Nitrogen-doped porous carbon and multivalent copper composite material and preparation method and application thereof

By applying nitrogen-doped porous carbon and multivalent copper composites in the electrofenton-like method, the problems of low generation efficiency and poor stability of the existing catalyst H2O2 are solved, and the efficient degradation of ciprofloxacin is achieved, ensuring the environment and Health and safety.

CN114452995BActive Publication Date: 2024-11-08TIANJIN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210011397.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-01-06
Publication Date
2024-11-08
Estimated Expiration
2042-01-06

AI Technical Summary

Technical Problem

In the electrofenton-like method, the selective generation efficiency of H2O2 is low, the degradation efficiency is low, and the catalyst is unstable, making it difficult to effectively remove ciprofloxacin (CIP) pollution, affecting the environment and health.

Method used

Using nitrogen-doped porous carbon and multivalent copper composite (Cu+/Cu0-NC) as catalyst, modified Cu-btc MOFs were synthesized by solvothermal method, and calcined at high temperature, combined with electrofenton-like technology, at room temperature Apply voltage and oxygen are introduced to achieve efficient degradation of CIP.

Benefits of technology

A 98.1% CIP degradation efficiency was achieved and high stability and reusability were maintained in an acidic environment, significantly improving the degradation efficiency and catalyst stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114452995B_ABST
    Figure CN114452995B_ABST
Patent Text Reader

Abstract

The invention discloses a nitrogen-doped porous carbon and multivalent copper composite material and a preparation method and application thereof. The preparation method comprises the following steps: mixing copper salt, benzimidazole, 1,3,5-benzenetricarboxylic acid and a solvent until uniform to obtain a solution, heating the solution at 80-100°C for 5-7h, naturally cooling to room temperature 20-25°C, centrifuging, washing, and drying to obtain modified Cu-btc MOFs; calcining the modified Cu-btc MOFs at 600-1000°C for 0.5-1.5h in a nitrogen or inert gas environment to obtain a nitrogen-doped porous carbon and multivalent copper composite material. The nitrogen-doped porous carbon and multivalent copper composite material is beneficial to the reaction of ·OH and ·O2 due to the doping of nitrogen sites and the circulation of multivalent copper. ‑ The nitrogen-doped porous carbon and multivalent copper composite material can maintain a high degradation efficiency in the acidic range of pH 1 to 3, and has excellent stability and reusability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of treating antibiotics in sewage by an electro-Fenton-like process, and specifically relates to a nitrogen-doped porous carbon and multivalent copper composite material, and a preparation method and application thereof. Background Art

[0002] The widespread use of antibiotics has made them a new class of potential pollutants, but at the same time has caused a series of environmental problems, such as the emergence of multidrug-resistant bacteria, which disrupts the balance of the ecosystem and human health. Ciprofloxacin (CIP) is a typical quinolone antibiotic, which is widely used in humans and animals due to its wide range of activity against bacteria. However, since it cannot be completely absorbed by humans and animals, it exists in large quantities in the natural environment in a pharmacological form, which is a potential threat to both humans and the ecological environment. Today, CIP has been detected in different environmental matrices. Therefore, it is urgent to develop effective technologies to remove CIP from the environment, which is very important for creating a green and harmonious ecological environment.

[0003] Fenton is considered to be an effective method for the degradation of organic pollutants. It can use the strong oxidizing property of OH to decompose various organic pollutants into CO2, H2O and other small molecules. However, its widespread use is limited by the low utilization rate of H2O2, the danger during transportation and storage, the secondary pollution of iron ions and the pH range of use. In order to solve this problem, more and more people are keen to develop an iron-free catalyst to achieve effective degradation of antibiotics through the electro-Fenton technology, which activates oxygen on the cathode surface to produce 2e - Reduction reaction, selectively generating H2O2 in situ, which is then activated and decomposed into various active free radicals, such as ·OH, ·O2 - and O2 1 , thereby achieving the degradation of CIP. In this process, the selective generation of H2O2 and the type and amount of active oxygen species are the main factors affecting the degradation efficiency. However, the catalysts reported so far face problems such as low selective generation efficiency of H2O2, low degradation efficiency and catalyst instability. Therefore, in order to solve this problem, it is crucial to develop an efficient and stable catalyst. Summary of the invention

[0004] In view of the shortcomings of the prior art, the present invention aims to provide a method for preparing a nitrogen-doped porous carbon and multivalent copper composite material, wherein the preparation method synthesizes a modified Cu-btc MOFs (precursor) by a solvent thermal method, and then calcines at a high temperature to obtain Cu + / Cu 0 -NC.

