A kind of nylon cheese yarn and dyeing method thereof
Through the non-aqueous medium dyeing method, the problems of low utilization rate and uneven dyeing of nylon tube yarns are solved, the dye utilization rate and uniform dyeing are improved, and the difficulty of generation and treatment of dyeing wastewater is reduced, and the efficient dyeing process is achieved.
Patent Information
- Application Number
- CN202210266011.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-17
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-03-17
AI Technical Summary
The traditional dyeing method of nylon tube yarn has problems such as low dye utilization, uneven dyeing, and difficult treatment of dyeing wastewater. The dyeing unevenness caused by pH changes and hydrolysis of non-aqueous media dyeing methods is more obvious.
The non-aqueous medium dyeing method is adopted to control the contact rate and pH of dye and fibers through steps such as pressing water, adding dye liquid, heating, washing and drying, so as to improve dye utilization and uniform dyeing, and reduce the generation of dyeing wastewater.
The dye utilization rate has reached more than 95%, and the uniform dyeability has reached 4-5 levels, reducing the difficulty of generation and treatment of dyed wastewater, reducing the dyeing cost and water usage, and simplifying wastewater treatment.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of dyeing and finishing, in particular to a nylon cheese yarn and a dyeing method thereof. Background Art
[0002] At present, the traditional dyeing method of nylon cheese yarn is water bath dyeing. This dyeing method has the problems of low dye uptake, uneven dyeing, and easy to produce color flowers. In view of the dye uptake problem, a large amount of dye accelerator is added in the water bath dyeing process to improve the dye uptake of the dye. In view of the uneven dyeing phenomenon, a leveling agent is often added to improve the dyeing levelness. Therefore, a large amount of dye accelerator and leveling agent are consumed to achieve the corresponding dyeing effect. In addition, a large amount of water is consumed in the dyeing process, and multiple washings are required after dyeing to remove the dye on the fiber surface to improve the color fastness. Therefore, the entire dyeing process consumes a large amount of fresh water. At the same time, the wastewater generated contains a large amount of dyeing auxiliaries, and the wastewater treatment is difficult, which does not meet the current theme of clean dyeing, energy conservation and emission reduction. In short, the current dyeing method of nylon cheese yarn has low dye utilization rate, and a large amount of dye accelerator is required to promote dyeing, and a large amount of leveling agent is required to dye evenly, which produces a large amount of dyeing wastewater, which is difficult to treat and has a low reuse rate.
[0003] CN107794788A discloses a silicon-based non-aqueous medium dyeing method suitable for cheese yarn. In this scheme, the dye is directly added as a chemical material. This feeding method will highlight the common problem of reactive dye non-aqueous medium dyeing. Specifically, since most of the water is adsorbed on the nylon cheese yarn, the chance of the dye contacting the nylon cheese yarn increases, and the dyeing is too fast, which is prone to uneven dyeing. In addition, the feeding method of this scheme will cause the local pH in the dye bath to rise sharply, resulting in the aggravation of the hydrolysis of the dye under high pH conditions, and will also cause the local dye to react with the fiber too quickly, thus causing uneven dyeing. In non-aqueous medium dyeing, the amount of water used is small, and this phenomenon will be more obvious. Summary of the invention
[0004] In view of the above-mentioned shortcomings and problems of the prior art, the object of the present invention is to provide a nylon cheese yarn and a dyeing method thereof, which can improve the utilization rate of the dye (reaching more than 95%) when dyeing the nylon cheese yarn using a non-aqueous medium; improve the dyeing levelness; do not add additional salt during dyeing to reduce alkalinity; and reduce the generation of dyeing wastewater, thereby simplifying the treatment of the dyeing wastewater and improving the reuse rate of the dyeing wastewater.
[0005] In a first aspect, a colored nylon cheese yarn is provided, wherein the nylon cheese yarn is dyed with a first dye, the dye utilization rate of the first dye is not less than 95%, and the levelness is level 4-5.
