A short process preparation method for high-strength and high-conductivity Cu-Ni-Co-Si-Li alloy high-precision narrow strip
By adding lithium Li and light rare earth RE to Cu-Ni-Co-Si alloy, a short process preparation method, including vacuum smelting, continuous extrusion and finishing rolling, the wide width of traditional Cu-Ni-Co-Si copper alloys was solved by using a short-process preparation method, including vacuum smelting, continuous extrusion and finishing rolling. The high cost of strip preparation and low material yield are problems such as high efficiency in preparing high-strength and high-conductance Cu-Ni-Co-Si-Li high-precision narrow bands.
Patent Information
- Application Number
- CN202210006749.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-01-05
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2042-01-05
AI Technical Summary
During the preparation of traditional Cu-Ni-Co-Si copper alloy wide-width strips, the equipment investment is large, the material yield is low, the processing process is long, and the alloy element content is high, which leads to difficulty in preparing ingots and serious dendrites segregation, resulting in strip processing. Difficult to form.
采用高强高导Cu-Ni-Co-Si-Li合金的短流程制备方法,包括真空熔炼、线坯铸造、连续挤压、扎制、精轧、固溶处理和时效处理,跳过传统宽幅带材切边分条制备,直接制备高精窄带,通过添加锂Li和轻稀土RE优化铸坯质量,降低高温变形抗力,实现连续加压加工。
Effectively reduces the cost of equipment investment, shortens the preparation process, improves the strength and conductivity of the alloy, reduces the size and heat treatment requirements of the casting billet, and obtains high-strength and high-conductivity Cu-Ni-Co with uniform second phase distribution and small grains. -Si-Li high precision narrow band.
Smart Images

Figure CN114453418B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of metal materials, and in particular to a short-process preparation method for a high-strength and high-conductivity Cu-Ni-Co-Si-Li alloy high-precision narrow strip. Background Art
[0002] Cu-Ni-Co-Si alloys have high strength, high elasticity, good electrical conductivity and good stress relaxation resistance. They are widely used in electronic, electrical, mechanical and other industrial fields. They can be used as integrated circuit lead frames, high current connectors, transistor carriers and high elastic contacts. In recent years, with the development of electronic information products towards miniaturization, lightness, multi-function and intelligence, the demand for high-strength and high-conductivity Cu-Ni-Co-Si copper alloy narrow strips has increased sharply. In the past, Cu-Ni-Co-Si alloy narrow strips were mostly prepared by cutting and stripping wide strips, while Cu-Ni-Co-Si alloy wide strips were mostly prepared by multi-pass rolling. This narrow strip preparation method has the following problems: (1) Large equipment investment and high preparation cost. Traditional Cu-Ni-Co-Si copper alloy wide strips have high requirements for rolling mills due to their large ingot size and deformation resistance, and require many rolling passes, resulting in low yield, long processing flow, and high preparation cost. (2) Due to the high alloying element content and the large number of alloying elements, large-sized Cu-Ni-Co-Si ingots are difficult to prepare, and the dendrite segregation inside the ingot is serious and cannot be completely eliminated, which brings difficulties to the subsequent rolling process and makes the strip extremely easy to crack during the processing and forming process. Summary of the invention
[0003] The present application provides a short-process preparation method for a high-strength and high-conductivity Cu-Ni-Co-Si-Li alloy high-precision narrow strip, which can solve the problems that traditional Cu-Ni-Co-Si copper alloy wide strips have large ingot size and deformation resistance, high requirements for rolling mills, and many rolling passes, resulting in large equipment investment, low yield rate, long processing flow, and high preparation cost; and the problem that large-sized Cu-Ni-Co-Si ingots are difficult to prepare due to high alloy element content and a large number of alloying elements, and the dendrite segregation inside the ingot is serious and cannot be completely eliminated, which brings difficulties to subsequent rolling processing and makes the strip extremely easy to crack during processing and forming.