[0005] Another object of the present invention is to provide a nitrogen-doped porous carbon and multivalent copper composite material (Cu + / Cu 0 -NC).

[0006] Another object of the present invention is to provide the use of the nitrogen-doped porous carbon and multivalent copper composite material as a catalyst in the degradation of CIP. + / Cu 0 -NC is uniformly dispersed in CIP wastewater as a catalyst, with carbon felt (CF) as the cathode and Pt sheet as the anode. Under the conditions of continuous stirring at room temperature, continuous introduction of oxygen and application of voltage, effective degradation of CIP is achieved, and the degradation efficiency can reach 98.1%.

[0007] The purpose of the present invention is achieved through the following technical solutions.

[0008] A method for preparing a nitrogen-doped porous carbon and multivalent copper composite material comprises the following steps:

[0009] 1) mixing copper salt, benzimidazole, 1,3,5-benzenetricarboxylic acid and a solvent until uniform to obtain a solution, wherein, by weight, the ratio of the copper salt, benzimidazole and 1,3,5-benzenetricarboxylic acid is 1:(15-20):(0.5-1.5);

[0010] In the step 1), the solvent is a mixture of ethanol and DMF, and the ratio of ethanol to DMF is (0.5-1.5): (0.5-1.5) by volume.

[0011] In the step 1), the ratio of the amount of the copper salt to the volume of the solvent is 1:(70-110), the unit of the amount of the substance is mmol, and the unit of the volume is mL.

[0012] In the step 1), copper salt, benzimidazole and 1,3,5-benzenetricarboxylic acid are respectively mixed evenly with the solvent to obtain a first solution, a second solution and a third solution in sequence, the first solution and the second solution are mixed, stirred at room temperature of 20 to 25° C. for 10 to 30 minutes, and then the third solution is added to achieve mixing of copper salt, benzimidazole, 1,3,5-benzenetricarboxylic acid and the solvent, wherein the ratio of the first solution, the second solution and the third solution is (0.5-1.5):(0.5-1.5):(1-3) by volume.

[0013] 2) heating the solution obtained in step 1) at 80-100° C. for 5-7 h, naturally cooling to room temperature (20-25° C.), centrifuging, washing, and drying to obtain modified Cu-btc MOFs;

[0014] 3) In a nitrogen or inert gas environment, calcining the modified Cu-btc MOFs at 600-1000° C. for 0.5-1.5 h to obtain a nitrogen-doped porous carbon and multivalent copper composite material.

[0015] In step 3), the heating rate is 1-4°C min -1 .

[0016] The nitrogen-doped porous carbon and multivalent copper composite material obtained by the preparation method.

[0017] The nitrogen-doped porous carbon and multivalent copper composite material is used as a catalyst in the degradation of CIP.

[0018] In the above technical solution, the degradation is an electro-Fenton system degradation.

[0019] In the above technical solution, the degradation efficiency reaches 98.1% within 2 hours.

[0020] In the above technical scheme, the method of degradation of the electro-Fenton system is: adding nitrogen-doped porous carbon and multivalent copper composite materials into CIP wastewater, using carbon felt and platinum sheet as cathode and anode respectively, introducing O2 into it under continuous stirring conditions, and applying a voltage of 2 to 6V.

[0021] In the above technical solution, the pH of the CIP wastewater is 1-7, preferably pH=3.

[0022] In the above technical solution, the flow rate of O2 is 90~110mL·min -1 .

[0023] In the above technical solution, the ratio of the mass fraction of the nitrogen-doped porous carbon and multivalent copper composite material to the volume fraction of the CIP wastewater is (5-15): (50-70), the unit of the mass fraction is mg, and the unit of the volume fraction is mL.

