Epoxy resin hydrophilic agent and preparation method thereof
Through the combination of starch, KH550 silane coupling agent and absolute ethanol, an epoxy resin hydrophilic agent is formed, which solves the problem of hydrophobicity of epoxy resin, achieves a balance of high hydrophilicity and structural strength, and is suitable for permeable pavement construction.
Patent Information
- Application Number
- CN202111535692.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-15
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2041-12-15
AI Technical Summary
The existing epoxy resin is a hydrophobic material, which makes it difficult for water droplets to penetrate into the permeable pavement or the penetration speed is slow, which affects the water permeability effect. Increasing the amount of hydrophilic materials added will increase the material cost and reduce the structural strength.
A combination of starch, KH550 silane coupling agent and absolute ethanol is used to form a stable chemical coating on the starch surface to form an epoxy resin hydrophilic agent, and to form a stable chemical link with the epoxy resin to improve its hydrophilicity sex.
The high hydrophilicity of epoxy resin is achieved, and the water contact angle is less than 50°, which improves the water permeability effect while maintaining structural strength and reducing material costs. It is suitable for large-area permeable pavement construction.
Smart Images

Figure BDA0003413131680000071
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of chemical engineering, in particular to an epoxy resin hydrophilic agent and a preparation method thereof. Background Art
[0002] With the substantial improvement of my country's urbanization level, the area of hardened pavement has increased dramatically, which not only destroyed the original ecosystem, but also changed the original natural ecological background and hydrological characteristics of the city. More than 70% of the runoff formed by rainfall is discharged, making it impossible for the city to store water, resulting in the phenomenon of "heavy rain will cause flooding, and drought after rain". Sponge city is a historical and strategic transformation from the era of engineering drainage with fast drainage, timely and nearby drainage, and rapid drainage to the six-in-one comprehensive drainage and ecological drainage of "infiltration, retention, storage, purification, use, and drainage". Permeable pavement is the core measure of sponge city. The existing method for preparing permeable pavement is to use epoxy resin to bond sand and gravel. After the epoxy resin is hardened, the sand and gravel are tightly bonded together to form a hard pavement; and water can flow into the ground from the gap to form the first permeable layer of sponge city. However, the existing ordinary epoxy resin is a hydrophobic material, and it is difficult for water droplets to penetrate it, or the penetration speed is slow, resulting in a greatly weakened permeable effect; therefore, it is necessary to modify the epoxy resin to be hydrophilic.
[0003] In the prior art, the epoxy resin is hydrophilically modified by chemical modification and physical mixing. The chemical modification method is to graft hydrophilic materials on the epoxy resin or curing agent molecular chain; while the physical mixing method is to mix hydrophilic materials into the epoxy resin so that the epoxy resin can achieve a hydrophilic effect after curing. However, there are the following disadvantages:
[0004] The hydrophilic effect is only good when the amount of hydrophilic material added is large enough; however, the increase in the amount of hydrophilic material added not only increases the material cost, but also has a significant impact on the structural strength of the permeable layer.
[0005] Therefore, there is an urgent need for an epoxy resin hydrophilizing agent with good hydrophilic effect. Summary of the invention
[0006] The purpose of the present invention is to provide an epoxy resin hydrophilic agent and a preparation method thereof in order to solve the problem that the hydrophilic effect of the currently used epoxy resin hydrophilic agent is insufficient.
[0007] In order to achieve the above object, the present invention provides an epoxy resin hydrophilic agent, comprising the following raw materials in parts by weight:
[0008] 100 parts of starch;
[0009] KH550 silane coupling agent 1-50 parts;
[0010] 100-500 parts of anhydrous ethanol.
[0011] Further, preferably, the following raw materials are included in parts by weight:
[0012] 100 parts of starch;
[0013] KH550 silane coupling agent 2-30 parts;
[0014] 200-400 parts of anhydrous ethanol.
[0015] Further, preferably,
[0016] The weight average molecular weight Mw of starch is 5,000 to 500,000.
