A simple synthesis method to control the morphology and structure of Co3O4 nanosheets
By using alanine and cobalt nitrate hexahydrate to synthesize Co3O4 nanosheets in a hydrothermal method and adjusting the reaction conditions, the problems of complex preparation methods, high costs and irregular products in the existing technology have been solved, achieving low-cost, controllable Preparation of nano-Co3O4 nanosheets, the product has a regular hexagonal sheet structure and high catalytic activity.
Patent Information
- Application Number
- CN202011091200.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-10-13
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-10-13
AI Technical Summary
The existing preparation methods of Co3O4 nanosheets are complex, high-cost, and cause serious environmental pollution, and the products are mostly irregular sheet structures. The content and size distribution of the hexagonal sheets are uneven, making it difficult to achieve simple, easy, low-cost, and controllable preparation. .
Alanine and cobalt nitrate hexahydrate are used as raw materials, and NaOH is used as a pH regulator. Co3O4 nanosheets are synthesized through a hydrothermal method. The reaction conditions such as material ratio, pH value and temperature are adjusted to control the morphology and structure of the nanosheets, including Hexagonal slices, irregular slices, flower-like structures, etc.
The low-cost, simple and controllable preparation of nano-Co3O4 structure and morphology has been achieved. The product has a regular hexagonal sheet structure, uniform size distribution and high dispersion, exposing higher index crystal planes and enhancing catalytic active sites.
Smart Images

Figure CN114349065B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a simple synthesis method capable of controlling the morphology and structure of Co3O4 nanosheets, belonging to the technical field of inorganic material synthesis. Background Art
[0002] Co3O4 is a traditional functional material, widely used as a catalyst, sensor, magnetic recording material, etc. Different morphologies and different crystal face exposures have a great influence on the physical and chemical properties of Co3O4 particles, so the growth behavior of Co3O4 particles in different environments has attracted widespread attention. Co3O4 single crystal nanoparticles have the conventional properties of nanomaterials, such as small size effect, surface effect, dielectric confinement effect, etc.; in addition, through certain synthesis methods, Co3O4 can selectively expose some crystal faces with higher indexes. These Co3O4 single crystal nanoparticles with higher index crystal faces usually have unexpected excellent properties, which has also attracted the attention of more and more researchers. The flake structure of cobalt tetroxide has attracted widespread attention from scientific researchers because it can expose specific index crystal faces and has a large surface area, which can provide more reaction sites and shorter ion diffusion channels. There are many Co3O4 flake structures reported so far, among which irregular flake structures are the most common, but Co3O4 nanohexagonal flakes with regular structure, high percentage and size of about 300nm are rarely reported.
[0003] The Co3O4 sheet structures reported in recent years mainly include: Huh et al. prepared hexagonal sheet Co(OH)2 in hydrazine aqueous solution and H2O2, and then obtained hexagonal sheet Co3O4 nanoparticles after high temperature treatment (MJ Kim, YD Huh, Materials Letters, 65 (2011) 650-652). Chen et al. used Co(NO3)2·6H2O and concentrated ammonia water as reaction raw materials, and obtained β-Co(OH)2 hexagonal blocks by oil bath reflux. The structure was aged for 15 hours to obtain a Co3O4 hexagonal micron box structure with nanotubes on the surface (R. Jing, AX Shan, RM Wang, et al., Cryst Eng Comm, 15 (2013) 3587-3592). Liu et al. used Co(CH3COO)2·4H2O and hydrazine hydrate as reaction materials, cyclohexane / water (v / v=1:1) as solvent, and obtained Co3O4 sheet structure with a large number of pores by water bath method and subsequent high temperature heat treatment (SSLu, XYJing, JYLiu, et al., Journal of Solid State Chemistry, 197 (2013) 345-351). Lin et al. also prepared Co3O4 nanosheets by CTAB-assisted hydrothermal method (CHChen, YCChen, MSLin, Biosensors and Bioelectronics, 42 (2013) 379-384). Li et al. prepared irregular Co3O4 nanosheets using cobalt acetate tetrahydrate, hexamethylenetetramine, polyoxyethylene-polyoxypropylene-polyoxyethylene as raw materials, water and ethylene glycol as solvents by solvothermal method and calcination process (Li Xiaoting, Zhang Lexi, Yin Jing, et al., Journal of Inorganic Chemistry, 32 (2016) 1739-1746). Men et al. prepared sheet-like porous hexagonal cobalt oxide using cobalt nitrate and succinic acid as raw materials by water bath method and subsequent calcination method. The hexagonal material has poor dispersibility, low regularity and low proportion of the product (Men Yongling, Zou Ruyi, Luo Guiling, et al., Journal of Hunan Normal University, 32 (2019) 6-11). Liu et al. prepared irregular porous Co3O4 nanosheets using cobalt nitrate and urea as raw materials by solvent thermal and subsequent calcination process (Liu Mi, Han Lifeng, Xiao Yuanhua, et al., Journal of Zhengzhou University, 34 (2013) 46-49). Yao et al. prepared Co3O4 nanosheets using cobalt nitrate, ascorbic acid, and inorganic base (ammonia water, sodium hydroxide) as raw materials by microwave method and subsequent calcination method (WL Hao, QN Dai, Y. Liu, Chem Electro Chem, 4 (2017) 1236-1242).Chinese patent 201210438944.8 discloses a method for preparing porous Co3O4 nanosheets using nickel foam as a substrate, nickel nitrate and DMSO as raw materials, electrochemical deposition and subsequent calcination. Chinese patent 201110075740.8 discloses a method for preparing Co3O4 nanosheets using cobalt chloride, polyvinyl pyrrolidone and urea as raw materials, hydrothermal method and subsequent calcination process. Chinese patent 201110319791.0 discloses a method for preparing Co3O4 nanosheets using cobalt salt, hexadecyltrimethylammonium bromide and urea as raw materials, hydrothermal method and heat treatment process.