[0024] In the above technical solution, the concentration of CIP in CIP wastewater is 40-60 mg·L -1 .

[0025] In the above technical solution, the CIP wastewater also contains Na2SO4, and the concentration of Na2SO4 in the CIP wastewater is 0.02-0.07 mol·L -1 .

[0026] Compared with the prior art, the present invention has the following advantages:

[0027] The nitrogen-doped porous carbon and multivalent copper composites are beneficial to the ·OH and ·O2 - The generation of , thereby improving the adsorption and degradation of CIP.

[0028] The nitrogen-doped porous carbon and multivalent copper composite material can maintain a high degradation efficiency in the acidic range of pH 1 to 3 and has excellent stability and reusability. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 The SEM, TEM and energy dispersive X-ray spectroscopy (EDS) elemental spectra of the nitrogen-doped porous carbon and multivalent copper composite material obtained in Example 2, wherein (a)-(b) are SEM images, (c)-(e) are TEM images, and (f) is an energy dispersive X-ray spectroscopy (EDS) elemental spectrum;

[0030] Figure 2 The Cu prepared in Examples 1 to 4 + / Cu 0 -NC and Cu + / Cu 0 -XRD pattern of C;

[0031] Figure 3 The Cu prepared in Examples 1 to 4 + / Cu 0 -NC and Cu + / Cu 0 - Raman spectrum of C;

[0032] Figure 4 The Cu prepared in Example 2 + / Cu 0 -N2 adsorption-desorption isotherm of NC;

[0033] Figure 5 The Cu prepared in Example 2 + / Cu 0 - pore size distribution of NC;

[0034] Figure 6 The Cu prepared in Example 2 + / Cu 0 -NC XPS full spectrum (a) and high-resolution XPS spectra of C1s (b), O 1s (c), Cu 2p (d), Cu Auger spectrum (e) and N1s (f);

[0035] Figure 7 Cu obtained in Example 2 + / Cu 0 -NC and Cu obtained in Example 4 + / Cu 0 -C electrochemical spectrum, where (a) is the CV curve and (b) is the EIS spectrum. + / Cu 0-C-800 is the Cu prepared in Example 4 + / Cu 0 -C, Cu + / Cu 0 -NC-800 is the Cu prepared in Example 2 + / Cu 0 -NC;

[0036] Figure 8 is the CIP degradation efficiency of Examples 5 to 8 (different temperatures and heteroatom doping);

[0037] Fig. 9 is the CIP degradation efficiency (different pH values) of Example 6 and Examples 9 to 12;

[0038] Fig.10 is the CIP degradation efficiency (under different voltages) of Example 6 and Examples 13 to 15;

[0039] Fig.11 The Cu prepared in Example 2 + / Cu 0 - Stability test of NC;

[0040] Fig.12 The CIP degradation efficiency of Examples 6, 16 and 17 in different processes;

[0041] Fig.13 It is the TOC removal efficiency of Example 6 and Example 8. DETAILED DESCRIPTION

[0042] The technical solution of the present invention is further described below in conjunction with specific embodiments.

[0043] The purity and purchasing manufacturers of the drugs involved in the following examples are as follows:

[0044]

[0045] The models and manufacturers of the instruments involved in the following embodiments are as follows:

[0046]

[0047]

[0048] The test method for the degradation efficiency described below is UV-Vis spectrophotometry.

[0049] Examples 1 to 3

[0050] A method for preparing a nitrogen-doped porous carbon and multivalent copper composite material comprises the following steps:

[0051] 1) Cu(NO3)2·3H2O is prepared as a copper salt, and the copper salt, benzimidazole, 1,3,5-benzenetricarboxylic acid and a solvent are mixed until uniform to obtain a solution, wherein the ratio of the copper salt, benzimidazole and 1,3,5-benzenetricarboxylic acid is 1:17:1 in terms of molar fractions; the solvent is a mixture of ethanol and DMF, and the ratio of ethanol to DMF is 1:1 in terms of volume fractions; the ratio of the molar fraction of the copper salt to the volume fraction of the solvent in the solution is 1:90, and the unit of the molar fraction is mmol, and the unit of the volume fraction is mL.