[0006] In some embodiments, the first dye is any one of an acid dye, a neutral dye, a direct dye, a metal complex dye, or a combination of at least two thereof.
[0007] In a second aspect, a nylon cheese yarn dyeing method based on a non-aqueous medium is provided, comprising the following steps:
[0008] (1) Squeezing water: Pressurizing and squeezing water out of the nylon cheese yarn after water treatment in a dyeing vat, wherein the pressurizing pressure is 0.01MPa-0.5MPa, so that the moisture content of the nylon cheese yarn is 10%-200% (owf.);
[0009] (2) Adding dyeing liquid: adding a non-aqueous medium to the dye vat in a mass ratio of the non-aqueous medium to the nylon cheese yarn of (1.5:1)-(30:1); then, adding a first mixed solution of the non-aqueous medium and the dyeing liquid to the dye vat; wherein, when adding the first mixed solution to the dye vat, the material is added in a first linear feeding method of first slow and then fast, and the dye bath temperature is 5-40°C; wherein, after adding the first mixed solution, the dye bath temperature is controlled to be 5-40°C for 10-60 minutes; after adding the first mixed solution, the mass ratio of the non-aqueous medium to the nylon cheese yarn in the dye vat is (2:1)-(30.5:1); wherein, the dyeing liquid is composed of 0.1%-30% (owf.) of the first dye, 0.01%-2% (owf.) of the leveling agent, 0%-3% (owf.) of acetic acid and 20%-200% (owf.) of water;
[0010] (3) Heating: the heating rate is controlled at 0.1-1.5°C / min, the insulation temperature after heating is controlled at 40-100°C, and the insulation time after heating is 10min-200min;
[0011] (4) washing: the number of washing times is 2-5 times, the water consumption for a single washing is no more than 4 (owf.), the washing temperature is 20-100°C, and the single washing time is 1min-30min;
[0012] (5) Drying.
[0013] In one embodiment, the first linear feeding method is specifically as follows: the feeding speed at the beginning is 0-10 L / min, the feeding speed at the end is 5-100 L / min, the feeding time is 1-100 min, and the feeding speed increases with time.
[0014] In one embodiment, the non-aqueous medium is a liquid having a surface tension of 1-60 mN / m at 20°C.
[0015] In one embodiment, the non-aqueous medium is any one of hydrocarbons, silicon-based hydrocarbons, cyclomethylsiloxane, liquid paraffin, or a combination of at least two thereof.
[0016] In one embodiment, the dye utilization rate of the first dye is not less than 95%, and the levelness is level 4-5.
[0017] In one embodiment, the first dye is any one of an acid dye, a neutral dye, a direct dye, and a metal complex dye, or a combination of at least two thereof.
[0018] In a third aspect, there is provided a nylon cheese yarn dyed according to the method of the second aspect.
[0019] In the nylon cheese dyeing bath used in the nylon cheese dyeing method provided in the embodiment of the present application, most of the liquid is a non-aqueous medium, the amount of water used is extremely small, and the dye is only dissolved in water but not in the non-aqueous medium. Most of the water is adsorbed on the nylon cheese, and the dyeing rate can be close to 100%. Due to the increase in the concentration difference of the dye inside and outside the fiber, the water volume is low, and the amount of dye dyed to the inside of the fiber increases. The above effects save more than 20% of the dye in the system compared with traditional water bath dyeing, and no accelerator is required during the dyeing process. The amount of leveling agent used is reduced, which reduces the material cost of nylon cheese dyeing, and also reduces the proportion of floating dyes that need to be washed from about 30% to less than 5%, which is reduced to 1 / 3-1 / 4 of traditional water bath dyeing, thereby reducing the number of washing times and reducing the amount of washing water from about 80 times (owf.) of traditional water bath dyeing to less than 25 times (owf.). In addition, the single-cylinder levelness of the present invention can reach level 4-5, which is significantly better than level 3-4 of the non-aqueous medium dyeing method in CN107794788A, and the cylinder difference is small, which is easier to promote and industrialize. Since the amount of auxiliaries used in the dyeing process is very small, the auxiliaries content and dye content in the dyeing wastewater are very low, and the subsequent water treatment is simple, which effectively reduces the difficulty and cost of enterprise wastewater treatment. DETAILED DESCRIPTION
[0020] The following is a description of the implementation of the present invention by means of specific embodiments. Those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification.
