A novel hydrophobic anti-reflection micro-nanostructured CaF2 film and its preparation method
By using SF6 gas to incorporate Ar2 in magnetron sputtering method, adjusting process parameters to etch out the micro-nano structure, the problems of low surface roughness and high refractive index of CaF2 film are solved, the transmittance and hydrophobicity are improved, and the transmission rate and hydrophobicity are improved. The efficiency and performance of solar cells.
Patent Information
- Application Number
- CN202011089056.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-10-13
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2040-10-13
AI Technical Summary
The existing magnetron sputtering method has a small surface roughness and a high refractive index, which affects its hydrophobicity and optical properties, and limits the photoelectric conversion efficiency of solar cells.
The magnetron sputtering method is prepared by adding SF6 gas into Ar2. By adjusting the sputtering process parameters, such as gas flow ratio, working pressure and power supply power, the concave and convex micro-nano structure is etched to improve the transmittance and hydrophobicity of the film. .
The transmittance and water contact angle of the CaF2 film are significantly improved, the dependence on the incident angle is reduced, and the photoelectric conversion efficiency and hydrophobic performance of solar cells are improved.
Smart Images

Figure CN114408852B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of optical films, and in particular relates to a method for preparing a hydrophobic anti-reflection micro-nano structure film by a magnetron sputtering method using CaF2 as a target material. Background Art
[0002] Solar cells can convert inexhaustible light energy into electrical energy and are usually used as one of the components of satellites, launch vehicles and ground-based solar generators. As an important component of solar cells, coated glass is in direct contact with the external environment and plays a role in wind, rain and dust protection. Outdoor solar cells usually work in harsh environments such as high humidity. Making a hydrophobic surface can reduce the contact between water droplets or other corrosive media and the film, thereby extending the service life of solar cells. Therefore, super hydrophobicity is one of the characteristics of high-quality outdoor anti-reflection films. At the same time, coated glass can change the transmittance of the solar spectrum, thereby affecting the photoelectric conversion efficiency of solar cells. Therefore, the coated glass of photovoltaic devices should have as high a transmittance as possible to convert more incident light into photocurrent. However, due to the different refractive indices of air and glass substrates, there is a Fresnel reflection loss of incident light on the surface of the glass substrate, which reduces the photoelectric conversion efficiency of solar cells to a certain extent. For example, when quartz glass is used as a protective layer for solar cells, the average transmittance of the glass is 93.2%. If scattering and absorption are not considered, the reflection loss of incident light on the surface of the glass substrate is about 6.8%, which limits the photoelectric conversion efficiency of solar cells. According to the interference theory of light, preparing one or more layers of optical thin films on a glass substrate can reduce the reflection loss of incident light and increase the transmittance of light, thereby improving the photoelectric conversion efficiency of solar cells. Layered anti-reflection films are usually divided into single-layer, double-layer and multi-layer anti-reflection films. However, the surface roughness of layered anti-reflection films is small, and the refractive index is relatively fixed without a gradient decrease trend. Therefore, the transmittance of the film is largely limited by the incident angle. For example, when light is incident vertically on the film surface, the transmittance has a higher value, and when the incident angle decreases, the transmittance decreases significantly. Micro-nano structure anti-reflection films usually have the following characteristics: the film surface has a nano array or nano hole structure, and the surface roughness is significantly higher than that of flat anti-reflection films. When light shines on the nanostructured anti-reflection film, the incident direction gradually bends, and the refractive index of the film shows a gradient decrease trend (the lowest refractive index is close to 1). Due to the unique surface structure of the micro-nano structured anti-reflection film, the coated glass has a higher transmittance within the anti-reflection wavelength range. As the incident angle of sunlight decreases, the transmittance of the coated glass is significantly higher than that of the flat anti-reflection film glass.
[0003] Utilizing micro-nano structure anti-reflection film to improve the transmittance and water contact angle of glass has become one of the effective methods for improving outdoor solar cell performance. In recent years, the method for preparing anti-reflection film includes vacuum evaporation method, sol-gel method, magnetron sputtering method, surface microstructure method, acid etching method etc. The film prepared by magnetron sputtering method is more compact, and the bonding force between film and substrate is strong, and the operation process is simple and has good repeatability. However, the CaF2 film prepared by magnetron sputtering method is relatively flat, and the surface roughness is less, which is unfavorable for the hydrophobicity of film, and the film refractive index prepared is higher, thereby having a strong impact on the optics and hydrophobicity of CaF2 anti-reflection film.