[0004] This application adopts the following technical solutions:
[0005] The present application provides a short-process preparation method for a high-strength and high-conductivity Cu-Ni-Co-Si-Li alloy high-precision narrow strip, comprising the following steps: vacuum melting the raw materials to obtain a mixed melt, casting the mixed melt into a wire billet to obtain a cast billet, wherein the composition of the cast billet is: nickel Ni 1.0-2.0wt.%, cobalt Co 0.5-1.0wt.%, silicon Si 1-2wt.%, magnesium Mg 0-0.1wt.%, lithium Li 0.03-0.1wt.%, light rare earth RE 0.05-0.2wt.%, and the rest is copper Cu. Continuously extruding the cast billet to obtain a copper bar. Rolling the copper bar to obtain a plate. Finish rolling the plate to obtain a strip. Solution treating the strip to obtain a solution treated strip, and aging treating the solution product to obtain an aging treated strip. Trimming and coiling the aging treated strip to obtain a high-precision narrow strip.
[0006] Furthermore, during the vacuum melting process, the raw materials are placed in a vacuum melting furnace with a vacuum degree of -0.1 MPa. Argon gas is continuously introduced into the vacuum melting furnace. The melt temperature is controlled at 1120-1200°C during melting. After being kept warm for 30-60 minutes, mechanical stirring is performed.
[0007] Furthermore, during the wire billet casting process, the casting temperature is controlled at 800-950°C, the drawing speed is controlled at 70-100mm / min, the cooling water flow rate is 40-60m3 / min, and a Φ25-40mm billet is obtained.
[0008] Furthermore, during the continuous extrusion process, the ingot is heated to 700-800°C, the extrusion die is preheated to 600-700°C for continuous extrusion, the extrusion ratio is 10-20, the extrusion wheel speed is 5-11 rpm, and the extrusion gap is 0.8-1.5 mm, so as to obtain a copper bar with a thickness of 5-8 mm and a width of 60-100 mm.
[0009] Furthermore, during the rolling process, the copper bar is subjected to a solution treatment to obtain a soft copper bar, and then the soft copper bar is rolled on a four-roll rolling mill to obtain a plate with a thickness of 0.8-1 mm and a width of 120-180 mm.
[0010] Further, the copper busbar is subjected to a solution treatment, including: the copper busbar is subjected to a solution treatment at a temperature of 860-1020° C. for 2-3 hours.
[0011] Furthermore, during the finishing rolling process, the plate is subjected to a solution treatment to obtain an annealed copper alloy plate, and then the copper alloy plate is subjected to finishing rolling on a twenty-roll rolling mill to obtain a strip with a thickness of 0.4-0.8 mm and a width of 140-200 mm.
[0012] Further, the plate is subjected to a solution treatment, including: the plate is subjected to a solution treatment at a temperature of 700-920° C. for a time of 1-2 hours.
[0013] Furthermore, during the solution treatment process, the strip is subjected to solution heat treatment at a temperature of 850-1000° C., and the cooling method is water cooling.
[0014] Furthermore, during the aging treatment process, the solution treated strip is subjected to aging treatment at 400-500° C. for 18-24 hours.
[0015] The present application also provides a high-strength and high-conductivity Cu-Ni-Co-Si-Li alloy, comprising 1.0-2.0wt.% nickel, 0.5-1.0wt.% cobalt, 1-2wt.% silicon, 0-0.1wt.% magnesium Mg, 0.03-0.1wt.% lithium, 0.05-0.2wt.% light rare earth, and the remainder copper.