[0021] The nylon cheese yarn can be prepared by the following dyeing method.
[0022] The embodiment of the present application provides a non-aqueous medium dyeing method for nylon cheese yarn, which is a relatively clean dyeing method and can dye nylon cheese yarn with dyes. When the method is used to dye nylon cheese yarn with dyes, the utilization rate of the dye can be increased to more than 95%.
[0023] In summary, in the nylon cheese yarn dyeing method provided in the embodiment of the present application, water squeezing is introduced before dyeing to accurately control the moisture content of the nylon cheese yarn before dyeing. While improving the dyeing effect of the subsequent dyeing process, it can also solve the cylinder difference problem caused by different moisture content of the nylon cheese yarn before dyeing.
[0024] During the implementation of the nylon cheese yarn dyeing method provided in the embodiment of the present application, in the non-aqueous medium dyeing system, non-aqueous medium is used to replace most of the traditional dyeing water, leaving only a very small amount of water-soluble dye, so the water content in the system is extremely low, and most of the dye solution can be dyed onto the nylon fiber through circulation. At the same time, since the dye concentration is much higher than that of traditional water bath dyeing, the amount of dye finally dyed onto the nylon fiber is higher than that of traditional water bath dyeing, and no accelerator does need to be added during the dyeing process.
[0025] In addition, in the nylon cheese yarn dyeing method provided in the embodiment of the present application, the dye liquor is stirred with the non-aqueous medium in the material cylinder, and the material is added linearly while stirring, first slowly and then quickly. This feeding method pre-disperses the dye liquor in the non-aqueous medium, slows down the speed at which the dye liquor contacts the nylon cheese yarn, thereby slowing down the dyeing rate. Therefore, in the system, better level dyeing can be obtained under the effect of adding a small amount of leveling agent. At the same time, most of the dye liquor is still adsorbed on the nylon cheese yarn during the dyeing process, and the dyeing rate will not be negatively affected. Thus, the level dyeing of the non-aqueous medium cheese yarn dyeing is improved, and finally most of the dye liquor is still adsorbed on the nylon cheese yarn, which will not have a negative impact on the dyeing rate. After testing, the level dyeing grade of the finished nylon cheese yarn dyed by the dyeing method provided in the embodiment of the present application is not less than 4-5 grades.
[0026] The dyeing method provided in the embodiment of the present application can save the time of mixing the dye solution and the non-aqueous medium, realize the dyeing and chemical processing at the same time, improve the utilization rate of the dye, and shorten the dyeing time.
[0027] Next, the process flow of the nylon cheese yarn dyeing method provided in the embodiment of the present application is described.
[0028] The method comprises the following process steps.
[0029] 1. Prepare dye solution
[0030] The recipe is as follows:
[0031] Dye: 0.1% - 30% (owf.). For example, the dye can be any one of acid dye, neutral dye, direct dye, metal complex dye, etc. or a combination of at least two. Wherein, owf. represents the percentage of the dyed object based on the weight of the object to be dyed. For example: under certain conditions, the amount of dye used to dye 100 kg of fabric is 4% (owf), which means that dyeing these fabrics requires: 100x0.04 = kg of dye.
[0032] Leveling agent: 0.01% - 2% (owf.); for example, the leveling agent may be any one of Albenol NR-12, Albenol AX-60B, Hipom HN-101*, Hipom Fix-3230, and the like.
[0033] Acetic acid: 0% - 3% (owf.);
[0034] The solvent is water, and the amount used is between 20%-200% (owf.).
