Silicon wafer texturing method, silicon wafer and solar cell
By employing a three-step texturing method, the problems of uneven texture and reflectivity fluctuations in crystalline Si solar cells were solved, resulting in higher cell conversion efficiency and improved short-circuit current and conversion efficiency.
Patent Information
- Application Number
- CN202111470210.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-03
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-12-03
Smart Images

Figure CN114335204B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of solar cells, and in particular relates to a silicon wafer texturing method, a silicon wafer and a solar cell. Background Art
[0002] With the depletion of fossil energy and the increasingly serious environmental pollution problems, solar energy has received widespread attention as a clean, sustainable and efficient energy source. Solar cells are devices that convert solar energy into electrical energy. Improving the photoelectric conversion efficiency of solar cells and reducing their power generation costs are research hotspots in the global photovoltaic field. Since crystalline Si has the advantages of long body minority carrier lifetime, low photo-induced attenuation, and good weak light response, it is very suitable for making low-cost and high-efficiency solar cells. Solar cells have become one of the development directions of high-efficiency crystalline silicon solar cells in the future. The preparation of solar cells generally starts with the texturing process. At present, the texturing process of single-crystal silicon solar cells mainly uses pre-cleaning + alkali texturing to complete the preparation of pyramid-shaped velvet. This texturing method is difficult to have both good uniformity and a large aspect ratio of the pyramid morphology and low reflectivity, and the reflectivity and pyramid velvet size after texturing will fluctuate with the extension of the life of the texturing tank solution. The above texturing methods seriously hinder the further improvement of battery conversion efficiency. Summary of the invention
[0003] The present invention aims to solve one of the technical problems in the related art to at least a certain extent. To this end, the purpose of the present invention is to propose a method for texturing a silicon wafer, a silicon wafer and a solar cell. The silicon wafer prepared by the present invention has good velvet uniformity, significantly reduces the reflectivity of the silicon wafer, and has a pyramid morphology with a large aspect ratio, which satisfies the good ohmic contact in the sintering process of the screen printing slurry. At the same time, it has a smaller velvet size fluctuation range and reflectivity fluctuation range during the entire texturing liquid cycle, which significantly improves the short-circuit current of the battery prepared during the entire texturing liquid cycle, thereby improving the conversion efficiency of the battery. The battery conversion efficiency is finally improved by 0.05-0.1%.
[0004] In one aspect of the present invention, the present invention provides a method for texturing a silicon wafer. According to an embodiment of the present invention, the method comprises:
[0005] (1) Placing the silicon wafer in a polishing liquid for pre-polishing to obtain a flat silicon wafer surface;
[0006] (2) placing the silicon wafer obtained in step (1) in a first texturing liquid to perform a first texturing;
[0007] (3) Placing the silicon wafer obtained in step (2) in a second texturing solution for a second texturing.
[0008] According to the method for texturing a silicon wafer in an embodiment of the present invention, first, the silicon wafer is pre-polished to effectively remove the small black cores (i.e., small pyramids) on the polished surface so as to obtain a flat silicon wafer surface, which provides a good foundation for growing a pyramid velvet surface with good uniformity; then, the silicon wafer is texturized for the first time to grow an overall pyramid velvet surface; finally, the silicon wafer is texturized for the second time to modify the small pyramid velvet surfaces, and the overall height of the pyramids is significantly improved. At the same time, the problem of excessive fluctuations in the velvet size and reflectivity of the silicon wafer in the middle and late stages of the life of the single texturing tank solution is improved, and the fluctuation range of the pyramid velvet size and reflectivity of the silicon wafer prepared within the entire texturing tank solution cycle is significantly reduced. As a result, the prepared silicon wafer has good velvet uniformity, significantly reduces the reflectivity of the silicon wafer, and has a pyramid morphology with a large aspect ratio, which satisfies the good ohmic contact in the sintering process of the screen printing slurry. At the same time, the entire velvet solution cycle has a smaller velvet size fluctuation range and reflectivity fluctuation range, which significantly improves the short-circuit current of the battery prepared in the entire velvet solution cycle, thereby improving the conversion efficiency of the battery. The battery conversion efficiency is ultimately improved by 0.05-0.1%.