[0016] Compared with the prior art, this application has the following beneficial effects:
[0017] (1) In the present application, the quality of the ingot is further optimized and the performance of the ingot is improved by adding lithium Li elements and light rare earth RE elements. Lithium Li combines with oxygen and sulfur in the alloy to remove gases and impurities, thereby improving the electrical conductivity of the alloy; secondly, lithium Li as a lattice filling material can increase the overall density of the alloy, improve the alloy plasticity, reduce the resistance to high-temperature deformation, and can perform conventional continuous pressurization processing; in addition, lithium Li also has the effect of refining pure copper grains, making the ingot nearly isotropic, providing a structural basis for subsequent large deformation. Light rare earth RE has the effect of purifying the solution, which can reduce the impurity content in the ingot and improve the uniformity of the ingot; secondly, the addition of light rare earth RE can refine the precipitated phase in the alloy and improve the strength and conductivity of the final product;
[0018] (2) In this application, the traditional method of preparing high-precision narrow strips by cutting and stripping wide strips is skipped, and high-precision narrow strips are directly prepared. This reduces the investment cost of the equipment on the one hand, and can effectively reduce the size of the ingot on the other hand, reduce the heat treatment requirements of the ingot, and effectively reduce the preparation cost;
[0019] (3) In the present application, under the combined effect of alloying elements and new preparation ideas, a short-process large deformation process of small-sized Cu-Ni-Co-Si-Li casting with high deformation resistance becomes possible. The present application adopts the "continuous extrusion + high-precision rolling" deformation method, which greatly shortens the preparation process and obtains high-strength and high-conductivity Cu-Ni-Co-Si-Li high-precision narrow strips with uniform second phase distribution and fine grains. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1This is a flow chart for preparing the Cu-Ni-Co-Si-Li alloy in the embodiments of the present application. DETAILED DESCRIPTION
[0021] The technical methods in the embodiments of the present application are described clearly and completely below. Obviously, the described embodiments are only a part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.
[0022] Continuous extrusion is a processing method with no extrusion excess, high material utilization rate, and can achieve continuous production of products with extremely high production efficiency. In order to prepare a short-process Cu-Ni-Co-Si copper alloy narrow strip, refer to Figure 1 The embodiment of the present application provides a short process method for preparing a high-strength and high-conductivity Cu-Ni-Co-Si-Li alloy high-precision narrow strip, comprising the following steps:
[0023] Step 1: vacuum-smelting the raw materials to obtain a mixed melt, and casting the mixed melt into a wire billet to obtain a cast billet, wherein the composition of the cast billet is: nickel Ni 1.0-2.0wt.%, cobalt Co 0.5-1.0wt.%, silicon Si1-2wt.%, magnesium Mg 0-0.1wt.%, lithium Li 0.03-0.1wt.%, light rare earth RE 0.05-0.2wt.%, and the rest is copper Cu.
[0024] In the above steps, during the vacuum melting process, the raw materials are placed in a vacuum melting furnace with a vacuum degree of -0.1 MPa. Argon gas is continuously introduced into the vacuum melting furnace. The melt temperature is controlled at 1120-1200°C during melting. After keeping the temperature for 30-60 minutes, mechanical stirring is performed.
[0025] The raw materials are placed in a vacuum melting furnace, which can be: intermediate alloys such as Cu-5Li, Cu-Ni and high-purity copper are placed in a vacuum melting furnace according to a certain ratio.
[0026] The vacuum melting furnace may be a vacuum medium frequency melting furnace, and the argon gas may be high-purity argon gas.
[0027] During the wire billet casting process, the casting temperature is controlled at 800-950°C, the drawing speed is controlled at 70-100mm / min, the cooling water flow rate is 40-60m3 / min, and a Φ25-40mm billet is obtained.
[0028] It should be noted that the light rare earth RE can be a mixture of two or more light rare earth REs, or can be only one light rare earth RE.
[0029] Step 2: Continuously extrude the ingot to obtain a copper bar.
[0030] In the above steps, during the continuous extrusion process, the ingot is heated to 700-800°C, the extrusion die is preheated to 600-700°C for continuous extrusion, the extrusion ratio is 10-20, the extrusion wheel speed is 5-11rpm, and the extrusion gap is 0.8-1.5mm. A copper bar with a thickness of 5-8mm and a width of 60-100mm is obtained.
[0031] Step 3: Roll the copper bars to obtain plates.
[0032] In the above steps, during the rolling process, the copper bar is subjected to a solution treatment to obtain a soft copper bar, and then the soft copper bar is rolled on a four-roll rolling mill to obtain a plate with a thickness of 0.8-1 mm and a width of 120-180 mm.