[0017] Furthermore, preferably, the weight average molecular weight Mw of the starch is 10,000 to 200,000.
[0018] Further, preferably, the application of epoxy resin hydrophilic agent in epoxy resin modification,
[0019] After the epoxy resin hydrophilic agent is added to the epoxy resin at a weight ratio of 1:1, the hydrophilic contact angle of the epoxy resin is less than 50°.
[0020] The present invention also protects a method for preparing an epoxy resin hydrophilic agent, the method comprising:
[0021] Weigh the raw materials according to weight ratio:
[0022] 100 parts of starch, 1-50 parts of KH550 silane coupling agent, 100-500 parts of anhydrous ethanol;
[0023] In the range of -5℃~50℃, pour the weighed anhydrous ethanol into the dissolving tank, and add KH550 silane coupling agent while stirring; wherein, the stirring speed is 50~200r / min, and stirring is carried out for 30 minutes;
[0024] Continue to add starch into the dissolving tank and stir for 60 minutes at a stirring speed of 50-200 r / min;
[0025] Obtain epoxy resin hydrophilic agent.
[0026] Further, preferably,
[0027] The weight average molecular weight Mw of starch is 5,000 to 500,000.
[0028] Further, preferably,
[0029] The preparation method of the epoxy resin hydrophilic agent is applied to epoxy resin modification. After the epoxy resin hydrophilic agent is added to the epoxy resin at a weight ratio of 1:1, the hydrophilic contact angle of the epoxy resin is less than 50°.
[0030] As described above, an epoxy resin hydrophilic agent and a preparation method thereof of the present invention produce a highly hydrophobic and highly durable anticorrosive coating through fluorocarbon resin and long-chain silane; the beneficial effects are as follows:
[0031] 1) The present invention selects starch and its content, and the epoxy resin hydrophilic agent obtains a hydrophilic film, and the water contact angle is less than 50°, thereby achieving the technical effect of improving the hydrophilicity of the epoxy resin hydrophilic agent.
[0032] 2) A method of obtaining an epoxy resin hydrophilic agent by hydrolyzing KH550 silane coupling agent in anhydrous ethanol and then treating starch to form a stable chemical coating on the starch surface; wherein the KH550 silane coupling agent can form a stable chemical link with the epoxy resin to achieve a technical effect of stable hydrophilicity;
[0033] 3) The epoxy resin hydrophilic agent is easy to prepare, the raw materials are cost-effective, and the market competitiveness is strong, which is suitable for large-scale promotion in the field of permeable pavement construction.
[0034] In order to achieve the above and related purposes, one or more aspects of the present invention include the features that will be described in detail later and are particularly pointed out in the claims. The following description describes some exemplary aspects of the present invention in detail. However, these aspects indicate only some of the various ways in which the principles of the present invention can be used. In addition, the present invention is intended to include all of these aspects and their equivalents. DETAILED DESCRIPTION
[0035] It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. If no specific techniques or conditions are specified in the embodiments, the techniques or conditions described in the literature in the field or the product instructions are used. If the manufacturers of the reagents or instruments used are not specified, they can be purchased from regular channels.
[0036] The present invention discloses an epoxy resin hydrophilic agent and a preparation method thereof, wherein silane and anhydrous ethanol are added for hydrolysis, starch is grafted and modified, and a stable chemical coating is formed on the starch surface to obtain the epoxy resin hydrophilic agent; wherein the KH550 silane coupling agent can form a stable chemical link with the epoxy resin, thereby forming a stable hydrophilic structure, and the epoxy resin is suitable for permeable pavement construction scenarios.
[0037] The present invention provides a raw material composition of an epoxy resin hydrophilic agent, including: 100 parts of starch; 1 to 50 parts of KH550 silane coupling agent; and 100 to 500 parts of anhydrous ethanol. The present invention limits the components of the raw materials to the above range, and can obtain an anti-corrosion coating with high stability and hydrophobicity that meets the requirements. The weight average molecular weight Mw of the starch is 5000 to 500000.