[0009] In addition, the texturing method for a silicon wafer according to the above embodiment of the present invention may also have the following additional technical features:
[0010] In some embodiments of the present invention, in step (1), the polishing liquid includes 3-4 wt % of a first base, 1-1.5 wt % of a first additive solution, and the balance is water.
[0011] In some embodiments of the present invention, the first base is selected from at least one of NaOH and KOH.
[0012] In some embodiments of the present invention, the first additive solution includes 0.9-1.1 wt % of perchlorate, 0.4-0.6 wt % of methyl cellulose and the balance of water.
[0013] In some embodiments of the present invention, the perchlorate is selected from at least one of sodium perchlorate and potassium perchlorate.
[0014] In some embodiments of the present invention, in step (1), after the pre-polishing treatment, the weight loss of the silicon wafer is 0.073-0.091 g / dm 2 .
[0015] In some embodiments of the present invention, in step (1), the time of the pre-polishing treatment is 120-150 seconds, and the temperature of the pre-polishing treatment is 70-75°C.
[0016] In some embodiments of the present invention, in step (2), the first texturing solution includes 1.1-1.3 wt % of a second alkali, 0.7-1.0 wt % of a second additive solution and the balance of water.
[0017] In some embodiments of the present invention, the second base is selected from at least one of NaOH and KOH.
[0018] In some embodiments of the present invention, the second additive solution includes 0.4-0.6 wt % of 2-phenylimidazoline, 0.4-0.6 wt % of 2-methyl-3-butyn-2-ol, 0.9-1.1 wt % of tannic acid and the balance of water.
[0019] In some embodiments of the present invention, in step (2), the time of the first texturing is 300-360s, and the temperature of the first texturing is 80-85°C.
[0020] In some embodiments of the present invention, in step (3), the second texturing solution includes 0.5-0.7 wt % of a third alkali, 0.2-0.4 wt % of a third additive solution and the balance of water.
[0021] In some embodiments of the present invention, the third base is selected from at least one of NaOH and KOH.
[0022] In some embodiments of the present invention, the third additive solution includes 0.4-0.6 wt % of 2-phenylimidazoline, 0.4-0.6 wt % of 2-methyl-3-butyn-2-ol, 0.9-1.1 wt % of tannic acid and the balance of water.
[0023] In some embodiments of the present invention, in step (3), the time of the second texturing is 100-150s, and the temperature of the second texturing is 80-85°C.
[0024] In some embodiments of the present invention, the weight loss of the silicon wafer during the second texturing is 1 / 5-1 / 3 of the weight loss during the first texturing.
[0025] In some embodiments of the present invention, the weight loss of the silicon wafer in the first texturing process is 0.091-0.14 g / dm 2 .
[0026] In some embodiments of the present invention, the weight loss of the silicon wafer during the second texturing is 0.018-0.036 g / dm 2 .
[0027] In another aspect of the present invention, the present invention provides a silicon wafer. According to an embodiment of the present invention, the silicon wafer is prepared by the method described in the above embodiment. As a result, the silicon wafer has good velvet uniformity, significantly reduces the reflectivity of the silicon wafer, and has a pyramid morphology with a large aspect ratio, which satisfies the good ohmic contact during the sintering process of the screen printing slurry, and has a smaller velvet size fluctuation range and reflectivity fluctuation range during the entire velvet liquid cycle.
[0028] In the third aspect of the present invention, the present invention provides a solar cell. According to an embodiment of the present invention, the solar cell has a silicon wafer prepared by the method described in the above embodiment or the silicon wafer described in the above embodiment. As a result, the short-circuit current of the solar cell is improved, so that the conversion efficiency of the cell is improved by 0.05-0.1%.
[0029] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0031] Figure 1 The present invention is a flowchart of a method for texturing a silicon wafer according to an embodiment of the present invention. DETAILED DESCRIPTION
[0032] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, and should not be construed as limiting the present invention.
[0033] In one aspect of the present invention, a method for texturing a silicon wafer is provided. Figure 1 , the method comprising:
[0034] S100: Place the silicon wafer in the polishing liquid for pre-polishing
[0035] In this step, the silicon wafer is placed in the polishing liquid and pre-polished to effectively remove the small black cores (i.e., small pyramids) on the polishing surface, so as to obtain a flat silicon wafer surface, which provides a good foundation for growing a pyramid velvet surface with good uniformity. Specifically, when the silicon wafer is in the polishing liquid, the 100 and 111 crystal planes of the silicon wafer do not have anisotropic corrosion, and isotropic corrosion obtains a flat silicon wafer surface. Among them, the first alkali plays a role in corroding the silicon wafer, and the first additive solution plays a role in reducing the difference in the rate of the 100 and 111 crystal planes and improving the degassing effect.