[0004] The above-mentioned methods for preparing Co3O4 nanosheets have the following problems: (1) The process is complicated and the steps are cumbersome. The use of substrates, organic solvents or organic reagents makes the preparation cost high, and the use of organic reagents is very easy to pollute the environment; (2) Some synthesis processes also require electrochemical deposition or microwave-assisted methods to synthesize sheet structures; (3) Most of the Co3O4 nanosheets reported so far are irregular sheet structures. There are few reports on Co3O4 nanohexagonal sheets, and even if there are similar reports, the content of hexagonal sheets in the product is not high and the size distribution is not uniform. Therefore, it is very necessary to find a simple, low-cost, controllable, environmentally friendly method for preparing Co3O4 nanohexagonal sheets with high content, regular morphology and uniform size distribution. Summary of the invention
[0005] The purpose of the present invention is to provide a simple synthesis method capable of controlling the morphology and structure of Co3O4 nanosheets. The present invention uses alanine and cobalt nitrate hexahydrate as reaction raw materials, uses NaOH as a pH value regulator, and synthesizes Co3O4 nanosheets by a hydrothermal method. In a specific synthesis process, the synthesis of nano Co3O4 with different structures and morphologies can be controlled by changing the ratio of the amount of alanine to the amount of cobalt salt, the pH value of the hydrothermal reaction system, the reaction temperature and other experimental conditions. The raw materials used for the synthesis of the Co3O4 nanosheets are low in price, the preparation process is simple and easy, the structure and morphology of the prepared nano Co3O4 are controllable, and nano Co3O4 materials with different structures and morphologies can be selected and synthesized according to specific applications.
[0006] The technical scheme of the present invention is: a simple synthesis method capable of controlling the morphology and structure of Co3O4 nanosheets, characterized in that a Co3O4 nanosheet precursor is synthesized by a hydrothermal method using cobalt salt and alanine as raw materials and NaOH as a pH value regulator.
[0007] Furthermore, the Co3O4 nanosheet precursor can be calcined at high temperature to obtain Co3O4 nanosheets. This structure can well maintain the structure of the precursor, and at the same time, it has a large number of pore structures after high temperature treatment. Preferably, the Co3O4 nanosheet precursor is treated at 400-500°C for 1.5-3 hours in a high-temperature tube furnace in an air environment, and naturally cooled to room temperature after the reaction is completed to obtain the Co3O4 nanosheet.
[0008] Preferably, the preparation method is: using cobalt nitrate hexahydrate as a cobalt source, alanine as a ligand, NaOH as a pH regulator, and deionized water as a solvent, and synthesizing a Co3O4 nanosheet precursor by a hydrothermal method.
[0009] Specifically, the method comprises the following steps: using cobalt nitrate hexahydrate as a cobalt source, alanine as a ligand, and deionized water as a solvent, and performing ultrasonic stirring to form a dark red transparent solution; then adding 1 mol / L NaOH aqueous solution to adjust the pH value of the system to 6.7-10.9; after stirring evenly, transferring the solution into a self-pressurized hydrothermal reactor, sealing the solution, and performing hydrothermal reaction in a high-temperature oven at 140±20°C for 0.5-12 hours; and allowing the solution to cool naturally to room temperature, collecting the product, washing it, and drying it to obtain a Co3O4 nanosheet precursor for later use.