[0033] The copper busbar is subjected to a solution treatment, which is: the copper busbar is subjected to a solution treatment at a temperature of 860-1020° C. for 2-3 hours.
[0034] Step 4: Finish rolling the plate to obtain a strip.
[0035] In the above steps, during the finishing rolling process, the plate is subjected to a solution treatment to obtain an annealed copper alloy plate, and then the copper alloy plate is finished rolled on a twenty-roll rolling mill to obtain a strip with a thickness of 0.4-0.8 mm and a width of 140-200 mm.
[0036] The plate is subjected to a solution treatment, which is: the plate is subjected to a solution treatment at a temperature of 700-920° C. for 1-2 hours.
[0037] Step 5: performing a solution treatment on the strip to obtain a solution treated strip, and performing an aging treatment on the solution product to obtain an aging treated strip.
[0038] In the above steps, during the solution treatment process, the strip is subjected to solution heat treatment at a temperature of 850-1000° C., and the cooling method is water cooling.
[0039] During the aging treatment, the solution treated strip is aged at 400-500°C for 18-24h.
[0040] Step 6: trim and roll the aging treated strip to obtain a high-precision narrow strip.
[0041] In the above steps, the high-precision narrow band is specifically a Cu-Ni-Co-Si-Li high-precision narrow band.
[0042] The embodiment of the present application also provides a high-strength and high-conductivity Cu-Ni-Co-Si-Li alloy, comprising 1.0-2.0wt.% nickel, 0.5-1.0wt.% cobalt, 1-2wt.% silicon, 0-0.1wt.% magnesium, 0.03-0.1wt.% lithium, 0.05-0.2wt.% light rare earth, and the remainder copper. The Cu-Ni-Co-Si-Li alloy is prepared by the short-process preparation method of the above embodiment.
[0043] This application adopts the "continuous extrusion + high-precision rolling" method. Through reasonable alloy composition design (addition of lithium Li and light rare earth), the high-temperature deformation resistance of the material is effectively reduced, and conventional continuous extrusion is achieved. The advantages of this method are as follows:
[0044] (1) By adding lithium Li and light rare earth RE elements, the quality of the ingot is further optimized and the performance of the ingot is improved. Lithium Li combines with oxygen and sulfur in the alloy to remove gases and impurities, thereby improving the electrical conductivity of the alloy; secondly, lithium Li as a lattice filling material can increase the overall density of the alloy, improve the alloy plasticity, reduce the high-temperature deformation resistance, and can perform conventional continuous pressurization processing; in addition, lithium Li also has the effect of refining pure copper grains, making the ingot nearly isotropic, providing a structural basis for subsequent large deformation. Light rare earth RE has the effect of purifying the solution, which can reduce the impurity content in the ingot and improve the uniformity of the ingot; secondly, the addition of light rare earth RE can refine the precipitation phase in the alloy and improve the strength and electrical conductivity of the final product.
[0045] (2) Skipping the traditional method of cutting and stripping wide strips to produce high-precision narrow strips, high-precision narrow strips are directly produced. This reduces the investment cost of the equipment on the one hand, and can effectively reduce the size of the ingot on the other hand, reduce the heat treatment requirements of the ingot, and effectively reduce the production cost.
[0046] (3) With the combined effect of alloying elements and new preparation ideas, a short-process large deformation process of small-sized Cu-Ni-Co-Si-Li casting with high deformation resistance becomes possible. This application adopts the "continuous extrusion + high-precision rolling" deformation method, which greatly shortens the preparation process and obtains a high-precision narrow strip of high-strength and high-conductivity Cu-Ni-Co-Si-Li alloy with uniform second phase distribution and fine grains.