[0004] In view of the above technical problems, the present invention proposes a method for preparing a novel hydrophobic anti-reflection micro-nanostructured CaF2 film. Summary of the invention
[0005] The purpose of the present invention is to provide a method for preparing a novel hydrophobic anti-reflective micro-nanostructure CaF2 film by magnetron sputtering using high-purity CaF2 as a target material, so that the water contact angle and transmittance of the prepared CaF2 film are significantly improved, and the dependence of the coated glass on the incident angle of sunlight is reduced. The preparation method is simple and easy to control.
[0006] A method for preparing a novel hydrophobic anti-reflection micro-nanostructured CaF2 film comprises the following steps:
[0007] (1) SF6 gas doping amount setting: high-purity Ar2 (99.999%) is used as the working gas, high-purity SF6 (99.999%) is used as the reaction gas, the total gas flow rate during sputtering is set to 60sccm-100sccm, and the SF6 / Ar2 gas flow rate ratio is set to 0.1%-20%;
[0008] (2) Sputtering working pressure setting: Set the working pressure of the vacuum chamber to 0.01Pa-4.0Pa
[0009] (3) Power supply sputtering power setting: The power supply sputtering power is set to 30W-500W;
[0010] The invention uses SF6 as a reaction gas and mixes it into the working gas Ar2. The F- ions ionized by SF6 react with the quartz glass SiO2 to etch a concave-convex micro-nano structure on the glass surface, and suppress the F deficiency of the CaF2 film. By adjusting the sputtering process parameters such as working pressure and sputtering power, the parameters of the micro-nano structure, such as the size of the pit (lower magnification, such as 2000 times), the size of the nanoparticles and the size of the nanopores (higher magnification, such as 70000 times), the porosity, etc., can be adjusted, so that the coated glass has high transmittance and high hydrophobicity.
[0011] The beneficial effects of the present invention are that SF6 is mixed into Ar2 as a reaction gas, pits are etched on a glass substrate by a magnetron sputtering method, and micro-nano structure CaF2 particles are deposited on the surface of the glass substrate. By adjusting the SF6 / Ar2 gas flow ratio during sputtering, a concave-convex micro-nano structure is etched on the glass surface, and the parameters of the micro-nano structure are further adjusted by adjusting the working pressure and the sputtering power. In addition, within the wavelength range of 300-1100nm, the average transmittance of the CaF2 coated glass reaches 95.2%, which is 2.06% higher than the transmittance of the uncoated glass (93.14%); the film water contact angle reaches 139.4°, which is close to a super-hydrophobic surface; when the CaF2 coated glass is applied to the top layer of a solar cell, the photoelectric conversion efficiency of the coated glass solar cell (28.45%) is 4.4% higher than the photoelectric conversion efficiency of the uncoated glass solar cell (27.25%), and the film is less dependent on the change of the incident angle. The CaF2 film prepared by the technical solution has a higher average transmittance (95.2%) and a higher hydrophobic angle (139.4°) for coated glass in the wavelength range of 300-1100nm, and exhibits less dependence on changes in the incident angle. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1 Figure 2 is a surface morphology of a novel hydrophobic anti-reflective micro-nanostructure CaF2 film obtained in an example of the present invention. Figure (a) is a surface morphology of the micro-nanostructure CaF2 film at a magnification of 2000, Figure (b) is a surface morphology of the micro-nanostructure CaF2 film at a magnification of 70000, and Figure (c) is an atomic force microscope (AFM) image of a 20μm*20μm micro-nanostructure CaF2 film.
[0013] Figure 2 The present invention provides an example of the 300-1100nm transmittance spectrum of the CaF2 anti-reflection film prepared under various gas flow rates.
[0014] Figure 3 The water contact angle diagram of the CaF2 film provided by the present invention is as follows. Figure 3 (a) is the water contact angle diagram of layered CaF2 film. Figure 3 (b) is the water contact angle diagram of micro-nanostructured CaF2 film.