[0052] In step 1), the method for mixing copper salt, benzimidazole, 1,3,5-benzenetricarboxylic acid and solvent until uniform is as follows: 0.1mmol copper salt is mixed with 9mL solvent to obtain a first solution; 1.7mmol benzimidazole is mixed with 9mL solvent to obtain a second solution; 0.1mmol 1,3,5-benzenetricarboxylic acid is mixed with 18mL solvent to obtain a third solution; the first solution and the second solution are mixed, stirred at room temperature of 20 to 25°C for 15 minutes, and then the third solution is added, wherein the ratio of the first solution, the second solution and the third solution is 1:1:2 by volume.

[0053] 2) heating the solution obtained in step 1) at 90° C. for 6 h, cooling naturally to room temperature (20-25° C.), centrifuging, washing the solid obtained by centrifugation with ethanol, and drying at 60° C. for 12 h to obtain modified Cu-btc MOFs;

[0054] 3) In a nitrogen environment, the modified Cu-btc MOFs were heated in a tube furnace from room temperature (20-25°C) at a rate of 2°C min -1 The temperature was raised to T℃ at a rate of 100 °C and calcined at T℃ for 1 h to obtain a nitrogen-doped porous carbon and multivalent copper composite material (Cu + / Cu 0 -NC).

[0055] Table 1

[0056] Example T(℃) Example 1 700 Example 2 800 Example 3 900

[0057] Example 4

[0058] A porous carbon and multivalent copper composite material (Cu + / Cu 0 -C) preparation method, comprising the following steps:

[0059] 1) dissolving 0.1 mmol Cu(NO3)2·3H2O in 9 mL of solvent and mixing well to obtain solution A, dissolving 0.1 mmol 1,3,5-benzenetricarboxylic acid in 18 mL of solvent to obtain solution B, and adding solution B to solution A to obtain solution C, wherein the solvent is a mixture of ethanol and DMF, and the ratio of ethanol to DMF is 1:1 by volume;

[0060] 2) Through a solvothermal reaction, solution C was heated at 90°C for 6 h, naturally cooled to room temperature 20-25°C, centrifuged, washed with ethanol, and dried at 60°C for 12 h to obtain a Cu-btc MOFs precursor;

[0061] 3) The Cu-btc MOFs precursor obtained in step 2) was placed in a tube furnace under a nitrogen atmosphere at 2°C min -1 The temperature was raised to 800 °C at a rate of 100 °C and calcined at 800 °C for 1 h to obtain a porous carbon and multivalent copper composite material (Cu + / Cu 0 -C).

[0062] The Cu in Example 2 was tested by scanning electron microscopy (SEM) and transmission electron microscopy (TEM). + / Cu 0 -NC at different magnifications of SEM images, TEM images and EDS images, characterizing the morphology and microstructure of the material. Figure 1 As shown, Figure 1 (a) and (b) are Cu + / Cu 0 -NC SEM picture, from which we can see that Cu + / Cu 0 -NC presents an octahedral morphology with a rough surface, and some metal ions are loaded on the surface of the carbon skeleton. Figure 1 (c)-(e) show the Cu obtained in Example 2 + / Cu 0 -NC TEM image shows obvious nitrogen-doped carbon layer and clear lattice fringes (d = 0.25nm), which may be related to the Cu2O (111) crystal plane. At the same time, energy dispersive X-ray spectroscopy (EDS) elemental spectrum analysis was also carried out, such as Figure 1 (f) The presence of C, N, O, and Cu elements was detected, indicating that Cu was successfully synthesized. + / Cu 0 -NC.

[0063] The Cu obtained in test examples 1 to 4 + / Cu 0 -NC and Cu + / Cu0 -C XRD pattern, the results are as follows Figure 2 As shown in the figure, Cu + / Cu 0 -NC and Cu + / Cu 0 -C has three obvious characteristic diffraction peaks at 43.2°, 50.4° and 74.1°, corresponding to the (111), (200) and (220) crystal planes of Cu (PDF NO.04-0836), respectively; the characteristic peak at 36.3° is attributed to the (111) crystal plane of Cu2O (PDF NO.78-2076), thus proving that the metal is composed of Cu and Cu2O.