[0035] 2. Staining
[0036] The dyeing process is as follows
[0037] A. Squeeze water
[0038] The nylon cheese yarn after scouring and washing needs to be pressurized and squeezed. This step is achieved by a non-aqueous medium nylon cheese yarn special dyeing cylinder. The pressurized pressure is between 0.01MPa-0.5MPa. After squeezing, the moisture content of the nylon cheese yarn is between 10%-200% (owf.). The non-aqueous medium nylon cheese yarn special dyeing cylinder used in this method has a pressurized water squeezing function. Exemplarily, the non-aqueous medium nylon cheese yarn special dyeing cylinder that can be used in this method can be: ultra-low bath ratio, high temperature and high pressure CLEANCOLOUR non-aqueous medium dyeing machine produced by Gaoxun Green Intelligent Equipment (Guangzhou) Co., Ltd.
[0039] B. Staining
[0040] Dyeing is achieved by the above-mentioned non-aqueous medium nylon cheese yarn special dyeing vat, and the dye bath is composed of a large amount of non-aqueous medium and a small amount of water during dyeing. Among them, under the condition that the total bath ratio remains unchanged, the water used for flow and heat conduction in traditional water bath dyeing is replaced with a non-aqueous medium (non-aqueous medium does not dissolve active dyes), leaving only a small amount of water for dissolving dyes and alkalis and providing a reaction environment. Under this condition, most of the dyes are adsorbed on the nylon cheese yarn without salt catalysis, thereby improving the dye uptake rate. Under this condition, most of the dyes are adsorbed on the nylon cheese yarn without salt catalysis, thereby improving the dye uptake rate. On this basis, the concentration difference of the dye inside and outside the nylon fiber surface is much greater than the concentration difference in the traditional water bath, so that more dyes can enter the fiber interior, thereby improving the dye utilization rate.
[0041] After squeezing water from the nylon cheese yarn in a dye vat, a non-aqueous medium is added to the dye vat, wherein the mass ratio of the non-aqueous medium to the nylon cheese yarn is between (1.5:1) and (30:1).
[0042] Add dye liquor to the dye vat, wherein the amount of the dye liquor is determined by the dye liquor formula of step 1 and the mass of the nylon cheese yarn. Specifically, the dye liquor can be stirred in the material vat of the dye vat together with a non-aqueous medium taken separately (i.e., the non-aqueous medium not taken from the dye vat) to obtain a dye liquor mixed with the non-aqueous medium. Then, add the dye liquor mixed with the non-aqueous medium to the dye vat. When the dye liquor is added to the dye vat, the dye bath temperature is controlled at 5-40°C. Among them, the lower the temperature, the less the dye hydrolysis, and controlling the temperature can achieve the purpose of reducing the dye hydrolysis and improving the dyeing rate. When adding dye liquid to the dye vat, stir the dye liquid while adding it in a linear manner (i.e., add the dye liquid mixed with a non-aqueous medium), slowly at first and then quickly. This operation can make the dye liquid relatively evenly distributed in the non-aqueous medium in the form of small droplets, slow down the contact between the dye liquid and the nylon cheese yarn, and slowly dye the dye onto the nylon cheese yarn, achieving a slow dyeing effect and improving the levelness of the nylon cheese yarn, thereby improving the shortcoming of poor levelness caused by too fast dyeing of non-aqueous media.
[0043] In this method of adding dye liquid, since the dye vat contains a non-aqueous medium, the dye liquid and the non-aqueous medium are first mixed in the material vat and then added to the dye vat to prevent the dye liquid from directly contacting the fiber before being evenly mixed with the non-aqueous medium after being added to the dye vat, which may easily cause color spots.
[0044] The linear feeding method can be specifically: the feeding speed at the beginning is 0-10L / min, the feeding speed at the end is 5-100L / min, the feeding time is 1-100min, the feeding speed increases with time, and the parameter of the feeding speed change can be adjusted in the range of 0-100L / min. The larger the parameter, the smaller the starting feeding speed, and the smaller the speed change for a period of time at the beginning. The dyeing vat used in this method has a linear feeding function, and the aforementioned linear feeding method can be implemented.