[0015] Figure 4 The present invention provides an example of the effect of the incident angle on the short-circuit current density (J) of the micro-nanostructure CaF2 coated glass solar cell sc ) and the impact of the improvement in photoelectric conversion efficiency (PCE). DETAILED DESCRIPTION
[0016] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0017] Embodiment 1
[0018] A method for preparing a novel hydrophobic anti-reflection micro-nanostructured CaF2 film comprises the following steps:
[0019] (1) SF6 gas doping amount setting: high-purity Ar2 (99.999%) was used as the working gas, high-purity SF6 (99.999%) was used as the reaction gas, the total gas flow rate during sputtering was set to 60 sccm, and the SF6 / Ar2 gas flow rate ratio was set to 0.1%;
[0020] (2) Sputtering working pressure setting: Set the working pressure of the vacuum chamber to 0.01 Pa;
[0021] (3) Power supply sputtering power setting: The power supply sputtering power is set to 30W;
[0022] Embodiment 2
[0023] A method for preparing a novel hydrophobic anti-reflection micro-nanostructured CaF2 film comprises the following steps:
[0024] (1) SF6 gas doping amount setting: high-purity Ar2 (99.999%) was used as the working gas, high-purity SF6 (99.999%) was used as the reaction gas, the total gas flow rate during sputtering was set to 70 sccm, and the SF6 / Ar2 gas flow rate ratio was set to 2.5%;
[0025] (2) Sputtering working pressure setting: Set the working pressure of the vacuum chamber to 1.0 Pa;
[0026] (3) Power supply sputtering power setting: The power supply sputtering power is set to 100W;
[0027] Embodiment 3
[0028] A method for preparing a novel hydrophobic anti-reflection micro-nanostructured CaF2 film comprises the following steps:
[0029] (1) SF6 gas doping amount setting: high-purity Ar2 (99.999%) was used as the working gas, high-purity SF6 (99.999%) was used as the reaction gas, the total gas flow rate during sputtering was set to 80 sccm, and the SF6 / Ar2 gas flow rate ratio was set to 5.0%;
[0030] (2) Sputtering working pressure setting: Set the working pressure of the vacuum chamber to 2.0 Pa;
[0031] (3) Power supply sputtering power setting: The power supply sputtering power is set to 200W;
[0032] Embodiment 4
[0033] A method for preparing a novel hydrophobic anti-reflection micro-nanostructured CaF2 film comprises the following steps:
[0034] (1) SF6 gas doping amount setting: high-purity Ar2 (99.999%) was used as the working gas, high-purity SF6 (99.999%) was used as the reaction gas, the total gas flow rate during sputtering was set to 90 sccm, and the SF6 / Ar2 gas flow rate ratio was set to 7.5%;
[0035] (2) Sputtering working pressure setting: Set the working pressure of the vacuum chamber to 3.0 Pa;
[0036] (3) Power supply sputtering power setting: The power supply sputtering power is set to 300W;
[0037] Embodiment 5
[0038] A method for preparing a novel hydrophobic anti-reflection micro-nanostructured CaF2 film comprises the following steps:
[0039] (1) SF6 gas doping amount setting: high-purity Ar2 (99.999%) was used as the working gas, high-purity SF6 (99.999%) was used as the reaction gas, the total gas flow rate during sputtering was set to 100 sccm, and the SF6 / Ar2 gas flow rate ratio was set to 10%;
[0040] (2) Sputtering working pressure setting: Set the working pressure of the vacuum chamber to 4.0 Pa;
[0041] (3) Power supply sputtering power setting: The power supply sputtering power is set to 400W;
[0042] Figure 1 This is the surface morphology of the novel hydrophobic anti-reflective micro-nanostructure CaF2 film obtained in the example of the present invention. Figure 1 (a) is the surface morphology of the micro-nanostructured CaF2 film at 2000 times. Figure 1 (b) is the surface morphology of the micro-nanostructured CaF2 film at 70,000 times magnification. Figure 1 (c) is an AFM image of a 20μm*20μm-sized micro-nanostructured CaF2 film. From the surface morphology image at 2000 times magnification, it can be seen that the surface of the CaF2 film is composed of many pits, the pits are uneven in size and separated by wavy boundaries; Figure 1(b) It can be seen that the CaF2 film is composed of a random mixture of nanoparticles of different sizes, with some uneven nanopores distributed between the particles, with a size of about 20-200nm. This structure of different particle sizes makes the surface roughness of the film reach 140nm.