[0064] The Cu obtained in Examples 1 to 4 was further studied by Raman spectroscopy. + / Cu 0 -NC and Cu + / Cu 0 -C defects and carbonization degree, thereby determining the active sites in the electro-Fenton process, and the results show that Figure 3 Medium. D belt (about 1330cm -1 ) and G belt (approximately 1580cm -1 ) represent sp3 defect carbon and sp2 hybridized graphitic carbon, respectively. Therefore, the intensity ratio of D band to G band (I D / I G ) to evaluate the defects and graphitization degree of the carbon material. D / I G The values ​​of CuO were 0.93, 1.22 and 1.15 respectively, which were lower than those of CuO obtained in Example 2. + / Cu 0 The value of -NC catalyst is 1.28, which indicates that changing the calcination temperature and heteroatom doping can increase the defect degree of the catalyst, thereby exposing more active sites and improving the catalytic performance.

[0065] Test Example 2 prepared Cu + / Cu 0 -NC N2 adsorption-desorption performance, the specific surface area and pore size of the samples were analyzed by BET method ( Figure 4 and Figure 5 ). For the Cu prepared in Example 2 + / Cu 0 -NC, the hysteresis curve belongs to type IV, which further proves the porosity of the material. + / Cu 0 -NC has a specific surface area of ​​270.18 m 2 ·g -1 , pore volume is 0.1cm3 ·g -1 , indicating that the Cu + / Cu 0 -NC has a larger specific surface area and pore size, which can expose more active sites and is beneficial to the degradation of pollutants.

[0066] Example 2 Cu + / Cu 0 The XPS wide scan spectrum of -NC and the fine spectra of C1s, O 1s, N 1s and Cu 2p are shown in Figure 2. Figure 6 As shown in af. + / Cu 0 -NC wide scan spectrum Figure 6 The presence of C, N, O and Cu spectral signals in a proves that Cu + / Cu 0 - Successful synthesis of NC. Figure 6 The XPS spectrum of C1s in b can be divided into four peaks, and the peaks at binding energies of 284.8 eV, 285.7 eV, 287.7 eV, and 290.5 eV correspond to C=C / CC, CN, C=O / CO, and O=CO. High-resolution O1s ( Figure 6 c) can be divided into three peaks, the diffraction peak at 531.2 eV is attributed to the Cu-O bond, the binding energy at 532.6 eV is attributed to the C=O on the carbon skeleton, and the binding energy at 534.0 eV is attributed to the adsorbed oxygen (·OH or O2). High-resolution Cu 2p spectra such as Figure 6 As shown in d, the existence of satellite peaks proves that Cu 2+ This may be attributed to the generation of Cu + and Cu 0 Oxidation in air, the peaks at binding energies of 932.9 eV and 952.7 eV are attributed to Cu + Cu 0 ; In order to distinguish Cu + and Cu 0 , the Cu Auger peak was analyzed, and the results are as follows Figure 6 As shown in e, the peaks at the binding energies of 570.4 eV and 568.4 eV correspond to Cu + and Cu 0 , thus proving the existence of Cu in multiple valence states. N1s spectra are shown in Figure 6 As shown in Fig. f, three types of nitrogen were observed, corresponding to pyridinic N (398.8 eV), pyrrolic N (400.0 eV) and graphitic N (401.4 eV), respectively. The results show that pyridinic N and graphitic N are beneficial to the oxygen reduction reaction, thereby improving the catalytic degradation efficiency.