[0010] Furthermore, by adjusting the synthesis conditions (ligand and cobalt source Co 2+ The molar ratio of the substance, the pH value of the hydrothermal reaction system, and the reaction temperature) are used to adjust the microscopic morphology and structure of the product, wherein the synthesis conditions used for each structure are as follows:
[0011] Nanohexagonal sheet structure: ligand and Co 2+ The molar ratio is 0.5, the hydrothermal reaction temperature is 140°C, and the pH value of the hydrothermal reaction system is 8.8. The prepared nanohexagonal sheets are about tens of nanometers wide and about 300 nanometers long, with uniform size distribution and good dispersibility.
[0012] Irregular nanosheet structure: ligand and Co 2+ The molar ratio is 0.2, the hydrothermal reaction temperature is 140°C, and the pH value of the hydrothermal reaction system is 8.8;
[0013] Flower-like structure of the ligand and Co 2+ The molar ratio is 2.5, the hydrothermal reaction temperature is 140°C, and the pH value of the hydrothermal reaction system is 8.8;
[0014] Short columnar structures formed by stacking nanosheets: ligands and Co 2+ The molar ratio is 0.5, the hydrothermal reaction temperature is 130°C, and the pH value of the hydrothermal reaction system is 8.8;
[0015] Nanopolyhedral structure: ligand and Co 2+The molar ratio is 0.5, the hydrothermal reaction temperature is 140°C, and the pH value of the hydrothermal reaction system is 6.7;
[0016] Elliptical nanosheet structure: ligand and Co 2+ The molar ratio is 0.5, the hydrothermal reaction temperature is 140°C, and the pH value of the hydrothermal reaction system is 9.8.
[0017] Wherein, in the above steps, the molar ratio of the deionized water to the cobalt source is 300-500:1.
[0018] The technical effects of the present invention are:
[0019] 1. The present invention uses alanine, a chiral molecule with special recognition function, as a ligand to accurately control the microscopic morphology and structure of the product. Alanine has a small structure and strong coordination ability. By appropriately changing its addition amount in the reaction system, the microscopic morphology and structure of the target product can be effectively controlled.
[0020] 2. Compared with the reported technologies, the present invention has the advantages of low raw material price, simple, rapid and environmentally friendly synthesis process, and the ability to adjust the product microscopic morphology and structure by adjusting the synthesis conditions (the molar ratio of the ligand to the cobalt source, the pH value of the reaction system, the reaction temperature, etc.) (nanohexagonal sheets, irregular nanothin sheets, flower-like structures of connected sheets, short columnar structures formed by stacking nanosheets, nanopolyhedrons and elliptical nanothick sheets, etc. can be prepared according to the changes in specific experimental conditions). Nano-Co3O4 materials with different morphologies and structures can be selectively synthesized in a controllable manner according to actual needs.
[0021] 3. The Co3O4 nanohexagonal flakes prepared by the present invention are regular hexagonal flakes with uniform size distribution (about tens of nanometers in width and about 300 nanometers in length), good dispersibility, pore structure, high percentage of product content, and can expose specific higher index crystal faces, thereby making it have more effective catalytic active sites. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is a scanning electron microscope (SEM) photo of the nanohexagonal sheet precursor;
[0023] Figure 2 This is a scanning electron microscope (SEM) photo of Co3O4 nanohexagonal flakes;
[0024] Figure 3 This is a scanning electron microscope (SEM) photo of irregular nanosheets;
[0025] Figure 4 This is a scanning electron microscope (SEM) photograph of a continuous flower-like structure;
[0026] Figure 5 This is a scanning electron microscope (SEM) photograph of a short columnar structure formed by stacking nanosheets;
[0027] Figure 6 This is a scanning electron microscope (SEM) photograph of a nanopolyhedron;
[0028] Figure 7 This is a scanning electron microscope (SEM) image of an elliptical nanosheet. DETAILED DESCRIPTION
[0029] The following are examples provided by the present invention, which are only intended to further illustrate the application of the present invention, but not to limit it. In the following examples, the volume of the deionized water is 12 mL, and the amount of the cobalt source added is 0.0017 mol.