[0047] The following is a detailed description with reference to specific embodiments:
[0048] Example 1
[0049] (1) Vacuum melting and wire casting
[0050] The master alloys such as Cu-5Li, Cu-Ni and high-purity copper are placed in a vacuum medium frequency melting furnace according to a certain ratio. The vacuum degree is -0.1MPa. High-purity argon is continuously introduced into the vacuum medium frequency melting furnace. The melt temperature is controlled at 1160℃ during melting. After 45 minutes of heat preservation, mechanical stirring is performed to obtain a mixed melt. The mixed melt is then cast into a wire billet. The casting temperature is controlled at 870℃, the casting speed is controlled at 80mm / min, and the cooling water flow rate is 50m 3 / min, to obtain a Φ35mm ingot, the composition of the ingot is: nickel Ni: 1.5wt.%; cobalt Co: 0.8wt.%; silicon Si: 1.5wt.%; magnesium Mg: 0.05wt.%; lithium Li: 0.04wt.%; light rare earth RE: 0.1wt.%; the rest is copper Cu.
[0051] (2) Continuous extrusion
[0052] The copper alloy ingot obtained in (1) was heated to 720°C, and the extrusion die was preheated to 620°C for continuous extrusion, with an extrusion ratio of 12, an extrusion wheel speed of 10 rpm, and an extrusion gap of 1.0 mm. A copper bar with a thickness of 7 mm and a width of 80 mm was obtained.
[0053] (3) Four-roll rolling
[0054] The copper bar obtained in (2) was subjected to solution treatment at 940°C for 2.5 hours to obtain a soft copper bar. The soft copper bar was then rolled on a four-roll mill to obtain a plate with a thickness of 0.9 mm and a width of 150 mm.
[0055] (4) Twenty-roller finishing rolling
[0056] The plate obtained in (3) was subjected to solution treatment at a temperature of 810°C for 1.5 hours to obtain an annealed copper alloy plate. The copper alloy plate was then finish rolled on a twenty-roll mill to obtain a strip with a thickness of 0.6 mm and a width of 160 mm.
[0057] (5) Solution treatment and aging treatment
[0058] The strip obtained in (4) was subjected to solution heat treatment at 920°C and water cooling to obtain a solution treated strip. The solution treated strip was then subjected to aging treatment at 450°C for 20 hours to obtain an aging treated strip.
[0059] (6) Trimming and rolling
[0060] The aging treated strip obtained in (5) is trimmed and rolled to obtain a Cu-Ni-Co-Si-Li alloy product - a Cu-Ni-Co-Si-Li alloy high-precision narrow strip, the performance indicators of which are shown in Table 1.
[0061] Table 1 Performance of Cu-Ni-Co-Si-Li alloy in Example 1
[0062] Tensile strength(MPa) 692 Yield strength (MPa) 637 Electrical conductivity (%IACS) 50.9
[0063] Example 2
[0064] (1) Vacuum melting and wire casting
[0065] The intermediate alloys such as Cu-5Li, Cu-Ni and high-purity copper are placed in a vacuum medium frequency melting furnace according to a certain ratio, the vacuum degree is -0.1MPa, and high-purity argon is continuously introduced into the vacuum medium frequency melting furnace. The temperature of the melt is controlled at 1160℃ during melting, and mechanical stirring is performed after 45 minutes of heat preservation to obtain a mixed melt. Subsequently, the mixed melt is cast into a wire billet, the casting temperature is controlled at 870℃, the casting speed is controlled at 80mm / min, and the cooling water flow rate is 50m3 / min to obtain a Φ35mm ingot. The composition of the ingot is: nickel Ni: 1.5wt.%; cobalt Co: 0.8wt.%; silicon Si: 1.5wt.%; magnesium Mg: 0.05wt.%; lithium Li: 0.06wt.%; light rare earth RE: 0.1wt.%; the rest is copper Cu.
[0066] (2) Continuous extrusion
[0067] The copper alloy ingot obtained in (1) was heated to 750°C, and the extrusion die was preheated to 650°C for continuous extrusion, with an extrusion ratio of 15, an extrusion wheel speed of 8 rpm, and an extrusion gap of 1.0 mm, to obtain a copper bar with a thickness of 7 mm and a width of 80 mm.