[0036] According to a specific embodiment of the present invention, the polishing liquid includes 3-4wt% of the first alkali, 1-1.5wt% of the first additive solution and the balance of water, thereby limiting the content of each component of the polishing liquid within the above range, further making the reaction speed controllable, thereby obtaining a flat silicon wafer surface. The inventors found that if the content of the first additive solution is too low, small black cores (small pyramids) will still exist after polishing, and the polishing effect will be poor. If the content of the first additive solution is too high, the polishing reaction rate will be slowed down, and too much additive will remain on the surface of the polished silicon wafer, affecting the cleaning effect; if the content of the first alkali is too low, it will cause anisotropic corrosion of the 100 and 111 surfaces, weakening the polishing effect. If the content of the first alkali is too high, the reaction will be too violent and out of control, and the cost of chemicals will increase.
[0037] According to another specific embodiment of the present invention, the first additive solution includes 0.9-1.1wt% perchlorate, 0.4-0.6wt% methyl cellulose and the balance of water. The role of the perchlorate is to bring the reaction rates of the silicon wafer 111 and 100 crystal planes closer, and the role of the methyl cellulose is to improve the degassing effect. Therefore, the content of the first additive solution is limited to the above range, and the first additive solution further has a better polishing effect. The inventors found that if the content of perchlorate is too low, the polishing effect will be poor, and if its content is too high, it will make it more difficult to clean the polished silicon wafer; if the content of methyl cellulose is too low, the degassing effect will be poor, and there will be a bubble print on the surface of the silicon wafer after polishing. If its content is too high, the polishing rate will be slowed down and the cleaning of the polished silicon wafer will be more difficult.
[0038] In an embodiment of the present invention, the specific type of the first base is not particularly limited, and those skilled in the art can select it at will according to actual needs. As a specific example, the first base is selected from at least one of NaOH and KOH.
[0039] In the embodiments of the present invention, the specific type of the perchlorate is not particularly limited, and those skilled in the art can select it at will according to actual needs. As a specific example, the perchlorate is selected from at least one of sodium perchlorate and potassium perchlorate.
[0040] According to another specific embodiment of the present invention, the time of the pre-polishing treatment is 120-150s, and the temperature of the pre-polishing treatment is 70-75°C. Thus, the time and temperature of the pre-polishing treatment are limited within the above range, and the reaction speed is further controllable, thereby obtaining a flat silicon wafer surface.
[0041] According to another specific embodiment of the present invention, after the pre-polishing process, the weight loss of the silicon wafer is 0.073-0.091 g / dm 2 Thus, a better polishing effect can be further obtained, and at the same time, the weight reduction of the silicon wafer will not be too great.
[0042] S200: First Velvet
[0043] In this step, the silicon wafer obtained in step S100 is placed in the first texturing liquid, and the first texturing is performed to grow an overall pyramid velvet surface. Specifically, the size of the pyramid velvet surface after the first texturing will vary, with the largest being about 1.5 μm and the smallest being about 1 μm. The principle of the first texturing reaction is that alkali corrodes the silicon surface, with a fast corrosion rate on the 100 crystal plane and a slow corrosion rate on the 111 crystal plane, eventually forming a pyramid tetrahedron structure. During the reaction process, the texturing additive (i.e., the second additive solution) provides nucleation points, increases the rate difference between the 111 and 100 crystal planes, and at the same time has a cleaning effect on the surface of the silicon wafer, and can also adjust the surface tension of the first texturing liquid to improve the degassing effect during the reaction of the silicon wafer.
[0044] According to another specific embodiment of the present invention, the first texturing liquid includes 1.1-1.3wt% of the second alkali, 0.7-1.0wt% of the second additive solution and the balance of water, thereby limiting the content of each component of the first texturing liquid to the above range, further making the reaction rate of the first texturing controllable, the appearance after texturing is uniform, the velvet size and reflectivity meet the requirements, and the process time can meet the mass production requirements.