[0030] Example 1
[0031] 1) Using cobalt nitrate hexahydrate as the cobalt source, alanine as the ligand, and deionized water as the solvent, a ligand and Co 2+ The solution with a molar ratio of 0.5 was stirred ultrasonically for 20 min at room temperature to form a dark red transparent solution;
[0032] 2) preparing a 1 mol / L NaOH aqueous solution, adding it dropwise into the solution prepared in step 1), stirring thoroughly, to obtain a solution with a pH value of 8.8;
[0033] 3) transferring the mixed system obtained in step 2) into a self-pressurized hydrothermal reactor, sealing it, and placing it in a high-temperature oven at 140° C. for reaction for 12 hours;
[0034] 4) After the reaction is completed, the product is collected by centrifugation, washed three times with deionized water and anhydrous ethanol respectively, and then dried in air at 80°C for 6 hours;
[0035] 5) Take the dried sample to characterize the phase and morphology. The results of scanning electron microscopy showed that the obtained product had a regular hexagonal sheet structure. The nano hexagonal sheet structure was uniform, with a narrow size distribution and good dispersibility. The structure was about tens of nanometers wide and about 300 nm long (see Figure 1 ).
[0036] 6) The nano hexagonal sheet precursor obtained in step 4) is placed in a high temperature tube furnace and calcined at 450°C for 2 hours at a heating rate of 5°C / min to obtain a nano Co3O4 structure. The structure has a similar morphology and structure to the precursor. In addition, the product after high temperature treatment also has a large number of pore structures (see Figure 2). The nano hexagonal sheet is about tens of nanometers wide and about 300nm long. In addition to having a certain thickness and rich pore structure, the Co3O4 nano hexagonal sheet has the biggest feature of exposing specific high-index crystal faces under the limited adsorption of alanine, which can make it have more effective catalytic active sites.
[0037] Example 2
[0038] 1) Using cobalt nitrate hexahydrate as the cobalt source, alanine as the ligand, and deionized water as the solvent, a ligand and Co 2+ The solution with a molar ratio of 0.2 was stirred ultrasonically for 20 min at room temperature to form a dark red transparent solution;
[0039] 2) preparing a 1 mol / L NaOH aqueous solution, adding it dropwise into the solution prepared in step 1), stirring thoroughly, to obtain a solution with a pH value of 8.8;
[0040] 3) transferring the mixed system obtained in step 2) into a self-pressurized hydrothermal reactor, sealing it, and placing it in a high-temperature oven at 140° C. for reaction for 12 hours;
[0041] 4) After the reaction is completed, the product is collected by centrifugation, washed three times with deionized water and anhydrous ethanol respectively, and then dried in air at 80°C for 6 hours;
[0042] 5) Take the dried sample to characterize its phase and morphology. The results of scanning electron microscopy showed that the obtained product was irregular nanosheets (see Figure 3 ).
[0043] Example 3
[0044] 1) Using cobalt nitrate hexahydrate as the cobalt source, alanine as the ligand, and deionized water as the solvent, a ligand and Co 2+ The solution with a molar ratio of 2.5 was stirred ultrasonically for 20 min at room temperature to form a dark red transparent solution;
[0045] 2) preparing a 1 mol / L NaOH aqueous solution, adding it dropwise into the solution prepared in step 1), stirring thoroughly, to obtain a solution with a pH value of 8.8;
[0046] 3) transferring the mixed system obtained in step 2) into a self-pressurized hydrothermal reactor, sealing it, and placing it in a high-temperature oven at 140° C. for reaction for 12 hours;
[0047] 4) After the reaction is completed, the product is collected by centrifugation, washed three times with deionized water and anhydrous ethanol respectively, and then dried in air at 80°C for 6 hours;
[0048] 5) Take the dried sample for phase and morphology characterization. The results of scanning electron microscopy showed that the obtained product was a continuous flower-like structure, the surface of which contained a rich film structure (see Figure 4 ). The flower-like structure has a large specific surface area and can be used in supercapacitors, active catalysts, electrochemical sensors and other fields.
[0049] Example 4
[0050] 1) Using cobalt nitrate hexahydrate as the cobalt source, alanine as the ligand, and deionized water as the solvent, a ligand and Co 2+ The solution with a molar ratio of 0.5 was stirred ultrasonically for 20 min at room temperature to form a dark red transparent solution;
[0051] 2) preparing a 1 mol / L NaOH aqueous solution, adding it dropwise into the solution prepared in step 1), stirring thoroughly, to obtain a solution with a pH value of 8.8;
[0052] 3) transferring the mixed system obtained in step 2) into a self-pressurized hydrothermal reactor, sealing it, and placing it in a high-temperature oven at 130° C. for reaction for 12 hours;
[0053] 4) After the reaction is completed, the product is collected by centrifugation, washed three times with deionized water and anhydrous ethanol respectively, and then dried in air at 80°C for 6 hours;
[0054] 5) Take the dried sample for phase and morphology characterization. Scanning electron microscopy test results show that the obtained product is a short columnar structure formed by stacking three or three nanosheets together (see Figure 5 ).