[0045] After adding the dye solution, the 5-40°C holding time is controlled between 10-60 minutes, at which time the mass ratio of the nylon cheese yarn to the non-aqueous medium is 1:2-1:30.5.
[0046] Heating: When heating, the heating rate is controlled at 0.1-1.5℃ / min, the insulation temperature after heating is controlled between 40-100℃, and the insulation time after heating is controlled between 10min-200min.
[0047] The non-aqueous medium used in the method needs to be liquid, and the surface tension is controlled at 1-60 mN / m (20° C.) The non-aqueous medium used in the method can be any one of hydrocarbons, silicon-based hydrocarbons, cyclomethylsiloxane, liquid paraffin, or a combination of at least two thereof.
[0048] In this specification, unless otherwise specified, the mass of nylon cheese yarn refers to the mass of dry nylon cheese yarn, that is, the mass of nylon cheese yarn that has not been washed before dyeing.
[0049] C. Washing
[0050] Washing is achieved by the above-mentioned non-aqueous medium nylon cheese yarn special dyeing vat. Since the dyeing step improves the utilization rate of dyes, the washing pressure is reduced and the number of washing times is reduced. The dyeing method of the embodiment of the present application reduces the amount of leveling agent used, and no auxiliary dye is added. The content of dye and auxiliary agent in the dyeing wastewater is very low, which is convenient for treatment and reuse. The whole washing process includes the number of washings being controlled between 2-5 times, the water consumption for a single washing being no more than 4 times (owf.), the total washing water being controlled below 8-20 times (owf.), the washing temperature being controlled between 20-100°C, and the single washing time being controlled between 1min-30min.
[0051] D. Drying
[0052] Drying is achieved by means of a dryer.
[0053] Next, in a specific embodiment, the nylon cheese yarn dyeing method provided in the embodiment of the present application is illustrated.
[0054] Example 1, preparation of blue nylon cheese yarn.
[0055] Package yarn to be dyed: nylon package yarn.
[0056] Nylon cheese yarn to be dyed: 300kg.
[0057] Dye solution formula:
[0058] Acid Red G: 2% (owf.);
[0059] Acetic acid: 0.1% (owf.);
[0060] Leveling agent: 0.5% (owf.);
[0061] Water for chemical dyes: 100% (owf.).
[0062] Dyeing process and parameters
[0063] 11. Weigh and mix materials.
[0064] 12. Before dyeing, the nylon cheese yarn after scouring and squeezing is placed in a non-aqueous medium nylon cheese yarn special dyeing vat. When squeezing, the pressure is 0.4 MPa. After squeezing, the moisture content of the nylon cheese yarn is 80% (owf.). In this embodiment, unless otherwise specified, the non-aqueous medium nylon cheese yarn special dyeing vat can be referred to as a dyeing vat.
[0065] 13. Add non-aqueous medium and put it into the dyeing vat. At this time, the mass ratio of nylon cheese yarn to non-aqueous medium is 1:4.
[0066] 14. Add dye liquid, add the dye liquid into the material tank of the dye vat through the automatic feeding system, and then add non-aqueous medium, stir, and linearly add material (i.e. dye liquid mixed with non-aqueous medium) into the dye vat. The dye bath temperature is 30℃ when the dye liquid is added to the dye vat, and the heat preservation time at 5-40℃ after adding the dye liquid is 40 minutes. The ratio of nylon cheese yarn to non-aqueous medium is 1:5.
[0067] 16. Heat up, and the heating rate is controlled at 1℃ / min.
[0068] 17. Keep warm: the temperature after heating is 85℃ and the keeping time is 60min.