[0038] Epoxy resin is an important thermosetting resin, which can be used as a resin matrix for adhesives, coatings and composite materials, and is widely used in industrial manufacturing fields such as coatings, machinery, electronics, and transportation. It was found through experiments that when the substance provided by the present invention is used as a hydrophilic agent in epoxy resin, the hydrophilic effect is greatly improved, while other substances either cannot provide better compatibility (such as glycol ether, glycerol ether, etc.), or may reduce the structural strength (such as various modified salts). Only the substance selected by the present invention, on the one hand, is chemically linked to the epoxy resin and has good compatibility with the main component; on the other hand, it can float to the surface during curing, forming a good hydrophilic effect and reducing the contact angle between the epoxy resin and water. The epoxy resin can be, but is not limited to, one or more of E20, E44 and E51.
[0039] It should be noted that by adding silane and anhydrous ethanol for hydrolysis, and then grafting the starch, a chemical reaction with the epoxy resin is achieved to form a stable hydrophilic structure. The KH550 silane coupling agent is called 3-aminopropyltriethoxysilane in Chinese and 3-Aminopropyltriethoxysilane in English, with a chemical formula of C 9 H 23 NO 3 Chemical substances of Si; a class of low molecular weight organic silicon compounds with special structures, which have active functional groups with affinity or reaction ability with polymer molecules. Its X-group water forms silanol, and the silanol of each silane molecule associates with each other to form a network structure film covering the surface of the powder particles, making the surface of the inorganic powder organic. It is a better choice for preparing epoxy resin hydrophilic agent.
[0040] The weight average molecular weight of starch is between 5000 and 500000 (g / mol), and the hydrophilic effect of epoxy resin hydrophilic agent is better when the weight average molecular weight of starch is between 10000 and 200000 (g / mol); when the weight average molecular weight is less than 5000 (g / mol), the compatibility with anhydrous ethanol is too good, and partial dissolution leads to surface modification failure; and when the weight average molecular weight is greater than 500000 (g / mol), the compatibility with water is poor.
[0041] The above materials are selected as modified materials mainly because these resins have the advantages of good compatibility with epoxy resin and good modification effect, and epoxy resin hydrophilic agents with high stability, good hydrophilic effect and low cost can be obtained. Specifically, the above materials are selected as modified materials mainly because the substances selected by the present invention are chemically linked to the epoxy resin on the one hand, and have good compatibility with the main components, and on the other hand, they can float to the surface during curing, forming a good hydrophilic effect, reducing the contact angle between the epoxy resin and water, and are a better choice as epoxy resin hydrophilic agents.
[0042] According to another aspect of the present invention, there is provided a method for preparing an epoxy resin hydrophilic agent, comprising the following steps:
[0043] Weigh 100 parts by weight of starch, 1 to 50 parts by weight of KH550 silane coupling agent, and 100 to 500 parts of anhydrous ethanol; pour the weighed anhydrous ethanol into a dissolving tank within a temperature range of -5°C to 50°C, add the weighed KH550 silane coupling agent while stirring at a speed of 50 to 200 r / min, react for 30 minutes, add starch, continue stirring at a speed of 50 to 200 r / min, and stir for 60 minutes to obtain an epoxy resin hydrophilic agent.
[0044] Various embodiments of the present invention will be described in detail below.
[0045] Example 1
[0046] Step S1: weigh the raw materials in the following weight ratio:
[0047] 100 parts of starch with a weight average molecular weight of 5000; 1 part of KH550 silane coupling agent; 100 parts of anhydrous ethanol;
[0048] Step S2: At a temperature of 25° C., pour the weighed anhydrous ethanol into a dissolving tank, add the weighed KH550 silane coupling agent while stirring, the stirring speed is 50 r / min, after reacting for 30 minutes, continue to add starch to the dissolving tank, continue stirring, the speed is 200 r / min, stir for 60 minutes, and finally obtain the epoxy resin hydrophilic agent of Example 1.