[0045] According to another specific embodiment of the present invention, the second additive solution includes 0.4-0.6wt% of 2-phenylimidazoline, 0.4-0.6wt% of 2-methyl-3-butyn-2-ol, 0.9-1.1wt% of tannic acid and the remainder of water, thereby limiting the content of each component of the second additive solution within the above range, and the second additive solution can achieve better effects of removing lint, degassing and cleaning the surface of silicon wafers.
[0046] In an embodiment of the present invention, the specific type of the second base is not particularly limited, and those skilled in the art can select it at will according to actual needs. As a specific example, the second base is selected from at least one of NaOH and KOH.
[0047] According to another specific embodiment of the present invention, the time of the first texturing is 300-360s, and the temperature of the first texturing is 80-85°C. Thus, the reaction rate of the first texturing is further controllable, thereby obtaining a more uniform velvet pyramid size, and the process time also meets mass production requirements.
[0048] According to another specific embodiment of the present invention, the weight loss of the silicon wafer in the first texturing is 0.091-0.14 g / dm 2 , thereby, further satisfying the completion of the growth of the overall pyramid, and finally completing the relatively uniform pyramid size and lower reflectivity after the second texturing.
[0049] S300: Secondary Texturing
[0050] In this step, the silicon wafer obtained in step S200 is placed in the second texturing solution for a second texturing, and the small pyramid velvet surface is modified, and the overall height of the pyramid is significantly improved. At the same time, the problem of excessive fluctuations in the velvet surface size and reflectivity of the silicon wafer in the middle and late stages of the life of the single texturing tank solution is improved, so that the fluctuation range of the pyramid velvet surface size and reflectivity of the silicon wafer prepared within the entire texturing tank solution cycle is significantly reduced. Specifically, during the second texturing, the alkali (i.e., the third alkali) is still used to anisotropically corrode the crystal planes 100 and 111 of the silicon wafer, and the large pyramid and the small pyramid are still growing, but the growth rate of the small pyramid is faster than that of the large pyramid. Because the size of the small pyramid has increased, the overall height of the pyramid is significantly improved.
[0051] According to another specific embodiment of the present invention, the second texturing liquid includes 0.5-0.7wt% of the third alkali, 0.2-0.4wt% of the third additive solution and the balance of water. Thus, the second texturing liquid within this range can make the small pyramids react quickly and the large pyramids react slowly, ultimately forming a relatively uniform pyramid size with a lower reflectivity.
[0052] According to another specific embodiment of the present invention, the third additive solution includes 0.4-0.6wt% of 2-phenylimidazoline, 0.4-0.6wt% of 2-methyl-3-butyn-2-ol, 0.9-1.1wt% of tannic acid and the remainder of water. Thus, the third additive solution can achieve better effects of removing lint, degassing and cleaning the surface of silicon wafers.
[0053] According to another specific embodiment of the present invention, the time of the second texturing is 100-150s, and the temperature of the second texturing is 80-85°C. Thus, the texturing conditions further make the reaction rate of the second texturing controllable, thereby obtaining a more uniform velvet pyramid size, and the process time also meets the mass production requirements.
[0054] In an embodiment of the present invention, the specific type of the third base is not particularly limited, and those skilled in the art can select it at will according to actual needs. As a specific example, the third base is selected from at least one of NaOH and KOH.
[0055] According to another specific embodiment of the present invention, the weight reduction of the silicon wafer in the second texturing is 1 / 5-1 / 3 of the weight reduction in the first texturing, thereby further satisfying the modification effect of the small pyramids, and finally obtaining a more uniform pyramid size, while at the same time preventing the weight reduction from being too great and causing the thickness of the silicon wafer to become thinner.
[0056] According to another specific embodiment of the present invention, the weight loss of the silicon wafer in the second texturing is 0.018-0.036 g / dm 2 , thereby, the modification effect on the small pyramids can be further satisfied, and finally a more uniform pyramid size can be obtained, while at the same time the weight reduction will not be too large, resulting in a thinning of the silicon wafer.