[0068] (3) Four-roll rolling
[0069] The copper bar obtained in (2) was subjected to a solution treatment at a temperature of 940°C for 2.5 hours to obtain a soft copper bar. The soft copper bar was then rolled on a four-roll mill to obtain a plate with a thickness of 0.9 mm and a width of 150 mm.
[0070] (4) Twenty-roller finishing rolling
[0071] The plate obtained in (3) was subjected to solution treatment at a temperature of 810°C for 1.5 hours to obtain an annealed copper alloy plate. The copper alloy plate was then finish rolled on a twenty-roll mill to obtain a strip with a thickness of 0.6 mm and a width of 160 mm.
[0072] (5) Solution treatment and aging treatment
[0073] The strip obtained in (4) was subjected to solution heat treatment at 920°C and water cooling to obtain a solution treated strip. The solution treated strip was then subjected to aging treatment at 450°C for 20 hours to obtain an aging treated strip.
[0074] (6) Trimming and rolling
[0075] The aging treated strip obtained in (5) is trimmed and rolled to obtain a Cu-Ni-Co-Si-Li alloy product - a Cu-Ni-Co-Si-Li alloy high-precision narrow strip, the performance indicators of which are shown in Table 2.
[0076] Table 2 Performance of Cu-Ni-Co-Si-Li alloy in Example 2
[0077] Tensile strength(MPa) 701 Yield strength (MPa) 642 Electrical conductivity (%IACS) 51.2
[0078] Example 3
[0079] (1) Vacuum melting and wire casting
[0080] The intermediate alloys such as Cu-5Li, Cu-Ni and high-purity copper are placed in a vacuum medium frequency melting furnace according to a certain ratio, the vacuum degree is -0.1MPa, and high-purity argon is continuously introduced into the vacuum medium frequency melting furnace. The temperature of the melt is controlled at 1160℃ during melting, and mechanical stirring is performed after 45 minutes of heat preservation to obtain a mixed melt. Subsequently, the mixed melt is cast into a wire billet, the casting temperature is controlled at 870℃, the casting speed is controlled at 80mm / min, and the cooling water flow rate is 50m3 / min to obtain a Φ35mm ingot. The composition of the ingot is: nickel Ni: 1.5wt.%; cobalt Co: 0.8wt.%; silicon Si: 1.5wt.%; magnesium Mg: 0.05wt.%; lithium Li: 0.08wt.%; light rare earth RE: 0.1wt.%; the rest is copper Cu.
[0081] (2) Continuous extrusion
[0082] The copper alloy ingot obtained in (1) was heated to 780°C, and the extrusion die was preheated to 680°C for continuous extrusion, with an extrusion ratio of 18, an extrusion wheel speed of 6 rpm, and an extrusion gap of 1.0 mm, to obtain a copper bar with a thickness of 7 mm and a width of 80 mm.
[0083] (3) Four-roll rolling
[0084] The copper bar obtained in (2) was subjected to a solution treatment at a temperature of 940°C for 2.5 hours to obtain a soft copper bar. The soft copper bar was then rolled on a four-roll mill to obtain a plate with a thickness of 0.9 mm and a width of 150 mm.
[0085] (4) Twenty-roller finishing rolling
[0086] The plate obtained in (3) was subjected to solution treatment at a temperature of 810°C for 1.5 hours to obtain an annealed copper alloy plate. The copper alloy plate was then finish rolled on a twenty-roll mill to obtain a strip with a thickness of 0.6 mm and a width of 160 mm.
[0087] (5) Solution treatment and aging treatment
[0088] The strip obtained in (4) was subjected to solution heat treatment at a temperature of 920°C and water cooling to obtain a solution treated strip. Subsequently, the strip after solution heat treatment was subjected to aging treatment at 450°C for 20 hours to obtain an aging treated strip.
[0089] (6) Trimming and rolling
[0090] The aging treated strip obtained in (5) is trimmed and rolled to obtain a Cu-Ni-Co-Si-Li alloy product - a Cu-Ni-Co-Si-Li alloy high-precision narrow strip, the performance indicators of which are shown in Table 3.