[0049] Example 2
[0050] Step S1: weigh the raw materials in the following weight proportions:
[0051] 100 parts of starch with a weight average molecular weight of 200,000; 2 parts of KH550 silane coupling agent; 200 parts of anhydrous ethanol;
[0052] Step S2: At a temperature of 45° C., pour the weighed anhydrous ethanol into a dissolving tank, add the weighed KH550 silane coupling agent while stirring, the stirring speed is 200 r / min, after reacting for 30 minutes, continue to add starch to the dissolving tank, continue stirring, the speed is 50 r / min, stir for 60 minutes, and finally obtain the epoxy resin hydrophilic agent of Example 2.
[0053] Example 3
[0054] Step S1: weigh the raw materials in the following weight ratio:
[0055] 100 parts of starch with a weight average molecular weight of 380,000; 50 parts of KH550 silane coupling agent; 5,000 parts of anhydrous ethanol;
[0056] Step S2: At a temperature of 35° C., pour the weighed anhydrous ethanol into a dissolving tank, add the weighed KH550 silane coupling agent while stirring, the stirring speed is 100 r / min, after reacting for 30 minutes, continue to add starch to the dissolving tank, continue stirring, the speed is 200 r / min, stir for 60 minutes, and finally obtain the epoxy resin hydrophilic agent of Example 3.
[0057] Example 4
[0058] Step S1: weigh the raw materials in the following weight ratio:
[0059] 100 parts of starch with a weight average molecular weight of 10,000; 30 parts of KH550 silane coupling agent; 280 parts of anhydrous ethanol;
[0060] Step S2: At a temperature of 30° C., pour the weighed anhydrous ethanol into a dissolving tank, add the weighed KH550 silane coupling agent while stirring, the stirring speed is 200 r / min, after reacting for 30 minutes, continue to add starch to the dissolving tank, continue stirring, the speed is 100 r / min, stir for 60 minutes, and finally obtain the epoxy resin hydrophilic agent of Example 4.
[0061] Example 5
[0062] Step S1: weigh the raw materials in the following weight ratio:
[0063] 100 parts of starch with a weight average molecular weight of 130,000; 15 parts of KH550 silane coupling agent; 400 parts of anhydrous ethanol;
[0064] Step S2: At a temperature of 25°C, pour the weighed anhydrous ethanol into a dissolution tank, add the weighed KH550 silane coupling agent while stirring, the stirring speed is 200r / min, after reacting for 30 minutes, continue to add starch to the dissolution tank, continue stirring, the speed is 100r / min, stir for 60 minutes, and finally obtain the epoxy resin hydrophilic agent of Example 5.
[0065] Example 6
[0066] Step S1: weigh the raw materials in the following weight ratio:
[0067] 100 parts of starch with a weight average molecular weight of 500,000; 10 parts of KH550 silane coupling agent; 450 parts of anhydrous ethanol;
[0068] Step S2: At a temperature of 25°C, pour the weighed anhydrous ethanol into a dissolving tank, add the weighed KH550 silane coupling agent while stirring, the stirring speed is 200r / min, after reacting for 30 minutes, continue to add starch to the dissolving tank, continue stirring, the speed is 200r / min, stir for 60 minutes, and finally obtain the epoxy resin hydrophilic agent of Example 6.
[0069] The epoxy resin hydrophilic agent obtained in Examples 1 to 6 was mixed with epoxy resin in a mass ratio of 1:1, and the products were cured; the pure epoxy resin in the comparative example and the products treated with the epoxy resin hydrophilic agent in Examples 1 to 6 were set as experimental groups 1 to 7 respectively; the contact angle of the products in experimental groups 1 to 7 to water was tested on a JCY series contact angle meter (Dataphysics) at room temperature, and the test results are shown in Table 1:
[0070] Table 1 Comparison of water contact angles of products in experimental groups 1 to 7
[0071]
[0072] It should be noted that when the water contact angle is 0°<90°, the liquid can wet the solid, and the smaller the angle, the better the wettability, which is called the hydrophilic contact angle. When the water contact angle is 90°<180°, the liquid does not wet the solid, which is also called the hydrophobic contact angle or the water-repellent contact angle.