[0067] Cu obtained in Study Example 2 + / Cu0 -NC and Cu obtained in Example 4 + / Cu 0 The electrochemical properties of -C were mainly studied by cyclic voltammetry (CV) and electrochemical impedance spectroscopy (EIS). The specific method is: using a CHI 660D electrochemical workstation, a three-electrode system, a platinum sheet as the auxiliary electrode, and a saturated calomel electrode as the reference electrode, the Cu obtained in Example 2 + / Cu 0 -NC or Cu obtained in Example 4 + / Cu 0 -C were used as catalysts and were evenly dispersed in ethanol, where the mass ratio of catalyst to ethanol was 1:1. They were then evenly dropped on a glassy carbon electrode and dried at 20-25°C for 30 min. As working electrodes, 0.5 mol·L -1 The performance test was carried out using the aqueous solution of Na2SO4 as the electrolyte solution. The results are as follows Figure 7 shown. Figure 7 a is Cu + / Cu 0 -NC and Cu + / Cu 0 -C CV curve, and Cu + / Cu 0 Compared with Cu-C + / Cu 0 -NC exhibited higher redox peaks, current response values, and peak areas, indicating that Cu + / Cu 0 -NC has good electron transport performance and electrochemical properties; Figure 7 b is Cu + / Cu 0 -NC and Cu + / Cu 0 EIS spectra of -C, Cu + / Cu 0 -NC has a smaller semicircle radius, indicating that it has a smaller resistance and is more conducive to electron transport.

[0068] Embodiments 5 to 13

[0069] The electro-Fenton degradation performance of CIP was tested in a 100 mL beaker at room temperature (20-25 °C). Specifically, 60 mL of simulated wastewater was poured into the beaker. The simulated wastewater was a mixture of Na2SO4, CIP and water. The concentration of Na2SO4 in the simulated wastewater was 0.05 mol·L -1 , the concentration of CIP is 50 mg·L -1 The pH of the simulated wastewater was increased from 0.5 mol·L -1 NaOH aqueous solution or 0.5 mol·L-1 The pH after adjustment is shown in Table 2. The carbon felt (3 cm × 5 cm × 0.6 cm) was pretreated by boiling in a 8.1% H2O2 aqueous solution at 90°C for 3 h, then boiling in a 9.72% HCl aqueous solution at 90°C for 1 h, then washing with clean water, and drying at 60°C for 24 h to obtain the pretreated carbon felt. The pretreated carbon felt was used as the cathode, the platinum sheet was used as the anode, and the Cu prepared in Examples 1 to 4 was + / Cu 0 -NC and Cu + / Cu 0 -C was used as a catalyst, 10 mg of the catalyst was poured into the simulated wastewater, and oxygen was continuously introduced under stirring at a flow rate of 100 mL min -1 ; After 30 minutes, the voltage was turned on to start the degradation process. The voltage value is shown in Table 2. In the electro-Fenton-like process, 2.5 mL of simulated wastewater was taken at regular time intervals and the absorbance of the solution was tested by UV-visible spectrophotometer.

[0070] Table 2

[0071] Example pH Voltage catalyst Example 5 3 4V Example 1 Example 6 3 4V Example 2 Example 7 3 4V Example 3 Example 8 3 4V Example 4 Example 9 1 4V Example 2 Example 10 2 4V Example 2 Embodiment 11 4 4V Example 2 Example 12 7 4V Example 2 Example 13 3 2V Example 2 Embodiment 14 3 3V Example 2 Embodiment 15 3 5V Example 2

[0072] The degradation effects of the CIP electro-Fenton systems of Examples 5 to 8 are as follows: Figure 8 As shown, in Examples 1 to 3, as the calcination temperature gradually increases, the highest degradation efficiency is shown at 800°C. This may be because the higher the calcination temperature, the more conducive it is to the exposure of active sites, thereby increasing the catalytic activity of the catalyst. However, too high a temperature may cause the destruction of the carbon skeleton structure, thereby reducing the degradation efficiency of CIP; in Example 4, by comparison, it can be seen that the doping of nitrogen sites can significantly improve the degradation efficiency of the catalyst. This may be because nitrogen doping accelerates the chemical adsorption of O2 by the catalyst, weakens OO, and promotes the effective generation of H2O2. In summary, the Cu prepared in Example 2 + / Cu 0 -NC can achieve the highest degradation efficiency, which can reach 98.1% degradation efficiency within 2h.