[0091] Table 3 Performance of Cu-Ni-Co-Si-Li alloy in Example 3
[0092] Tensile strength(MPa) 724 Yield strength (MPa) 648 Electrical conductivity (%IACS) 51.9
[0093] The above shows and describes the basic principles, main features and advantages of the present application. Those skilled in the art should understand that the present application is not limited by the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present application. Without departing from the spirit and scope of the present application, the present application may have various changes and improvements, and the scope of protection required by the present application is defined by the attached claims, description and their equivalents.
[0094] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present application rather than to limit the scope of protection of the present application. Although the present application has been described in detail with reference to the preferred embodiments, ordinary technicians in this field should understand that the technical solution of the present application can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present application.
Claims
1. A short process method for preparing high-strength and high-conductivity Cu-Ni-Co-Si-Li alloy high-precision narrow strip, characterized in that: The following steps are involved: The raw materials are vacuum-melted to obtain a mixed melt, and the mixed melt is wire-casted to obtain a cast billet, wherein the composition of the cast billet is: 1.0-2.0wt.% nickel, 0.5-1.0wt.% cobalt, 1-2wt.% silicon, 0-0.1wt.% magnesium Mg, 0.03-0.1wt.% lithium, 0.05-0.2wt.% light rare earth, and the rest is copper; Continuously extruding the ingot to obtain a copper bar; Rolling the copper bar to obtain a plate; Finish rolling the plate to obtain a strip; The strip is subjected to a solution treatment to obtain a solution treated strip. During the solution treatment, the strip is subjected to a solution heat treatment at a temperature of 850-1000° C. and a cooling method is water cooling. The solution treated strip is subjected to an aging treatment to obtain an aging treated strip. trimming and rolling the aging treated strip to obtain a high-precision narrow strip; Wherein, during the continuous extrusion process, the ingot is heated to 700-800°C, the extrusion die is preheated to 600-700°C for continuous extrusion, the extrusion ratio is 10-20, the extrusion wheel speed is 5-11rpm, the extrusion gap is 0.8-1.5mm, and a copper bar with a thickness of 5-8mm and a width of 60-100mm is obtained; During the rolling process, the copper bar is subjected to a solution treatment to obtain a soft copper bar, and then the soft copper bar is rolled on a four-roll rolling mill to obtain a plate with a thickness of 0.8-1 mm and a width of 120-180 mm; During the finishing rolling process, the plate is subjected to a solution treatment to obtain an annealed copper alloy plate, and then the copper alloy plate is subjected to a finishing rolling on a twenty-roll rolling mill to obtain a strip with a thickness of 0.4-0.8 mm and a width of 140-200 mm; During the vacuum melting process, the raw materials are placed in a vacuum melting furnace with a vacuum degree of -0.1 MPa, argon gas is continuously introduced into the vacuum melting furnace, the melt temperature is controlled at 1120-1200°C during melting, and mechanical stirring is performed after heat preservation for 30-60 minutes; During the wire billet casting process, the casting temperature is controlled at 800-950°C, the casting speed is controlled at 70-100 mm / min, the cooling water flow rate is 40-60 m³ / min, and a Φ25-40 mm billet is obtained; The copper bus is subjected to a solution treatment, comprising: The copper bar is subjected to solution treatment at a temperature of 860-1020° C. for 2-3 hours; The plate is subjected to a solution treatment, comprising: The plate is subjected to solution treatment at a temperature of 700-920° C. for 1-2 hours; During the aging treatment, the solution treated strip is aged at 400-500° C. for 18-24 hours.
2. A high-strength and high-conductivity Cu-Ni-Co-Si-Li alloy prepared by the short-process preparation method according to claim 1, characterized in that: Nickel 1.0-2.0wt.%, cobalt 0.5-1.0wt.%, silicon 1-2wt.%, magnesium Mg 0-0.1wt.%, lithium 0.03-0.1wt.%, light rare earth 0.05-0.2wt.%, and the rest is copper.