[0069] 18. Washing, washing temperature is 80℃, single washing time is 10min, washing times are 3 times, water consumption for each washing is 4 times (owf.). The total washing water consumption for 3 washing times is 12 times (owf.).
[0070] 19. Drying.
[0071] 20. The dye uptake (dye uptake refers to the ratio of dye adsorbed from dye liquor to fiber before dye is fixed with soda ash) is 99.5%, the dye utilization is 95%, and the levelness is 4-5. The levelness can be measured as follows: the cheese yarn is woven into cloth, and the DE value is measured at a certain number of positions on the cloth surface. If the value is less than 0.8, it is levelness 4-5.
[0072] 21. The various indicators of the finished nylon cheese yarn are shown in Table 1.
[0073] The main fastness of the finished nylon cheese yarn was tested according to the National Standard GB / T 3921-2008 and the National Standard GB / T 3920-2008. The test results are shown in Table 1.
[0074] Table 1
[0075] Soap fastness Dry rubbing fastness Wet rubbing fastness Level 4-5 Level 4-5 Level 3-4
[0076] In addition, after testing, the uniformity of the finished nylon cheese yarn can meet customer requirements, and there is no difference between the inner and outer layers; the yarn strength of the finished nylon cheese yarn can meet customer requirements; the yarn softness can meet weaving requirements; the surface effect and feel of the yarn after weaving can also meet customer requirements.
[0077] Example 2, lake blue nylon cheese yarn.
[0078] Package yarn to be dyed: nylon package yarn.
[0079] The mass of nylon cheese yarn to be dyed: 300kg.
[0080] Dye solution formula:
[0081] Acid Lake Blue A: 0.5% (owf.);
[0082] Acetic acid: 0.5% (owf.);
[0083] Leveling agent: 0.5% (owf.);
[0084] Water for chemical dyeing: 110% (owf.).
[0085] Dyeing process and parameters
[0086] 21. Weigh and prepare materials.
[0087] 22. Before dyeing, the nylon cheese yarn after scouring and squeezing is placed in a non-aqueous medium nylon cheese yarn special dyeing vat. When squeezing, the pressure is 0.4 MPa. After squeezing, the moisture content of the nylon cheese yarn is 70% (owf.). In this embodiment, unless otherwise specified, the non-aqueous medium nylon cheese yarn special dyeing vat can be referred to as a dyeing vat.
[0088] 23. Add non-aqueous medium and put it into the dyeing vat. At this time, the mass ratio of nylon cheese yarn to non-aqueous medium is 1:4.
[0089] 24. Add dye liquid, add the dye liquid into the material tank of the dye vat through the automatic feeding system, and then add non-aqueous medium, stir, and linearly add material (i.e. dye liquid mixed with non-aqueous medium) into the dye vat. The dye bath temperature is 25℃ when the dye liquid is added to the dye vat, and the heat preservation time at 5-40℃ after adding the dye liquid is 30 minutes. The ratio of nylon cheese yarn to non-aqueous medium is 1:5.
[0090] 25. Heat up, and the heating rate is controlled at 1℃ / min.
[0091] 26. Keep warm. After heating, the temperature is kept at 91°C and the keeping time is 60 minutes.
[0092] 27. Washing, washing temperature is 60℃, single washing time is 10min, washing times are 3 times, water consumption for each washing is 4 times (owf.). The total washing water consumption for 3 washing times is 12 times (owf.).
[0093] 29. Drying.
[0094] 30. The test results show that the dyeing rate is 99%, the dye utilization rate is 97%, and the levelness is 4-5.
[0095] 31. The various indicators of the finished nylon cheese yarn are shown in Table 2.
[0096] The main fastness of the finished nylon cheese yarn was tested according to the National Standard GB / T 3921-2008 and the National Standard GB / T 3920-2008. The test results are shown in Table 2.