[0057] According to the method for texturing a silicon wafer in an embodiment of the present invention, first, the silicon wafer is pre-polished to effectively remove the small black cores (i.e., small pyramids) on the polished surface so as to obtain a flat silicon wafer surface, which provides a good foundation for growing a pyramid velvet surface with good uniformity; then, the silicon wafer is texturized for the first time to grow an overall pyramid velvet surface; finally, the silicon wafer is texturized for the second time to modify the small pyramid velvet surfaces, and the overall height of the pyramids is significantly improved. At the same time, the problem of excessive fluctuations in the velvet size and reflectivity of the silicon wafer in the middle and late stages of the life of the single texturing tank solution is improved, and the fluctuation range of the pyramid velvet size and reflectivity of the silicon wafer prepared within the entire texturing tank solution cycle is significantly reduced. As a result, the prepared silicon wafer has good velvet uniformity, significantly reduces the reflectivity of the silicon wafer, and has a pyramid morphology with a large aspect ratio, which satisfies the good ohmic contact in the sintering process of the screen printing slurry. At the same time, the entire velvet solution cycle has a smaller velvet size fluctuation range and reflectivity fluctuation range, which significantly improves the short-circuit current of the battery prepared in the entire velvet solution cycle, thereby improving the conversion efficiency of the battery. The battery conversion efficiency is ultimately improved by 0.05-0.1%.
[0058] Furthermore, the method also includes the steps of cleaning, slow pulling and drying, and the process is: pre-polishing, pre-cleaning, first water washing, first texturing, second texturing, second water washing, post-cleaning, third water washing, pickling, fourth water washing, slow pulling and drying. Among them, the specific process of pre-cleaning, first water washing, second water washing, post-cleaning, third water washing, pickling, fourth water washing, slow pulling and drying belongs to the prior art in this field and will not be repeated here.
[0059] In another aspect of the present invention, the present invention provides a silicon wafer. According to an embodiment of the present invention, the silicon wafer is prepared by the method described in the above embodiment. As a result, the silicon wafer has good velvet uniformity, significantly reduces the reflectivity of the silicon wafer, and has a pyramid morphology with a large aspect ratio, which satisfies the good ohmic contact during the sintering process of the screen printing slurry, and has a smaller velvet size fluctuation range and reflectivity fluctuation range during the entire velvet liquid cycle.
[0060] In the third aspect of the present invention, the present invention provides a solar cell. According to an embodiment of the present invention, the solar cell has a silicon wafer prepared by the method described in the above embodiment or the silicon wafer described in the above embodiment. As a result, the short-circuit current of the solar cell is improved, so that the conversion efficiency of the cell is improved by 0.05-0.1%.
[0061] The embodiments of the present invention are described in detail below. It should be noted that the embodiments described below are exemplary and are only used to explain the present invention, and cannot be interpreted as limiting the present invention. In addition, if not explicitly stated, all reagents used in the following embodiments are commercially available, or can be synthesized according to this article or known methods, and the reaction conditions not listed are also easily available to those skilled in the art.
[0062] Example 1
[0063] This embodiment provides a solar cell, and the preparation method thereof is as follows:
[0064] Texturing: The silicon wafer first enters the polishing tank, which uses 3wt% NaOH and 1wt% polishing additive solution (the components of the alkaline polishing additive are 1wt% sodium perchlorate, 0.5wt% methyl cellulose, and the rest is water in terms of mass percentage), polishing time 120s, polishing temperature 75°C, and controlled polishing weight loss 0.2g (M6 silicon wafer); after polishing, the silicon wafer enters the pre-cleaning tank, which uses an aqueous solution of 1.6wt% H2O2 and 0.45wt% NaOH for pre-cleaning, with a cleaning time of 180s and a cleaning temperature of 65°C; after pre-cleaning, the silicon wafer enters the water Washing 1, washing time 180s, washing temperature room temperature; after washing, the silicon wafer enters texturing 1, texturing 1 uses 