[0055] Example 5
[0056] 1) Using cobalt nitrate hexahydrate as the cobalt source, alanine as the ligand, and deionized water as the solvent, a ligand and Co 2+ The solution with a molar ratio of 0.5 was stirred ultrasonically for 20 min at room temperature to form a dark red transparent solution;
[0057] 2) preparing a 1 mol / L NaOH aqueous solution, adding it dropwise into the solution prepared in step 1), stirring thoroughly, to obtain a solution with a pH value of 6.7;
[0058] 3) transferring the mixed system obtained in step 2) into a self-pressurized hydrothermal reactor, sealing it, and placing it in a high-temperature oven at 140° C. for reaction for 12 hours;
[0059] 4) After the reaction is completed, the product is collected by centrifugation, washed three times with deionized water and anhydrous ethanol respectively, and then dried in air at 80°C for 6 hours;
[0060] 5) Take the dried sample to characterize its phase and morphology. The results of scanning electron microscopy showed that the main structure of the obtained product was a nano-polyhedral structure (see Figure 6 ).
[0061] Example 6
[0062] 1) Using cobalt nitrate hexahydrate as the cobalt source, alanine as the ligand, and deionized water as the solvent, a ligand and Co 2+ The molar ratio of the solution was 0.5, and a dark red transparent solution was formed by ultrasonic stirring for 20 min at room temperature;
[0063] 2) preparing a 1 mol / L NaOH aqueous solution, adding it dropwise into the solution prepared in step 1), stirring thoroughly, to obtain a solution with a pH value of 9.8;
[0064] 3) transferring the mixed system obtained in step 2) into a self-pressurized hydrothermal reactor, sealing it, and placing it in a high-temperature oven at 140° C. for reaction for 12 hours;
[0065] 4) After the reaction is completed, the product is collected by centrifugation, washed three times with deionized water and anhydrous ethanol respectively, and then dried in air at 80°C for 6 hours;
[0066] 5) Take the dried sample to characterize its phase and morphology. The results of scanning electron microscopy showed that the main structure of the obtained product was elliptical nano-thick sheets (see Figure 7 ).
[0067] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should be included in the scope of the claims of the present invention.
Claims
1. A simple synthesis method for controlling the morphology and structure of Co3O4 nanosheets, characterized in that: Using cobalt nitrate hexahydrate as a cobalt source, alanine as a ligand, and deionized water as a solvent, ultrasonic stirring is performed to form a dark red transparent solution, and then a 1 mol / L NaOH aqueous solution is added to adjust the pH value of the system, and after stirring evenly, the solution is transferred into a self-pressurized hydrothermal reactor, sealed, and subjected to a hydrothermal reaction in a high-temperature oven for 0.5-12 hours; the solution is cooled naturally to room temperature, the product is collected, washed, and dried to obtain a Co3O4 nanosheet precursor, and then calcined at high temperature to obtain a Co3O4 nanosheet; By adjusting the ligand and cobalt source Co 2+ The molar ratio of the substance, the pH value of the hydrothermal reaction system and the reaction temperature are used to adjust the microscopic morphology and structure of the product, as follows: Nanohexagonal sheet structure: ligand and Co 2+ The molar ratio is 0.5, the hydrothermal reaction temperature is 140°C, and the pH value of the hydrothermal reaction system is 8.8; Flower-like structure of the ligand and Co 2+ The molar ratio is 2.5, the hydrothermal reaction temperature is 140°C, and the pH value of the hydrothermal reaction system is 8.
8.
2. A simple synthesis method capable of controlling the morphology and structure of Co3O4 nanosheets as claimed in claim 1, characterized in that: The molar ratio of the deionized water to the cobalt source is 300-500:
1.
3. A simple synthesis method capable of controlling the morphology and structure of Co3O4 nanosheets as claimed in claim 1, characterized in that: The high temperature calcination is as follows: in a high temperature tube furnace in an air environment, the Co3O4 nanosheet precursor is treated at 400-500°C for 1.5-3 hours, and then naturally cooled to room temperature to obtain the Co3O4 nanosheet.
Citation Information
Patent Citations
Method for preparing Co3O4 nanometer sheet
CN102139929A
Co3O4 nano lamellar material and preparation method and application thereof
CN102412397A
Preparation method of porous Co3O4 nanosheet
CN102874882B
Method for accessorily preparing nanometer cobaltosic oxide granules at room temperature by utilizing amino acids
CN102134105A
Three-dimensional nanometer tricobalt tetraoxide, preparation method and application
CN106935869A