[0097] Table 2
[0098] Soap fastness Dry rubbing fastness Wet rubbing fastness Level 4-5 Level 4-5 Level 3-4
[0099] In addition, after testing, the uniformity of the finished nylon cheese yarn can meet customer requirements, and there is no difference between the inner and outer layers; the yarn strength of the finished nylon cheese yarn can meet customer requirements; the yarn softness can meet weaving requirements; the surface effect and feel of the yarn after weaving can also meet customer requirements.
[0100] Example 3, orange nylon cheese yarn.
[0101] Package yarn to be dyed: nylon package yarn.
[0102] The mass of nylon cheese yarn to be dyed: 300kg.
[0103] Dye solution formula:
[0104] Neutral Orange R: 1.0% (owf.)
[0105] Acetic acid: 0.1% (owf.)
[0106] Leveling agent: 1% (owf.)
[0107] Water for chemical dyes: 100% (owf.).
[0108] Dyeing process and parameters
[0109] 31. Weigh and prepare materials.
[0110] 32. Before dyeing, the nylon cheese yarn after scouring and squeezing is placed in a non-aqueous medium nylon cheese yarn special dyeing vat. When squeezing, the pressure is 0.4 MPa. After squeezing, the moisture content of the nylon cheese yarn is 70% (owf.). In this embodiment, unless otherwise specified, the non-aqueous medium nylon cheese yarn special dyeing vat can be referred to as a dyeing vat.
[0111] 33. Add non-aqueous medium and put it into the dyeing vat. At this time, the mass ratio of nylon cheese yarn to non-aqueous medium is 1:4.
[0112] 34. Add dye liquid, add the dye liquid into the material tank of the dye vat through the automatic feeding system, and then add non-aqueous medium, stir, and linearly add material (i.e. dye liquid mixed with non-aqueous medium) into the dye vat. The dye bath temperature is 25℃ when the dye liquid is added to the dye vat, and the heat preservation time at 5-40℃ after adding the dye liquid is 50 minutes. The ratio of nylon cheese yarn to non-aqueous medium is 1:5.
[0113] 35.Heat up, and the heating rate is controlled at 1℃ / min.
[0114] 36. Keep warm. After heating, the temperature is kept at 91°C and the keeping time is 60 minutes.
[0115] 37. Washing, washing temperature is 60℃, single washing time is 10min, washing times are 2 times, water consumption for each washing is 4 times (owf.). The total washing water consumption for 2 washing times is 8 times (owf.).
[0116] 39. Drying.
[0117] The test results show that the dyeing rate is 99.8%, the dye utilization rate is 98%, and the levelness is 4-5.
[0118] 41. The various indicators of the finished nylon cheese yarn are shown in Table 3.
[0119] The main fastness of the finished nylon cheese yarn was tested according to the National Standard GB / T 3921-2008 and the National Standard GB / T 3920-2008. The test results are shown in Table 2.
[0120] Table 3
[0121] Soap fastness Dry rubbing fastness Wet rubbing fastness Level 4-5 Level 4-5 Level 3-4
[0122] In addition, after testing, the uniformity of the finished nylon cheese yarn can meet customer requirements, and there is no difference between the inner and outer layers; the yarn strength of the finished nylon cheese yarn can meet customer requirements; the yarn softness can meet weaving requirements; the surface effect and feel of the yarn after weaving can also meet customer requirements.
[0123] In the nylon cheese dyeing bath used in the nylon cheese dyeing method provided in the embodiment of the present application, most of the liquid is a non-aqueous medium, the amount of water used is extremely small, and the dye is only dissolved in water but not in the non-aqueous medium. Most of the water is adsorbed on the nylon cheese, and the dyeing rate can be close to 100%. Due to the increase in the concentration difference of the dye inside and outside the fiber, the water volume is low, and the amount of dye dyed to the inside of the fiber increases. The above effects save more than 20% of the dye in the system compared with traditional water bath dyeing, and no accelerator is required during the dyeing process. The amount of leveling agent used is reduced, which reduces the material cost of nylon cheese dyeing. At the same time, the proportion of floating dyes that need to be washed can be reduced from about 30% to less than 5%, which is reduced to 1 / 3-1 / 4 of traditional water bath dyeing, thereby reducing the number of washing times and reducing the amount of washing water from about 80 times (owf.) of traditional water bath dyeing to less than 25 times (owf.). In addition, the single-cylinder levelness of the present invention can reach level 4-5, which is significantly better than level 3-4 of the non-aqueous medium dyeing method in CN107794788A, and the cylinder difference is small, which is easier to promote and industrialize. Since the amount of auxiliaries used in the dyeing process is very small, the auxiliaries content and dye content in the dyeing wastewater are very low, and the subsequent water treatment is simple, which effectively reduces the difficulty and cost of enterprise wastewater treatment.