[0073] The degradation effects of the electro-Fenton systems of Examples 6 and 9 to 12 are as follows Fig. 9 As shown in Figure 2, when the pH changes from 1 to 3, the degradation efficiency of CIP gradually increases, and then the pH continues to increase, the degradation efficiency of CIP decreases significantly, and the maximum CIP degradation efficiency is reached at pH 3. This may be due to the fact that in an acidic environment, it is conducive to the degradation of Cu 0 The activation of H2O2 produces more multivalent copper, thereby promoting the degradation of pollutants. However, in a strong acidic environment, H2O2 can capture H +, generating a more stable [H3O2] + , thus hindering the effective activation of H2O2. When the pH is high, Cu + With OH in solution - The combination forms precipitation, which hinders the circulation of Cu's multiple valence states and reduces the generation of active oxygen species, thereby reducing the degradation efficiency.

[0074] The degradation effects of the electro-Fenton systems of Examples 6 and 13 to 15 are as follows Fig.10 As shown in the figure, when the voltage gradually increases from 2 V to 5 V, the degradation efficiency of CIP shows a degradation trend of increasing first and then decreasing, reaching the maximum degradation efficiency at 4 V. This phenomenon is mainly due to the fact that when the voltage gradually increases, many side reactions may occur, such as 4e - Oxygen reduction reaction, H2O2 further reduction to H2O and hydrogen evolution reaction, etc. When the voltage gradually decreases, the electron transfer speed is slower, which may hinder the Cu + / Cu 2+ cyclic reaction, thereby reducing the generation of reactive oxygen species.

[0075] Explore Cu + / Cu 0 According to the method of Example 6, four cycles of electro-Fenton degradation of CIP were carried out. The results are as follows Fig.11 In each cycle of the experiment, the simulated wastewater was replaced, the carbon felt and catalyst were recovered, washed with distilled water, and dried in an oven at 60°C before the next experiment. + / Cu 0 After four cycles of experiments, the degradation efficiency of CIP can still reach 98.2%, which shows that the Cu + / Cu 0 -NC has good stability and reusability.

[0076] Example 16 (Electrosorption)

[0077] The electrosorption performance of CIP was tested in a 100 mL beaker at room temperature of 20-25°C. Specifically, 60 mL of simulated wastewater was poured into the beaker. The simulated wastewater was a mixture of Na2SO4, CIP and water. The concentration of Na2SO4 in the simulated wastewater was 0.05 mol·L -1 , the concentration of CIP is 50 mg·L -1 The pH of the simulated wastewater was increased from 0.5 mol·L -1 NaOH aqueous solution or 0.5 mol·L -1The H2SO4 aqueous solution was adjusted to pH = 3. The pretreated carbon felt was used as the cathode and the platinum sheet was used as the anode. Oxygen was continuously introduced under stirring at a flow rate of 100 mL min -1 ; After 30 minutes, a voltage of 4 V was connected to start the degradation process. During the experiment, 2.5 mL of simulated wastewater was taken at regular intervals and its absorbance was tested by UV-Vis spectrophotometer.

[0078] Example 17 (Physical adsorption)

[0079] The physical adsorption test of CIP was carried out in a 100 mL beaker at room temperature of 20-25°C. Specifically, 60 mL of simulated wastewater was poured into the beaker. The simulated wastewater was a mixture of Na2SO4, CIP and water. The concentration of Na2SO4 in the simulated wastewater was 0.05 mol·L -1 , the concentration of CIP is 50 mg·L -1 The pH of the simulated wastewater was increased from 0.5 mol·L -1 NaOH aqueous solution or 0.5 mol·L -1 The H2SO4 aqueous solution was adjusted to pH = 3. The pretreated carbon felt was put into simulated wastewater, and 10 mg of Cu obtained in Example 2 was added thereto. + / Cu 0 -NC, oxygen was continuously introduced under stirring, and the flow rate of oxygen was 100 mL min -1 During the physical adsorption process, 2.5 mL of simulated wastewater was taken at regular time intervals to test its absorbance using a UV-visible spectrophotometer.