[0043] Figure 2 The transmittance spectra of the CaF2 coated glass prepared in each example within 300-1100nm are uncoated glass. As the wavelength increases, the transmittance of the coated glass of Examples 1, 4, and 5 gradually increases, and the transmittance of the coated glass of Examples 2 and 3 first increases and then decreases. Among them, the transmittance curve of the coated glass of Example 1 is lower than the transmittance curve of the uncoated glass in the wavelength range of 300-850nm, and after 850nm, the transmittance curve is basically the same as the uncoated glass curve. The transmittance curves of the coated glasses of Examples 2 and 4 have similar trends, increasing rapidly in the wavelength range of 300-550nm and slowly decreasing in the range of 550-1100nm, and the average transmittance of Example 2 is higher than that of Example 4. The transmittance of the coated glass of Example 3 has a maximum value of 96.08% at 460nm, and the average transmittance at 300-1100nm reaches 95.2%, which is 2 percentage points higher than the average transmittance of the uncoated glass (93.2%), and the anti-reflection effect is achieved in the entire wavelength range. The transmittance of the coated glass of Example 5 increases rapidly in the range of 300-900 nm and decreases slowly in the range of 900-1100 nm.
[0044] Figure 3 The water contact angle diagram of the CaF2 film provided by the present invention is as follows. Figure 3 (a) The water contact angle of the layered CaF2 film is 92°. Figure 3 (b) The water contact angle of the micro-nanostructured CaF2 film is 139.4°. The micro-nanostructured CaF2 film prepared by SF6 etching greatly improves the surface water contact angle, and the film has obvious self-cleaning ability.
[0045] Figure 4 The present invention provides an example of the effect of the incident angle on the short-circuit current density (J) of the micro-nanostructure CaF2 coated glass solar cell sc ) and the effect of the improvement of the photoelectric conversion efficiency (PCE), it can be more intuitively seen that as the incident light angle decreases from 90° to 30°, J sc The percentage of improvement increased from 7.6% to 17.68%, and the percentage of PCE improvement increased from 4.3% to 13.42%. That is, J sc The decreases of IR and PCE are much smaller than those at 30°. The micro-nanostructured CaF2 film has better anti-reflection performance than the uncoated glass and is less dependent on the change of the incident angle.
[0046] Compared with the super-hydrophobic anti-reflective CaF2 anti-reflection film prepared by oblique-angle vapor deposition technology reported in the literature (Superhydrophobic and antireflective nanograss-coated glass for high performance solar cells; Nano Res. Vol. 7 (005) (2014) p. 670-678.), the hydrophobic anti-reflective micro-nanostructure anti-reflection film prepared by the technical solution of this example has an increased transmittance band, improved anti-reflection performance, and further increased water contact angle of the film.
[0047] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A hydrophobic anti-reflection micro-nanostructure CaF 2 film, It is characterized in that The surface of the film presents an uneven micro-nanostructure, which appears as uneven pits at 2000 times magnification and as nanoparticles of different sizes at 70000 times magnification. The film was prepared by magnetron sputtering with CaF 2 As the target material, SF 6 As a reaction gas, it is added to the working gas Ar 2 Medium, SF 6 Ionized F - Ions are both in contact with quartz glass SiO 2 The reaction etches a concave-convex micro-nano structure on the glass surface, inhibiting the CaF 2 The F deficiency of the film; adjusting the sputtering process parameters working pressure and sputtering power can adjust the size of the pits, the size of the nanoparticles, and the size and porosity of the nanopores.
2. The hydrophobic anti-reflection micro-nanostructure CaF according to claim 1 2 film, It is characterized in that The surface of the film presents an uneven micro-nanostructure, which appears as unevenly sized pits at 2000 times and a random mixture of nanoparticles of different sizes at 70,000 times. Nanopores of different sizes are distributed between the particles, and their sizes are between 20-200nm; the root mean square roughness of the film surface reaches 20-300nm.
3. The hydrophobic anti-reflection micro-nanostructure CaF according to claim 1 2 film, It is characterized in that SF 6 As a reaction gas, it is added to the working gas Ar 2 Medium, SF 6 Ionized F - Ions are both in contact with quartz glass SiO 2 The reaction etches a concave-convex micro-nano structure on the glass surface, inhibiting the CaF 2 The film is poor in F, the SF 6 The gas doping amount is 0.1%-20%.
4. The hydrophobic anti-reflection micro-nanostructure CaF according to claim 1 2 film, It is characterized in that The average transmittance of the substrate glass in the wavelength range of 300-1100nm can be increased by 1-5 percentage points, and the water contact angle on the film surface can reach up to 139.4°, which is close to a super hydrophobic surface.