[0124] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A nylon cheese dyeing method based on non-aqueous medium, characterized in that: The method is used to dye nylon cheese yarn using a non-aqueous medium and a first dye, wherein the dye utilization rate of the first dye is not less than 95%, The levelness is 4-5; the method comprises the following steps: (1) preparing a dye solution, wherein the dye solution contains a leveling agent in an amount of 0.01% to 2% owf.; and the dye solution does not contain a dyeing auxiliary; and the dye solution contains a first dye in an amount of 0.1% to 30% (owf.), acetic acid in an amount of 0% to 3% owf., and water in an amount of 20% to 200% owf.; (2) Squeezing water: Pressurizing and squeezing water out of the washed nylon cheese yarn in a dye vat, wherein the pressurizing pressure is 0.01MPa-0.5MPa, so that the moisture content of the nylon cheese yarn is 10%-200% owf.; (3) Adding dye solution: adding a non-aqueous medium to the dye vat at a mass ratio of the non-aqueous medium to the nylon cheese yarn of (1.5:1)-(30:1); then, adding a first mixed solution of the non-aqueous medium and the dye solution to the dye vat; wherein, when adding the first mixed solution to the dye vat, the material is added in a first linear feeding method of first slow and then fast, and the dye bath temperature is 5-40°C; wherein, after adding the first mixed solution, the dye bath temperature is controlled to be 5-40°C for 10-60 minutes; after adding the first mixed solution, the mass ratio of the non-aqueous medium to the nylon cheese yarn in the dye vat is (2:1)-(30.5:1); (4) Heating: The heating rate is controlled at 0.1-1.5℃ / min, and the insulation temperature is controlled at 40-100℃ after heating. After heating, the insulation time is 10min-200min; (5) Washing: The number of washing times is 2-5 times, the water consumption for a single washing is no more than 4 owf., the washing temperature is 20-100°C, and the single washing time is 1min-30min; (6) Drying.
2. The method according to claim 1, characterized in that The first linear feeding method is specifically as follows: the feeding speed is 0-10 L / min at the beginning, the feeding speed is 5-100 L / min at the end, the feeding time is 1-100 min, and the feeding speed increases with time.
3. The method according to claim 1 or 2, characterized in that: The non-aqueous medium is a liquid and has a surface tension of 1-60 mN / m at 20°C.
4. The method according to claim 3, characterized in that The non-aqueous medium is any one of hydrocarbons, silicon-based hydrocarbons, cyclomethylsiloxane, and liquid paraffin, or a combination of at least two thereof.
5. The method according to claim 1 or 2, characterized in that: The first dye is any one of acid dye, neutral dye, direct dye and metal complex dye, or a combination of at least two thereof.
6. Nylon cheese yarn dyed according to any one of claims 1 to 5.
Citation Information
Patent Citations
Silicon based non-aqueous medium dyeing method suitable for cheese
CN107794788A
New dyeing method of active dye taking methylsiloxane as medium
CN101922121A
Dyeing method of disperse dyestuff with special methylsiloxane as medium
CN103074781A
Method for dyeing textiles with dye liquor prepared from miscible organic solvent and water
CN109667161A
Little-water medium dyeing method for cellulosic fiber cheese
CN109722924A