1.12wt% NaOH and 0.7wt% texturing additive solution (texturing additive solution includes 0.5wt% 2-phenylimidazoline, 0.5wt% 2-methyl-3-butyn-2-ol, 1.0wt% tannic acid and the remainder of water), texturing time 300s, texturing temperature 82°C, and the texturing weight loss is controlled to be 0.3g (M6 silicon wafer); after texturing 1, the silicon wafer enters texturing 2, texturing 2 uses 0.56wt% NaOH and 0.28wt% texturing additive solution (texturing additives include 0.5wt% 2-phenylimidazoline, 0.5wt% 2-methyl-3-butyn-2-ol, 1.0wt% tannic acid and the remainder of water), texturing time 110 seconds, texturing temperature 82°C, texturing weight loss controlled 0.05g (M6 silicon wafer); after texturing 2, the silicon wafer enters water washing 2, the water washing time is 180s, and the water washing temperature is room temperature; after water washing, the silicon wafer enters post-cleaning, and the post-cleaning adopts an aqueous solution of 1.6wt% H2O2 and 0.45wt% NaOH to clean The time is 180s, and the cleaning temperature is 70℃; after the silicon wafer is cleaned, it enters water washing 3, the water washing time is 180s, and the water washing temperature is room temperature; after the silicon wafer is washed, it enters acid washing, and the acid washing adopts a mixed aqueous solution of 3wt% HF and 3wt% HCL, the acid washing time is 180s, and the acid washing temperature is room temperature; after the silicon wafer is acid washed, it enters water washing 4, the water washing time is 180s, and the water washing temperature is room temperature; after the silicon wafer is washed, it enters hot water slow pulling, and uses 80℃ hot water to pull away the residual water and impurities on the surface of the silicon wafer; after the silicon wafer is slowly pulled with hot water, it enters the drying tank, and the drying time is 600s, and the drying temperature is 80℃. So far, the entire silicon wafer texturing and cleaning process is completed.
[0065] Then, diffusion, junction, passivation, coating and screen printing are carried out according to the PERC process to form a solar cell.
[0066] The reflectivity of the silicon wafer obtained after the texturing step to light was tested, and the test results are shown in Table 1. The short-circuit current and conversion efficiency of the cell were tested, and the test results are shown in Table 1.
[0067] Example 2
[0068] In this embodiment, the polishing tank uses 4wt% NaOH and 1.5wt% polishing additive solution (the components of the alkaline polishing additive solution are 1.1wt% sodium perchlorate, 0.6wt% methyl cellulose, and the rest is water in terms of mass percentage), the polishing time is 130s, and the polishing temperature is 75°C; the texturing 1 uses 1.1wt% NaOH and 0.8wt% texturing additive solution (the texturing additive solution includes 0.5wt% 2-phenylimidazoline, 0.5wt% 2-methyl-3 -butyne-2-ol, 1.0wt% tannic acid and the remainder water), texturing time 330s, texturing temperature 80°C; Texturing 2 uses 0.5wt% NaOH and 0.2wt% texturing additive solution (the texturing additive solution includes 0.5wt% 2-phenylimidazoline, 0.5wt% 2-methyl-3-butyne-2-ol, 1.0wt% tannic acid and the remainder water), texturing time 150 seconds, texturing temperature 80°C; other contents are the same as Example 1.
[0069] The reflectivity of the silicon wafer obtained after the texturing step to light was tested, and the test results are shown in Table 1. The short-circuit current and conversion efficiency of the cell were tested, and the test results are shown in Table 1.
[0070] Example 3
[0071] In this embodiment, the polishing tank uses 3.5wt% NaOH and 1.25wt% polishing additive solution (the components of the alkaline polishing additive solution are 0.9wt% sodium perchlorate, 0.4wt% methyl cellulose, and the rest is water by mass percentage), the polishing time is 150s, and the polishing temperature is 70°C; the texturing 1 uses 1.3wt% NaOH and 1.0wt% texturing additive solution (the texturing additive solution includes 0.5wt% 2-phenylimidazoline, 0.5wt% 2-methyl- 3-butyne-2-ol, 1.0wt% tannic acid and the remainder water), texturing time 360s, texturing temperature 85°C; Texturing 2 uses 0.7wt% NaOH and 0.4wt% texturing additive solution (the texturing additive solution includes 0.5wt% 2-phenylimidazoline, 0.5wt% 2-methyl-3-butyne-2-ol, 1.0wt% tannic acid and the remainder water), texturing time 100 seconds, texturing temperature 85°C; other contents are the same as Example 1.
[0072] The reflectivity of the silicon wafer obtained after the texturing step to light was tested, and the test results are shown in Table 1. The short-circuit current and conversion efficiency of the cell were tested, and the test results are shown in Table 1.