[0080] The effects of different degradation processes on CIP removal efficiency were studied by Example 6, Example 16 and Example 17. The results are as follows: Fig.12 Example 6 is a Fenton-like process, in which an external voltage is connected and Cu is added. + / Cu 0 -NC; Example 16 is an electrosorption process, in which only the external voltage is connected without adding Cu + / Cu 0 -NC; Example 17 is a physical adsorption process, in which no voltage is applied, but the same amount of Cu is added + / Cu 0-NC. For Example 17, it can be found that the removal efficiency of CIP by physical adsorption is negligible, with only 0.1% removal efficiency within 2 hours. In addition, in Example 16, electrosorption has a certain effect on the removal efficiency of CIP. At 30 minutes, the removal efficiency reaches 1.19%, but only 60.3% within 2 hours. In Example 6, it is found that the degradation efficiency of CIP reaches 81.24% in 30 minutes, and the degradation efficiency is greatly improved, reaching 98.1% degradation efficiency within 2 hours, which obviously highlights the superiority of the electro-Fenton method of the catalyst.

[0081] Example 6 ( Fig.13 Medium Cu + / Cu 0 -NC-800) and Example 8 ( Fig.13 Medium Cu + / Cu 0 -C-800) degradation process, such as the removal and mineralization efficiency of total organic carbon Fig.13 It is found that the TOC removal rate gradually increases with time. Compared with the conditions of Example 8, the TOC removal rate of Example 6 is significantly improved. This trend is consistent with the degradation efficiency of CIP. This may be because the doping of nitrogen sites promotes the exposure of more active sites, produces more active oxygen species, and breaks organic macromolecules, thereby improving the mineralization efficiency of CIP.

[0082] The present invention is described above by way of example. It should be noted that, without departing from the core of the present invention, any simple deformation, modification or other equivalent replacement that can be made by those skilled in the art without inventive effort falls within the protection scope of the present invention.

Claims

1. Application of a nitrogen-doped porous carbon and multivalent copper composite material as a catalyst in the degradation of ciprofloxacin, characterized in that: The degradation is an electro-Fenton system degradation method, and the electro-Fenton system degradation method is as follows: nitrogen-doped porous carbon and multivalent copper composite material is added to CIP wastewater, carbon felt and platinum sheet are used as cathode and anode respectively, O2 is introduced into the wastewater under continuous stirring conditions, and a voltage of 4V is applied. The pH of the CIP wastewater is 3, and the degradation efficiency reaches 98.1% within 2 hours; The preparation method of the nitrogen-doped porous carbon and multivalent copper composite material comprises the following steps: 1) mixing a copper salt, benzimidazole, 1,3,5-benzenetricarboxylic acid, and a solvent until uniformly mixed to obtain a solution, wherein the ratio of the copper salt, benzimidazole, and 1,3,5-benzenetricarboxylic acid is 1:(15-20):(0.5-1.5) based on the amount of the substance; 2) heating the solution obtained in step 1) at 80-100° C. for 5-7 hours, naturally cooling to room temperature (20-25° C.), centrifuging, washing, and drying to obtain modified Cu-btc MOFs; 3) calcining the modified Cu-btc MOFs at 800° C. for 1 h in a nitrogen or inert gas environment to obtain a nitrogen-doped porous carbon and multivalent copper composite material.

2. The use according to claim 1, characterized in that In the step 1), the solvent is a mixture of ethanol and DMF, and the ratio of ethanol to DMF is (0.5-1.5): (0.5-1.5) by volume.

3. The use according to claim 1, characterized in that In the step 1), the ratio of the amount of the copper salt to the volume of the solvent is 1:(70-110), the unit of the amount of the copper salt is mmol, and the unit of the volume is mL.

4. The use according to claim 1, characterized in that In step 3), the heating rate is 1-4°C·min -1 .

5. The use according to claim 1, characterized in that The flow rate of O2 is 90-110 mL min -1 .

6. The use according to claim 1, characterized in that The ratio of the mass fraction of the nitrogen-doped porous carbon and multivalent copper composite material to the volume fraction of the CIP wastewater is (5-15):(50-70), the unit of the mass fraction is mg, and the unit of the volume fraction is mL.

7. The use according to claim 1, characterized in that The CIP wastewater also contains Na2SO4, and the concentration of Na2SO4 in the CIP wastewater is 0.02-0.07 mol·L -1 .