[0073] The hydrophilic contact angle of the epoxy resin not treated with a hydrophilic agent in the experimental group 1 of the comparative example tested in this experiment is 80°; while the hydrophilic contact angles of the experimental groups 2 to 7 are reduced (the maximum is 48°); by selecting the raw materials and the content, an epoxy resin hydrophilic agent with good hydrophilic effect is obtained. Compared with the ordinary hydrophilic agent in the prior art, the formed hydrophilic contact angle is less than 50°, and it has hydrophilicity.
[0074] Furthermore, the hydrophilic contact angles of Experiments 3, 5, and 6 are smaller (maximum 44°), indicating that when the weight average molecular weight Mw of starch is 10,000 to 200,000, the KH550 silane coupling agent is 2 to 30 parts, and the anhydrous ethanol is 200 to 400 parts, the hydrophilic effect of the epoxy resin hydrophilic agent obtained is better.
[0075] In summary, the epoxy resin hydrophilic agent of the present invention and the epoxy resin hydrophilic agent obtained by the preparation method have good compatibility with the main components of epoxy resin and curing agent on the one hand; on the other hand, after adding the epoxy resin hydrophilic agent, the epoxy resin has good affinity with water when applied to the permeable pavement, can quickly guide water penetration, can effectively improve the hydrophilicity of the epoxy resin after curing, and when applied on the permeable pavement, water droplets can quickly penetrate. It has the technical effect of simple preparation, high cost performance of raw materials, strong market competitiveness, and is suitable for large-scale promotion in the field of permeable pavement construction.
[0076] However, those skilled in the art should understand that various improvements can be made to the epoxy resin hydrophilic agent and preparation method provided by the present invention without departing from the content of the present invention. Therefore, the protection scope of the present invention should be determined by the content of the attached claims.
Claims
1. An epoxy resin hydrophilic agent, characterized in that: It is composed of the following raw materials in parts by weight: Starch 100 parts; KH550 silane coupling agent 1-50 parts; 100-500 parts of anhydrous ethanol; The weight average molecular weight Mw of the starch is 10000-200000; After the epoxy resin hydrophilizing agent is added to the epoxy resin, the hydrophilic contact angle of the epoxy resin is less than 50°.
2. The epoxy resin hydrophilizing agent according to claim 1, characterized in that: The invention comprises the following raw materials in parts by weight: Starch 100 parts; KH550 silane coupling agent 2-30 parts; 200-400 parts of anhydrous ethanol.
3. The use of the epoxy resin hydrophilizing agent according to claim 1 in epoxy resin modification, characterized in that: The epoxy resin hydrophilic agent is added to the epoxy resin at a weight ratio of 1:
1.
4. A method for preparing an epoxy resin hydrophilic agent, characterized in that the method include: Weigh the raw materials according to weight ratio: 100 parts of starch, 1-50 parts of KH550 silane coupling agent, 100-500 parts of anhydrous ethanol; Pour the weighed anhydrous ethanol into a dissolving tank at -5°C to 50°C, and add KH550 silane coupling agent while stirring; wherein the stirring speed is 50-200 r / min, and the stirring is performed for 30 minutes; Continue to add starch into the dissolving tank and stir for 60 minutes at a stirring speed of 50-200 r / min to obtain an epoxy resin hydrophilic agent; The weight average molecular weight Mw of the starch is 10000-500000; After the epoxy resin hydrophilizing agent is added to the epoxy resin, the hydrophilic contact angle of the epoxy resin is less than 50°.
5. Application of the preparation method of epoxy resin hydrophilic agent according to claim 4 in epoxy resin modification, characterized in that: The epoxy resin hydrophilic agent is added to the epoxy resin at a weight ratio of 1:1.