[0059] Embodiment 4:
[0060] 1.24 g of 2,6-di-tert-butylphenol, 0.24 g of [CP*IrCl2]2, and 3.6 g of potassium carbonate were added into a 50 ml flask, and then 25 g of polyethylene glycol monomethyl ether (molecular weight 400) was added, and nitrogen was purged 3 times and then protected with nitrogen, and then the temperature was maintained at 105°C for 24 hours. After the reaction was completed, the temperature was lowered to room temperature, and the product was separated to obtain 2,6-di-tert-butyl-4-polyethylene glycol phenol, with a yield of 62%.
[0061] Embodiment 5:
[0062] 2.48g of 2,6-di-tert-butylphenol, 0.48g of [CP*IrCl2]2, and 2.0g of sodium hydroxide were added into a 50ml flask, and then 10g of polypropylene glycol (molecular weight 400) was added. After purging with nitrogen for 3 times, nitrogen protection was used, and the temperature was maintained at 105°C for 48h. After the reaction was completed, the temperature was lowered to room temperature, and 2,6-di-tert-butyl-4-polypropylene glycol phenol was separated, with a yield of 37%.
[0063] Embodiment 6:
[0064] We added 1.24g of 2,6-di-tert-butylphenol, 0.48g of [CP*IrCl2]2, and 2.6g of potassium hydroxide into a 100ml flask, and then added 50g of polypropylene glycol (molecular weight 2000), purged with nitrogen three times, and then protected with nitrogen, and kept the temperature at 105℃ for 24h. After the reaction was completed, the temperature was lowered to room temperature, and 2,6-di-tert-butyl-4-polypropylene glycol phenol was separated, with a yield of 91%.
[0065] Embodiment 7:
[0066] 1.24 g of 2,6-di-tert-butylphenol, 0.24 g of [Ir(cod)Cl]2, 0.3 g of PPh3, and 2.0 g of sodium hydroxide were added to a flask, and then 25 g of polypropylene glycol monomethyl ether (molecular weight 400) was added. After purging with nitrogen for 3 times, nitrogen protection was used, and the temperature was maintained at 120°C for 24 hours. After the reaction was completed, the temperature was lowered to room temperature, and 2,6-di-tert-butyl-4-polypropylene glycol phenol was separated, with a yield of 67%.
[0067] Embodiment 8:
[0068] Dissolve 0.24g of [Ir(cod)Cl]2 in 25g of polypropylene glycol monomethyl ether (molecular weight 400), mix well, take 1g of the mixed solution and add it to a 50ml flask together with 24g of polypropylene glycol monomethyl ether, then add 1.24g of 2,6-di-tert-butylphenol, 0.03g of PPh3, and 0.65g of potassium hydroxide into the flask, purge with nitrogen three times and then use nitrogen protection, keep the temperature at 120℃ and react for 72h. After the reaction is completed, the temperature is lowered to room temperature, and 2,6-di-tert-butyl-4-polypropylene glycol phenol can be separated, with a yield of 26%.
[0069] Embodiment 9:
[0070] 1.24 g of 2,6-di-tert-butylphenol, 0.48 g of [Ir(cod)Cl]2, 0.6 g of PPh3, and 3.2 g of potassium methoxide were added to a flask, and then 25 g of polypropylene glycol (molecular weight 2000) was added, and nitrogen was purged 3 times and then protected with nitrogen, and the temperature was maintained at 120°C for 24 hours. 2,6-di-tert-butyl-4-polypropylene glycol phenol was obtained with a yield of 44%.
[0071] Embodiment 10:
[0072] 1.08 g of 2-methyl-6-tert-butylphenol, 0.36 g of [Ir(cod)Cl]2, 0.5 g of PPh3, and 3.6 g of potassium methoxide were added into a flask, and then 25 g of polypropylene glycol (molecular weight 8000) was added and heated to 95°C, purged with argon for 3 times, and then protected with argon, and the temperature was maintained at 150°C for 48 hours. 2-methyl-6-tert-butyl-4-polypropylene glycol phenol was obtained with a yield of 22%.
[0073] Comparative Example:
[0074] 1000ppm of 1010, 1076, 2,6-di-tert-butyl-4-polyethylene glycol phenol (named as antioxidant 1) polyether and blank sample were tested according to VDA277 standard to observe the TVOC content of the samples after oxidation. The results are shown in Table 1.
[0075] Table 1 Comparison of TVOC content of antioxidant tests of various antioxidants
[0076] sample blank 1076 1010 Antioxidant 1 TVOC(ug / g) 632 442 502 382
[0077] It can be seen from the above that the modified hindered phenol antioxidant has better antioxidant properties.
[0078] The above specific embodiments are merely examples for clearly illustrating the invention, and are not intended to be specific limitations of the invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description, and the conventional alternative solutions applied to other similar requirements are obviously equivalent technical solutions claimed in the claims of the present invention.
Claims
1. A method for preparing an antioxidant of formula I, characterized in that: wherein n is a positive integer; R0 is tert-butyl; R1 is H or methyl; R2 is H or methyl; R3 is H; The reaction conditions are selected from one of a), b), and c): a) the hindered phenol is 2,6-di-tert-butylphenol, the catalyst is dichloro(pentamethylcyclopentadienyl)iridium(III) dimer, the base is potassium hydroxide, the polyether is polyethylene glycol with a molecular weight of 400, and the masses of the hindered phenol, the catalyst, the base, and the polyether are 1.24 g, 0.24 g, 1.3 g, and 25 g, respectively; under an inert atmosphere, the hindered phenol, the polyether, the base, and the catalyst are mixed and heated to react, and after mixing, the temperature is gradually increased to 105° C. and the reaction is maintained for 24 hours to obtain 2,6-di-tert-butyl-4-polyethylene glycol phenol; b) the hindered phenol is 2,6-di-tert-butylphenol, the catalyst is dichloro(pentamethylcyclopentadienyl)iridium(III) dimer, the base is potassium methoxide, the polyether is polyethylene glycol with a molecular weight of 2000, and the masses of the hindered phenol, the catalyst, the base, and the polyether are 1.24 g, 0.48 g, 1.6 g, and 25 g, respectively; under an inert atmosphere, the hindered phenol is mixed with the polyether, the base, and the catalyst and heated to react, and after mixing, the temperature is gradually increased to 115° C. and the reaction is maintained for 24 hours to obtain 2,6-di-tert-butyl-4-polyethylene glycol phenol; c) the hindered phenol is 2,6-di-tert-butylphenol, the catalyst is dichloro(pentamethylcyclopentadienyl)iridium(III) dimer, the base is potassium hydroxide, the polyether is polypropylene glycol with a molecular weight of 2000, and the masses of the hindered phenol, the catalyst, the base, and the polyether are 1.24 g, 0.48 g, 2.6 g, and 50 g, respectively; under an inert atmosphere, the hindered phenol is mixed with the polyether, the base, and the catalyst and heated to react, and after mixing, the temperature is gradually increased to 105° C. and the reaction is maintained for 24 hours to obtain 2,6-di-tert-butyl-4-polypropylene glycol phenol.