[0073] Comparative Example 1
[0074] This comparative example adopts pre-cleaning + one-step alkali texturing to complete the preparation of pyramid-shaped velvet, the pre-cleaning adopts an aqueous solution of 1.6wt% H2O2 and 0.45wt% NaOH, the cleaning time is 180s, and the cleaning temperature is 65°C; the one-step alkali texturing adopts 1.12wt% NaOH and 0.7wt% texturing additive solution (the texturing additive solution includes 0.5wt% 2-phenylimidazoline, 0.5wt% 2-methyl-3-butyn-2-ol, 1.0wt% tannic acid and the balance water), the texturing time is 420s, and the texturing temperature is 82°C. Other contents are the same as Example 1.
[0075] The reflectivity of the silicon wafer obtained after the texturing step to light was tested, and the test results are shown in Table 1. The short-circuit current and conversion efficiency of the cell were tested, and the test results are shown in Table 1.
[0076] Table 1
[0077] Reflectivity of light / % Short circuit current / A Conversion efficiency / % Example 1 8.65 13.6593 23.30 Example 2 8.71 13.6455 23.28 Example 3 8.75 13.6355 23.26 Comparative Example 1 9.26 13.5980 23.21
[0078] It can be seen from Table 1 that, compared with Comparative Example 1, the light reflectivity of Examples 1-3 is reduced, and the short-circuit current and conversion efficiency are improved.
[0079] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0080] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A method for texturing a silicon wafer, characterized in that: include: (1) placing a silicon wafer in a polishing solution for pre-polishing treatment to obtain a flat silicon wafer surface; wherein the polishing solution comprises 3-4 wt % of a first alkali, 1-1.5 wt % of a first additive solution, and the balance is water, wherein the first additive solution comprises 0.9-1.1 wt % of perchlorate, 0.4-0.6 wt % of methyl cellulose, and the balance is water; (2) placing the silicon wafer obtained in step (1) in a first texturing solution for a first texturing; wherein the first texturing solution comprises 1.1-1.3 wt % of a second base, 0.7-1.0 wt % of a second additive solution and the balance is water, and the second additive solution comprises 0.4-0.6 wt % of 2-phenylimidazoline, 0.4-0.6 wt % of 2-methyl-3-butyn-2-ol, 0.9-1.1 wt % of tannic acid and the balance is water; (3) Placing the silicon wafer obtained in step (2) in a second texturing solution for a second texturing; wherein the second texturing solution comprises 0.5-0.7wt% of a third alkali, 0.2-0.4wt% of a third additive solution and the balance is water, and the third additive solution comprises 0.4-0.6wt% of 2-phenylimidazoline, 0.4-0.6wt% of 2-methyl-3-butyn-2-ol, 0.9-1.1wt% of tannic acid and the balance is water.
2. The texturing method according to claim 1, characterized in that: In step (1), the first base is selected from at least one of NaOH and KOH.
3. The texturing method according to claim 2, characterized in that: The perchlorate is selected from at least one of sodium perchlorate and potassium perchlorate.
4. The texturing method according to claim 1, characterized in that: In step (1), after the pre-polishing treatment, the weight loss of the silicon wafer is 0.073-0.091 g / dm 2 .
5. The texturing method according to claim 1, characterized in that: In step (1), the pre-polishing treatment time is 120-150 seconds, and the pre-polishing treatment temperature is 70-75°C.
6. The texturing method according to any one of claims 1 to 5, characterized in that: In step (2), the second base is selected from at least one of NaOH and KOH; In step (2), the time of the first texturing is 300-360 seconds, and the temperature of the first texturing is 80-85°C.
7. The texturing method according to any one of claims 1 to 5, characterized in that: In step (3), the third base is selected from at least one of NaOH and KOH; In step (3), the time of the second texturing is 100-150 seconds, and the temperature of the second texturing is 80-85°C.
8. The texturing method according to any one of claims 1 to 5, characterized in that: The weight loss of the silicon wafer in the second texturing process is 1 / 5-1 / 3 of the weight loss in the first texturing process; The weight loss of the silicon wafer in the first texturing process is 0.091-0.14 g / dm 2 ; The weight loss of the silicon wafer during the second texturing process is 0.018-0.036 g / dm 2 .
9. A silicon wafer, characterized in that: The silicon wafer is prepared by the method according to any one of claims 1 to 8.